Boron doping method of N-type crystalline silicon cell and application thereof

By adopting a boron doping process with low-pressure diffusion furnace and step temperature treatment in N-type crystalline silicon batteries, the problems of high temperature and long-term diffusion in the boron doping process are solved, equipment loss and production costs are reduced, and boron doping is improved. efficiency.

CN119069576APending Publication Date: 2024-12-03合肥大恒智慧能源科技有限公司
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411203830.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-30
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

The boron doping process in N-type crystalline silicon batteries has high temperature and long-term thermal diffusion difficulty, resulting in high hardware requirements and large losses, long process time and high cost.

Method used

Boron doping is carried out using a low-pressure diffusion furnace. By step temperature heating and constant temperature treatment, the boron diffusion oxidation propulsion temperature is reduced, and the boron diffusion process steps are optimized, including heating, deposition, junction pushing and oxidation propulsion, and BCl3 is used as the boron diffusion doping source. Form a pyramid-like surface structure and optimize the surface treatment of silicon wafers.

Benefits of technology

It effectively reduces the boron diffusion oxidation propulsion temperature, extends the service life of the equipment, reduces production costs, and improves the boron doping efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119069576A_ABST
    Figure CN119069576A_ABST
Patent Text Reader

Abstract

The invention provides a boron doping method of an N-type crystalline silicon battery and application of the boron doping method. The boron doping method of the N-type crystalline silicon cell comprises the following steps: S1, feeding an N-type silicon wafer into a low-pressure diffusion furnace, and completing temperature rise and leakage detection; s2, the temperature is raised to the first pre-deposition temperature, and first oxidation and first deposition are completed; s3, raising the temperature to a pre-deposition temperature II and keeping the temperature constant for a certain time to finish deposition II; s4, raising the temperature to a pre-deposition temperature III, and keeping the temperature for a certain time to finish deposition III; s5, raising the temperature to a pushing temperature to push junctions; s6, raising the temperature to an oxidation propulsion temperature for propulsion; and S7, cooling and discharging from the pipe. According to the boron doping method of the N-type crystalline silicon battery and the application of the boron doping method, the boron diffusion oxidation propelling temperature is reduced by about 40 DEG C, the service life of an auxiliary material of boron diffusion equipment can be effectively prolonged, and the production cost is further reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of solar cells, and in particular to a boron doping method for an N-type crystalline silicon cell and an application thereof. Background Art

[0002] With the research and development of solar photovoltaic technology, photovoltaic technology based on crystalline silicon substrate has occupied the mainstream position in the market. Crystalline silicon is divided into P-type and N-type silicon. With the mass production of P-type crystalline silicon cells, the conversion efficiency gradually approaches the theoretical upper limit. However, due to its silicon wafer characteristics, N-type crystalline silicon cells have a higher minority carrier life, which is suitable for more complex cell processes and obtains higher cell conversion efficiency.

[0003] The boron source diffusion used in the preparation of PN junctions for N-type TOPcon cells has a similar technical process to phosphorus diffusion, but is more difficult. The difference in atomic size between boron atoms and silicon atoms makes the thermal diffusion process of boron more difficult than that of phosphorus.

[0004] Boron atoms are more difficult to move in the silicon lattice than phosphorus atoms, so higher temperatures are required to provide sufficient thermal energy to allow boron atoms to diffuse more effectively in the silicon wafer (the boron diffusion temperature is 200°C higher than that of phosphorus diffusion, reaching about 1050°C). In addition, the diffusion time is long, the diffusion temperature is high, the process time is long, the hardware quality requirements of the diffusion equipment are high, and the loss of the machine is also large.

[0005] Therefore, it is necessary to provide a boron doping method for N-type crystalline silicon cells and its application to solve the above technical problems. Summary of the invention

[0006] The present invention provides a boron doping method for an N-type crystalline silicon battery and application thereof, which solves the problems of the background technology.

[0007] In order to solve the above technical problems, the boron doping method of N-type crystalline silicon cell provided by the present invention comprises the following steps:

[0008] S1, put the N-type silicon wafer into the low-pressure diffusion furnace and complete the heating and leak detection;

[0009] S2, heating to pre-deposition temperature to complete pre-oxidation and deposition;

[0010] S3, raising the temperature to pre-deposition temperature 2 and maintaining the temperature constant for a certain period of time to complete deposition 2;

[0011] S4, raising the temperature to pre-deposition temperature 3 and maintaining the temperature for a certain period of time to complete deposition 3;

[0012] S5, heating to the pushing temperature for pushing;

[0013] S6, heating to oxidation advancement temperature for advancement;

[0014] S7, cool down and discharge the pipe.

