Electrode plate and preparation method thereof, secondary battery and electric device

By using ion trapping agent and insulating layer in the secondary battery electrode sheet, the reduction of structural stability and interface mask decomposition caused by transition metal ion dissolution is solved, the cycle performance and life of the battery is significantly improved, and acidic substances are removed Further improve battery performance.

CN119069624AActive Publication Date: 2024-12-03CONTEMPORARY AMPEREX TECHNOLOGY CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202310637388.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-31
Publication Date
2024-12-03
Estimated Expiration
2043-05-31

AI Technical Summary

Technical Problem

Existing secondary batteries have transition metal ion dissolution problems in the electrochemical environment, resulting in reduced structural stability of the positive electrode material and decomposition of the negative electrode interface mask, affecting battery life and performance.

Method used

An electrode sheet is designed, and the coating includes an ion trapping agent. The reduction potential of the ion trapping agent relative to lithium metal is 0 to 2V. It can reduce the transition metal ions into low-priced state or metal element that is not easy to dissolve, and pass the insulation. The layer isolates the active material layer, reducing the direct contact between the ion trapping agent and the electrode active material, and reducing the risk of redox activity.

Benefits of technology

It effectively improves the circulation performance of the secondary battery, extends the battery life, and further improves the battery performance by removing the acidic substances in the electrolyte.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119069624A_ABST
    Figure CN119069624A_ABST
Patent Text Reader

Abstract

The embodiment of the invention provides an electrode plate, a preparation method of the electrode plate, a secondary battery and a power utilization device. The electrode plate comprises a current collector; an active material layer disposed on at least one surface of the current collector; an insulating layer disposed on the active material layer; and a coating layer disposed on the insulating layer, the coating layer including an ion scavenger, the reduction potential of the ion scavenger with respect to the lithium metal being 0-2 V. The cycle performance of the secondary battery containing the electrode plate is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field The present application relates to the field of battery technology, and in particular to an electrode plate and a preparation method thereof, a secondary battery and an electrical device. Background Art In recent years, secondary batteries have been widely used in energy storage power systems such as hydropower, thermal power, wind power and solar power stations, as well as power tools, electric bicycles, electric motorcycles, electric vehicles, military equipment, aerospace and other fields due to their high energy density and recyclability. With the great development and wide application of secondary batteries, higher requirements have been put forward for their electrochemical performance. Therefore, how to provide a secondary battery with good performance is a technical problem that needs to be solved urgently. Summary of the invention The present application is made in view of the above-mentioned technical problems, and its purpose is to provide an electrode plate and a preparation method thereof, a secondary battery and an electrical device, wherein the cycle performance of the secondary battery containing the electrode plate is improved. In a first aspect, the present application provides an electrode plate, comprising: a current collector; an active material layer, disposed on at least one surface of the current collector; an insulating layer, disposed on the active material layer; a coating, disposed on the insulating layer, and the coating comprises an ion capture agent, and the reduction potential of the ion capture agent relative to lithium metal is 0 to 2V. In the embodiment of the present application, the coating of the electrode plate includes an ion capture agent, and the reduction potential of the ion capture agent relative to lithium metal is 0 to 2V. The positive electrode material is an important component of the secondary battery and directly affects the performance of the secondary battery. The positive electrode material containing transition metals will inevitably undergo the phenomenon of transition metal ion dissolution in the electrochemical environment. On the one hand, the dissolved transition metal ions destroy the structural stability of the original positive electrode material and thus affect the life of the secondary battery. On the other hand, the dissolved transition metal ions will migrate and deposit on the surface of the negative electrode material, catalyzing the decomposition and regeneration of the electrolyte and the negative electrode interface film, continuously consuming reversible active metals, and ultimately leading to a decrease in the performance of the secondary battery. In the technical solution of the embodiment of the present application, the reduction potential of the ion capture agent in the coating of the electrode plate relative to lithium metal is 0 to 2V, and the reduction potential of the transition metal ions relative to lithium metal is generally above 2V. Therefore, the ion capture agent can reduce the transition metal ions dissolved in the secondary battery into low-valent ions that are not easily dissolved, or into metal elements, thereby improving the situation where the transition metal ions catalyze the decomposition of the electrolyte and the negative electrode interface film, thereby improving the cycle performance of the secondary battery. In addition, due to H + The reduction potential of ions relative to lithium metal is higher than that of transition metal ions relative to lithium metal, so the ion scavenger can also convert H in the battery cell into + Reduction, that is, removing acidic substances in the electrolyte (such as HF, organic acid RH+ , H· free radicals, etc.), further improving the performance of the secondary battery. The electrode plate is provided with a coating containing an ion capture agent, and an insulating layer is provided to isolate the active material layer and the coating, reducing the possibility of direct contact between the ion capture agent and the electrode active material, thereby reducing the risk of the ion capture agent losing its redox activity and reducing the risk of the ion capture agent affecting the performance of the electrode active material. In a possible implementation, the ion capture agent includes at least one of an active metal and an alkali metal compound. Optionally, the active metal includes at least one of Li, Na, K, Rb, Cs, Fr, Mg, Ca, Sr, Ba, Al, Ti or V; Optionally, the active metal includes at least one of Li, Na, Mg, Al, Ti or V; Optionally, the alkali metal compound includes A 1 x B, A 2 y Ti5O 12 , and at least one of the compounds represented by formula (I), formula (II) or formula (III): RA 3 (I) Among them, A 1 , A 2 , A 3 , A 4 , A 5 , A 6 Each independently includes at least one of Li, Na or K, B includes C, Si or Sn, x≥0.05, y>4, R, R1, R2, R3, and R4 independently include a hydrogen atom, an alkyl group having 1 to 20 carbon atoms, an alkyl group having 1 to 20 carbon atoms substituted by a sulfonic acid group or a sulfonyl group, an alkenyl group having 2 to 20 carbon atoms, an alkenyl group having 2 to 20 carbon atoms substituted by a sulfonic acid group or a sulfonyl group, an alkenyl group having 6 to 8 carbon atoms, The present invention further comprises at least one of an aryl group having 6 to 26 carbon atoms, an aryl group having 6 to 26 carbon atoms substituted by a sulfonic acid group or a sulfonyl group, a carboxyl group having 1 to 20 carbon atoms, a carboxyl group having 1 to 20 carbon atoms substituted by a sulfonic acid group or a sulfonyl group, a carbonyl group having 1 to 20 carbon atoms, a carbonyl group having 1 to 20 carbon atoms substituted by a sulfonic acid group or a sulfonyl group, an aryloxy group having 6 to 26 carbon atoms, and an aryloxy group having 6 to 26 carbon atoms substituted by a sulfonic acid group or a sulfonyl group. In a possible implementation, the A 1 x B includes Li 1 / 6 C. Na 1 / 6 C.K 1 / 8 C. Li 4.4 Si, or Li 4.4 At least one of Sn. In a possible implementation, 5≤y≤7, the A 2 y Ti5O 12 Including Li7Ti5O 12 or Na7Ti5O 12 At least one of . In a possible implementation, the compound represented by formula (I) includes at least one of n-butyl lithium, naphthyl lithium or biphenyl lithium. In a possible implementation, the compound represented by formula (II) comprises At least one of . In a possible implementation, the compound represented