[0015] Preferably, the N-type silicon wafer is used as the substrate material, and a pyramid-shaped surface structure is generated on the surface of the silicon wafer through alkaline cleaning and texturing.

[0016] Preferably, the boron diffusion doping source is BCl3.

[0017] Preferably, in S1, the heating temperature is 830-845° C., the constant pressure is 150-300 mbar, and the N2 flow rate is 3400-4200 sccm.

[0018] Preferably, the deposition temperature in the Deposition 1 / Deposition 2 / Deposition 3 steps is in a step-growth state, the Deposition 3 temperature > the Deposition 2 temperature > the Deposition 1 temperature, and the deposition times in the Deposition 1, Deposition 2 and Deposition 3 steps are different, the Deposition 2 time > the Deposition 1 temperature > the Deposition 3 temperature.

[0019] Preferably, the S5 push junction temperature is 920-950° C., the constant pressure is 150-300 mba, and the N2 flow rate is 2000-4000 sccm.

[0020] Preferably, the knotting is completed in two steps, and the knotting time is 480-580s respectively.

[0021] Preferably, the S6 oxidation push junction temperature is 995-1005°C, the constant pressure is 250-1000mba, the O2 flow rate is 12000-25000sccm, and the oxidation push is completed in two steps, with oxidation push times of 800-950s and 600-6300s respectively.

[0022] A preparation process of an N-type crystalline silicon cell, which uses any one of the boron doping methods for an N-type crystalline silicon cell.

[0023] Preferably, the method comprises the following steps:

[0024] Step 1: Texturing and cleaning of N-type silicon wafers;

[0025] Step 2: Boron diffusion to form a low-compound shallow doping region, and BSG is formed on the boron diffusion surface;

[0026] Step 3: back polishing;

[0027] Step 4: Prepare an oxide tunneling layer and a phosphorus-doped amorphous silicon layer by PECVD, wherein the phosphorus-doped amorphous silicon layer has a thickness of 75-100 nm;

[0028] Step 5: high temperature annealing and crystallization to activate phosphorus atoms, the crystallization annealing temperature is 980-1020°C;

[0029] Step 6: Clean the back side and remove PSG and edge wrapping;

[0030] Step 7: depositing a passivation film on both sides, wherein the passivation layer is a stack of two or more layers of AlOx, SiNx, SiOx, and SiONx;

[0031] Step 8: Printing metal electrodes and sintering;

[0032] Step 9. Optimize front contact through laser enhanced contact.

[0033] Compared with the related art, the boron doping method of N-type crystalline silicon cell provided by the present invention and its application have the following beneficial effects:

[0034] The present invention provides a boron doping method for an N-type crystalline silicon cell and application thereof. The present invention reduces the temperature of boron diffusion oxidation advancement by about 40°C, can effectively improve the service life of auxiliary materials of boron diffusion equipment, and thus reduce production costs. BRIEF DESCRIPTION OF THE DRAWINGS

[0035] Figure 1 A schematic diagram of the process of the boron doping method for N-type crystalline silicon cells provided by the present invention;

[0036] Figure 2 A schematic diagram of the process flow of the preparation process of the N-type crystalline silicon cell provided by the present invention. DETAILED DESCRIPTION

[0037] The present invention will be further described below in conjunction with the accompanying drawings and implementation modes.

[0038] Please refer to Figure 1 , Figure 2 ,in, Figure 1 A schematic diagram of the process of the boron doping method for N-type crystalline silicon cells provided by the present invention; Figure 2 A schematic diagram of the process flow of the preparation process of the N-type crystalline silicon cell provided by the present invention.

[0039] Embodiment 1: A boron doping method for an N-type crystalline silicon cell comprises the following steps:

[0040] S1. Place the N-type silicon wafer into a low-pressure diffusion furnace and complete heating and leak detection. The N-type silicon wafer is the substrate material. A pyramid-shaped surface structure is produced on the surface of the silicon wafer by alkaline cleaning and texturing. The heating temperature is 830°C, the constant pressure is 150mbar, and the N2 flow rate is 3400sccm.

[0041] S2, heating to pre-deposition temperature to complete pre-oxidation and deposition;

[0042] S3, raising the temperature to pre-deposition temperature 2 and maintaining the temperature constant for a certain period of time to complete deposition 2;

[0043] S4, raising the temperature to pre-deposition temperature 3 and maintaining the temperature for a certain period of time to complete deposition 3;

[0044] S5, heating to the push temperature for pushing, the pushing temperature is 920℃, the constant pressure is 150mba, the N2 flow rate is 2000sccm, the pushing is completed in two steps, the pushing time is 480s respectively. In normal production, the temperature and time of this step are mainly used to control the overall square resistance and its uniformity;

[0045] S6, heating to the oxidation advancement temperature for advancement, the oxidation advancement temperature is 995°C, the constant pressure is 250mba, the O2 flow rate is 12000sccm, the oxidation advancement is completed in two steps, and the oxidation advancement time is 800s and 600s respectively;

[0046] S7, cool down and discharge the pipe.

[0047] The deposition temperature in the deposition one / deposition two / deposition three steps is in a step-growth state, wherein the deposition three temperature> the deposition two temperature> the deposition one temperature. The deposition times in the deposition one, deposition two and deposition three steps are different, wherein the deposition two time> the deposition one temperature> the deposition three temperature.

[0048] Preferably, after the boron diffusion process is completed, the square resistance of the silicon wafer surface is 320-380Ω, and the boron diffusion doping source is BCl3.

[0049] Embodiment 2: A boron doping method for an N-type crystalline silicon cell comprises the following steps:

[0050] S1. Place the N-type silicon wafer into a low-pressure diffusion furnace and complete heating and leak detection. The N-type silicon wafer is the substrate material. A pyramid-shaped surface structure is produced on the surface of the silicon wafer by alkaline cleaning and texturing. The heating temperature is 835°C, the constant pressure is 200mbar, and the N2 flow rate is 3600sccm.

[0051] S2, heating to pre-deposition temperature to complete pre-oxidation and deposition;

[0052] S3, raising the temperature to pre-deposition temperature 2 and maintaining the temperature constant for a certain period of time to complete deposition 2;

[0053] S4, raising the temperature to pre-deposition temperature 3 and maintaining the temperature for a certain period of time to complete deposition 3;

[0054] S5, heating to the push temperature for push bonding, the push bonding temperature is 930°C, the constant pressure is 170mba, the N2 flow rate is 2500sccm, the push bonding is completed in two steps, and the push bonding time is 500s respectively;

[0055] S6, heating to the oxidation advancement temperature for advancement, the oxidation advancement temperature is 1000°C, the constant pressure is 400mba, the O2 flow rate is 15000sccm, the oxidation advancement is completed in two steps, and the oxidation advancement time is 850s and 610s respectively;

[0056] S7, cool down and discharge the pipe.

[0057] The deposition temperature in the deposition one / deposition two / deposition three steps is in a step-growth state, wherein the deposition three temperature> the deposition two temperature> the deposition one temperature. The deposition times in the deposition one, deposition two and deposition three steps are different, wherein the deposition two time> the deposition one temperature> the deposition three temperature.

[0058] Preferably, after the boron diffusion process is completed, the square resistance of the silicon wafer surface is 330-380Ω, and the boron diffusion doping source is BCl3.

[0059] Embodiment 3: A boron doping method for an N-type crystalline silicon cell comprises the following steps:

[0060] S1. Place the N-type silicon wafer into a low-pressure diffusion furnace and complete heating and leak detection. The N-type silicon wafer is the substrate material. A pyramid-shaped surface structure is produced on the surface of the silicon wafer by alkaline cleaning and texturing. The heating temperature is 840°C, the constant pressure is 250mbar, and the N2 flow rate is 3800sccm.

[0061] S2, heating to pre-deposition temperature to complete pre-oxidation and deposition;

[0062] S3, raising the temperature to pre-deposition temperature 2 and maintaining the temperature constant for a certain period of time to complete deposition 2;

[0063] S4, raising the temperature to pre-deposition temperature 3 and maintaining the temperature for a certain period of time to complete deposition 3;

[0064] S5, heating to the pushing temperature for pushing, the pushing temperature is 940℃, the constant pressure is 220mba, the N2 flow rate is 3000sccm, the pushing is completed in two steps, and the pushing time is 520s respectively;

[0065] S6, heating to the oxidation advancement temperature for advancement, the oxidation advancement temperature is 1000°C, the constant pressure is 600mba, the O2 flow rate is 20000sccm, the oxidation advancement is completed in two steps, and the oxidation advancement time is 850s and 615s respectively;

[0066] S7, cool down and discharge the pipe.

[0067] The deposition temperature in the deposition one / deposition two / deposition three steps is in a step-growth state, wherein the deposition three temperature> the deposition two temperature> the deposition one temperature. The deposition times in the deposition one, deposition two and deposition three steps are different, wherein the deposition two time> the deposition one temperature> the deposition three temperature.