by formula (III) comprises At least one of . In a possible implementation, the mass proportion of the ion capture agent in the coating is 50% to 99%. Optionally, the mass proportion of the ion capture agent in the coating is 80% to 98%. The mass proportion of the ion capture agent in the coating is within the given range, and the ion capture agent can play a good role in reducing transition metal ions, thereby further improving the cycle performance of the battery. In a possible implementation, the thickness d1 of the coating is 0.01 μm to 20 μm. Optionally, d1 is 0.1 μm to 10 μm. If the coating thickness is too small, the content of the ion capture agent in the electrode plate is too small, and the ion capture agent cannot play a good role in chemically reducing transition metal ions; if the coating thickness is too large, it will hinder the migration of active metal ions in the active material of the electrode plate, and deteriorate the performance of the secondary battery, for example, affecting the cycle performance of the secondary battery. Therefore, setting the coating thickness to 0.01μm to 20μm is conducive to improving the performance of the secondary battery. In a possible implementation manner, the thickness d2 of the insulating layer is 0.01 μm to 20 μm. Optionally, d2 is 0.1 μm to 10 μm. If the thickness of the insulating layer is too small, it cannot play a good role in isolating the ion capture agent and the electrode active material; if the thickness of the insulating layer is too large, it will hinder the migration of active metal ions in the active material of the electrode plate, deteriorating the performance of the secondary battery, for example, affecting the cycle performance of the secondary battery. Therefore, setting the thickness of the insulating layer to 0.01μm to 20μm is conducive to improving the performance of the secondary battery. In one possible implementation, the coating also includes a binder; optionally, the binder includes at least one of polyacrylate, polyacrylic acid, polytetrafluoroethylene, polyvinylidene fluoride, vinylidene fluoride-trichloroethylene copolymer, polyvinyl pyrrolidone, polyvinyl acetate, ethylene-vinyl acetate copolymer, polyethylene oxide, polyarylate, carboxymethyl cellulose, hydroxypropyl cellulose, regenerated cellulose, cellulose acetate, cellulose acetate propionate, cellulose acetate butyrate, polyacrylonitrile, polyvinyl alcohol, polyethylene, polypropylene, starch, or cyanoethyl pullulan. The ion capture agent in the coating layer can be bonded to the active material layer through the adhesive, so that there is good bonding force between the ion capture agent and the active material layer, so as to improve the overall structural strength of the electrode plate. In a possible implementation, the coating further includes a filler; Optionally, the filler includes at least one of inorganic particles, organic particles, or organic-metal framework materials; optionally, the inorganic particles include at least one of inorganic particles having a dielectric constant of 5 or more or inorganic particles having ion conductivity but not storing ions; optionally, the organic particles include at least one of polycarbonate, polythiophene, polypyridine, polystyrene, polyacrylic wax, polyethylene, polypropylene, cellulose, cellulose modifier, melamine resin, phenolic resin, polyester, silicone resin, polyimide, polyamideimide, polyaromatic amide, polyphenylene sulfide, polysulfone, polyethersulfone, polyetheretherketone, polyaryletherketone, or a copolymer of butyl acrylate and ethyl methacrylate; optionally, the organic-metal framework material includes at least one of a nitrogen-containing heterocyclic ligand building structure, an organic carboxylic acid ligand building structure, and a nitrogen-oxygen mixed ligand building structure. Fillers are added to the coating to provide pores in the coating for ions to pass through, thereby improving the cycle performance of the secondary battery. In one possible implementation, the insulating layer includes at least one of inorganic particles, organic particles, or an organic-metal framework material; optionally, the inorganic particles include at least one of inorganic particles having a dielectric constant of 5 or more or inorganic particles having ion conductivity but not storing ions; optionally, the organic particles include at least one of polycarbonate, polythiophene, polypyridine, polystyrene, polyacrylic wax, polyethylene, polypropylene, cellulose, cellulose modifier, melamine resin, phenolic resin, polyester, silicone resin, polyimide, polyamideimide, polyaromatic amide, polyphenylene sulfide, polysulfone, polyethersulfone, polyetheretherketone, polyaryletherketone, or a copolymer of butyl acrylate and ethyl methacrylate; optionally, the organic-metal framework material includes at least one of a nitrogen-containing heterocyclic ligand building structure, an organic carboxylic acid ligand building structure, and a nitrogen-oxygen mixed ligand building structure. The insulating materials provided by the above technical solutions all have good insulating properties and can play a good role in electronic insulation and isolating ion capture agents and electrode active materials. In a second aspect, a method for preparing an electrode pole piece is provided, comprising: providing a current collector; providing an active material slurry, coating the active material slurry on at least one surface of the current collector to form an active material layer; providing an insulating slurry, coating the insulating slurry on the active material layer to form an insulating layer; providing a coating slurry, the coating slurry comprising an ion capture agent, the ion capture agent having a reduction potential of 0 to 2 V relative to lithium metal, coating the coating slurry on the insulating layer to obtain an electrode pole piece. In a third aspect, a secondary battery is provided, comprising the electrode plate in the first aspect and any possible implementation thereof. In a fourth aspect, an electrical device is provided, comprising the secondary battery described in the third aspect. The embodiment of the present application provides an electrode plate, the coating of the electrode plate includes an ion capture agent, and the reduction potential of the ion capture agent relative to lithium metal is 0 to 2V. The positive electrode material is an important component of the secondary battery and directly affects the performance of the secondary battery. The positive electrode material containing transition metals will inevitably undergo the phenomenon of transition metal ion dissolution in the electrochemical environment. On the one hand, the dissolved transition metal ions destroy the structural stability of the original positive electrode material and thus affect the life of the secondary battery. On the other hand, the dissolved transition metal ions will migrate and deposit on the surface of the negative electrode material, catalyzing the decomposition and regeneration of the electrolyte and the