[0068] Preferably, after the boron diffusion process is completed, the square resistance of the silicon wafer surface is 340-380Ω, and the boron diffusion doping source is BCl3.

[0069] Embodiment 4: A boron doping method for an N-type crystalline silicon cell comprises the following steps:

[0070] S1. Place the N-type silicon wafer into a low-pressure diffusion furnace and complete heating and leak detection. The N-type silicon wafer is the substrate material. A pyramid-shaped surface structure is produced on the surface of the silicon wafer by alkaline cleaning and texturing. The heating temperature is 840°C, the constant pressure is 280mbar, and the N2 flow rate is 4000sccm.

[0071] S2, heating to pre-deposition temperature to complete pre-oxidation and deposition;

[0072] S3, raising the temperature to pre-deposition temperature 2 and maintaining the temperature constant for a certain period of time to complete deposition 2;

[0073] S4, raising the temperature to pre-deposition temperature 3 and maintaining the temperature for a certain period of time to complete deposition 3;

[0074] S5, heating to the pushing temperature for pushing, the pushing temperature is 940°C, the constant pressure is 240mba, the N2 flow rate is 3500sccm, the pushing is completed in two steps, and the pushing time is 540s respectively;

[0075] S6, heating to the oxidation advancement temperature for advancement, the oxidation advancement temperature is 1000°C, the constant pressure is 800mba, the O2 flow rate is 20000sccm, the oxidation advancement is completed in two steps, and the oxidation advancement time is 940s and 625s respectively;

[0076] S7, cool down and discharge the pipe.

[0077] The deposition temperature in the deposition one / deposition two / deposition three steps is in a step-growth state, wherein the deposition three temperature> the deposition two temperature> the deposition one temperature. The deposition times in the deposition one, deposition two and deposition three steps are different, wherein the deposition two time> the deposition one temperature> the deposition three temperature.

[0078] Preferably, after the boron diffusion process is completed, the square resistance of the silicon wafer surface is 360-380Ω, and the boron diffusion doping source is BCl3.

[0079] Embodiment 5: A boron doping method for an N-type crystalline silicon cell comprises the following steps:

[0080] S1. Place the N-type silicon wafer into a low-pressure diffusion furnace and complete heating and leak detection. The N-type silicon wafer is the substrate material. A pyramid-shaped surface structure is produced on the surface of the silicon wafer by alkaline cleaning and texturing. The heating temperature is 845°C, the constant pressure is 300mbar, and the N2 flow rate is 4200sccm.

[0081] S2, heating to pre-deposition temperature to complete pre-oxidation and deposition;

[0082] S3, raising the temperature to pre-deposition temperature 2 and maintaining the temperature constant for a certain period of time to complete deposition 2;

[0083] S4, raising the temperature to pre-deposition temperature 3 and maintaining the temperature for a certain period of time to complete deposition 3;

[0084] S5, heating to the pushing temperature for pushing, the pushing temperature is 950°C, the constant pressure is 300mba, the N2 flow rate is 4000sccm, the pushing is completed in two steps, and the pushing time is 580s respectively;

[0085] S6, heating to the oxidation advancement temperature for advancement, the oxidation advancement temperature is 1005°C, the constant pressure is 1000mba, the O2 flow rate is 25000sccm, the oxidation advancement is completed in two steps, and the oxidation advancement time is 9500s and 630s respectively;

[0086] S7, cool down and discharge the pipe.

[0087] The deposition temperature in the deposition one / deposition two / deposition three steps is in a step-growth state, wherein the deposition three temperature> the deposition two temperature> the deposition one temperature. The deposition times in the deposition one, deposition two and deposition three steps are different, wherein the deposition two time> the deposition one temperature> the deposition three temperature.

[0088] Preferably, after the boron diffusion process is completed, the square resistance of the silicon wafer surface is 370-380Ω, and the boron diffusion doping source is BCl3.

[0089] A preparation process of an N-type crystalline silicon cell, characterized in that it applies the boron doping method of the N-type crystalline silicon cell.

[0090] The preparation process of the N-type crystalline silicon cell comprises the following steps:

[0091] Step 1: Texturing and cleaning of N-type silicon wafers;

[0092] Step 2: Boron diffusion to form a low-compound shallow doping region, and BSG is formed on the boron diffusion surface;

[0093] Step 3: back polishing;

[0094] Step 4: Prepare an oxide tunneling layer and a phosphorus-doped amorphous silicon layer by PECVD, wherein the phosphorus-doped amorphous silicon layer has a thickness of 75-100 nm;

[0095] Step 5: high temperature annealing and crystallization to activate phosphorus atoms, the crystallization annealing temperature is 980-1020°C;

[0096] Step 6: Clean the back side and remove PSG and edge wrapping;

[0097] Step 7: depositing a passivation film on both sides, wherein the passivation layer is a stack of two or more layers of AlOx, SiNx, SiOx, and SiONx;

[0098] Step 8: Printing metal electrodes and sintering;

[0099] Step 9. Optimize front contact through laser enhanced contact.

[0100] The boron diffusion doping source is BCl3.

[0101] Compared with the related art, the boron doping method of N-type crystalline silicon cell provided by the present invention and its application have the following beneficial effects:

[0102] The present invention reduces the temperature of boron diffusion oxidation advancement by about 40° C., can effectively improve the service life of auxiliary materials of boron diffusion equipment, and further reduce production costs.

[0103] The above descriptions are merely embodiments of the present invention and are not intended to limit the patent scope of the present invention. Any equivalent structure or equivalent process transformation made using the contents of the present invention specification and drawings, or directly or indirectly applied in other related technical fields, are also included in the patent protection scope of the present invention.

Claims

1. A boron doping method for an N-type crystalline silicon cell, characterized in that: The following steps are involved: S1, put the N-type silicon wafer into the low-pressure diffusion furnace and complete the heating and leak detection; S2, heating to pre-deposition temperature to complete pre-oxidation and deposition; S3, raising the temperature to pre-deposition temperature 2 and maintaining the temperature constant for a certain period of time to complete deposition 2; S4, raising the temperature to pre-deposition temperature 3 and maintaining the temperature for a certain period of time to complete deposition 3; S5, heating to the pushing temperature for pushing; S6, heating to oxidation advancement temperature for advancement; S7, cool down and discharge the pipe.

2. The boron doping method for N-type crystalline silicon cells according to claim 1, characterized in that: The N-type silicon wafer is a substrate material, and a pyramid-shaped surface structure is generated on the surface of the silicon wafer through alkaline cleaning and texturing.

3. The boron doping method for N-type crystalline silicon cells according to claim 1, characterized in that: In the S1, the heating temperature is 830-845° C., the constant pressure is 150-300 mbar, and the N2 flow rate is 3400-4200 sccm.

4. The boron doping method for N-type crystalline silicon cells according to claim 1, characterized in that: The deposition temperature in the deposition one / deposition two / deposition three steps is in a step-growth state, wherein the deposition three temperature> the deposition two temperature> the deposition one temperature. The deposition times in the deposition one, deposition two and deposition three steps are different, wherein the deposition two time> the deposition one temperature> the deposition three temperature.

5. The boron doping method for N-type crystalline silicon cells according to claim 1, characterized in that: The S5 push junction temperature is 920-950°C, the constant pressure is 150-300mba, and the N2 flow rate is 2000-4000sccm.

6. The boron doping method for N-type crystalline silicon cells according to claim 1, characterized in that: The pushing and knotting is completed in two steps, and the pushing and knotting time is 480-580s respectively.

7. The boron doping method for N-type crystalline silicon cells according to claim 1, characterized in that: The S6 oxidation advancement temperature is 995-1005° C., the constant pressure is 250-1000 mba, the O2 flow rate is 12000-25000 sccm, and the oxidation advancement is completed in two steps, with oxidation advancement times of 800-950 s and 600-630 s respectively.

8. A process for preparing an N-type crystalline silicon cell, characterized in that: The method for boron doping of an N-type crystalline silicon cell is applied as claimed in any one of claims 1 to 8.

9. The process for preparing an N-type crystalline silicon cell according to claim 8, characterized in that: The following steps are involved: Step 1: Texturing and cleaning of N-type silicon wafers; Step 2: Boron diffusion to form a low-compound shallow doping region, and BSG is formed on the boron diffusion surface; Step 3: back polishing; Step 4: Prepare an oxide tunneling layer and a phosphorus-doped amorphous silicon layer by PECVD, wherein the phosphorus-doped amorphous silicon layer has a thickness of 75-100 nm; Step 5: high temperature annealing and crystallization to activate phosphorus atoms, the crystallization annealing temperature is 980-1020°C; Step 6: Clean the back side and remove PSG and edge wrapping; Step 7: depositing a passivation film on both sides, wherein the passivation layer is a stack of two or more layers of AlOx, SiNx, SiOx, and SiONx; Step 8: Printing metal electrodes and sintering; Step 9. Optimize front contact through laser enhanced contact.

10. The boron doping method for N-type crystalline silicon cells according to claim 9, characterized in that: The boron diffusion doping source is BCl3.