negative electrode interface film, continuously consuming reversible active metals, and ultimately leading to a decrease in the performance of the secondary battery. In the technical solution of the embodiment of the present application, the reduction potential of the ion capture agent in the coating of the electrode plate relative to lithium metal is 0 to 2V, and the reduction potential of the transition metal ions relative to lithium metal is generally above 2V. Therefore, the ion capture agent can reduce the transition metal ions dissolved in the secondary battery into low-valent ions that are not easily dissolved, or into metal elements, thereby improving the situation where the transition metal ions catalyze the decomposition of the electrolyte and the negative electrode interface film, thereby improving the cycle performance of the secondary battery. In addition, due to H + The reduction potential of ions relative to lithium metal is higher than that of transition metal ions relative to lithium metal, so the ion scavenger can also convert H in the battery cell into + Reduction, that is, removing acidic substances in the electrolyte (such as HF, organic acid RH + , H· free radicals, etc.), further improving the performance of the secondary battery. The electrode plate is provided with a coating containing an ion capture agent, and an insulating layer is provided to isolate the active material layer and the coating, reducing the possibility of direct contact between the ion capture agent and the electrode active material, thereby reducing the risk of the ion capture agent losing its redox activity and reducing the risk of the ion capture agent affecting the performance of the electrode active material. BRIEF DESCRIPTION OF THE DRAWINGS In order to more clearly illustrate the technical solutions of the embodiments of the present application, the drawings required for use in the embodiments of the present application will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present application. For ordinary technicians in this field, other drawings can be obtained based on the drawings without paying creative work. Figure 1 A schematic diagram of an electrode plate according to an embodiment of the present application; Figure 2 A schematic diagram of an electrode plate according to an embodiment of the present application; Figure 3 A schematic diagram of an electrode plate according to an embodiment of the present application; Figure 4 A schematic diagram of a method for preparing an electrode sheet according to an embodiment of the present application; Figure 5 is a schematic diagram of a secondary battery disclosed in one embodiment of the present application; Figure 6 is a schematic diagram of the exploded structure of a secondary battery disclosed in one embodiment of the present application; Figure 7 is a structural schematic diagram of a battery module disclosed in an embodiment of the present application; Figure 8 is a schematic diagram of the exploded structure of a battery pack disclosed in one embodiment of the present application; Fig. 9 It is a schematic diagram of an electrical device disclosed in one embodiment of the present application. In the drawings, the drawings are not drawn to scale. DETAILED DESCRIPTION Below, the embodiments of the electrode plates, battery cells, batteries and electrical devices of the present application are specifically disclosed in detail with appropriate reference to the accompanying drawings. However, there may be cases where unnecessary detailed descriptions are omitted. For example, there are cases where detailed descriptions of well-known matters and repeated descriptions of actually the same structures are omitted. This is to avoid the following description from becoming unnecessarily lengthy and to facilitate the understanding of those skilled in the art. In addition, the drawings and the following descriptions are provided for those skilled in the art to fully understand the present application and are not intended to limit the subject matter described in the claims. In the description of this application, it should be noted that, unless otherwise specified, "multiple" means more than two; the terms "upper", "lower", "left", "right", "inner", "outer", etc., indicating directions or positional relationships, are only for the convenience of describing this application and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific direction, be constructed and operated in a specific direction, and therefore cannot be understood as limiting this application. In addition, the terms "first", "second", "third", etc. are only used for descriptive purposes and cannot be understood as indicating or implying relative importance. "Scope" disclosed in the present application is limited in the form of lower limit and upper limit, and a given range is limited by selecting a lower limit and an upper limit, and the selected lower limit and upper limit define the boundary of a special range. The scope limited in this way can be including end values ​​or not including end values, and can be arbitrarily combined, that is, any lower limit can be combined with any upper limit to form a scope. For example, if the scope of 60-120 and 80-110 is listed for a specific parameter, it is understood that the scope of 60-110 and 80-120 is also expected. In addition, if the minimum range values ​​1 and 2 are listed, and if the maximum range values ​​3, 4 and 5 are listed, the following scope can be all expected: 1-3, 1-4, 1-5, 2-3, 2-4 and 2-5. In the present application, unless otherwise specified, the numerical range "ab" represents the abbreviation of any real number combination between a and b, wherein a and b are real numbers. For example, the numerical range "0-5" means that all real numbers between "0-5" are listed in this document, and "0-5" is just an abbreviation of these numerical combinations. In addition, when a parameter is expressed as an integer ≥ 2, it is equivalent to disclosing that the parameter is, for example, an integer of 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, etc. If there is no special explanation, all steps of the present application can be performed sequentially or randomly, preferably sequentially. For example, the method includes steps (a) and (b), which means that the method may include steps (a) and (b) performed sequentially, or may include steps (b) and (a) performed sequentially. For example, the method may further include step (c), which means that step (c) may be added to the method in any order. For example, the method may include steps (a), (b) and (c), or may include steps (a), (c) and (b), or may include steps (c), (a) and (b), etc. If there is no special explanation, the "include" and "comprising" mentioned in this application represent open-ended. For example, the "include" and "comprising" may mean including or comprising other components not listed. If not specifically stated, in this application, the term "and / or" is inclusive. For example, the phrase "A and / or B" means "A, B, or both A and B". More specifically, any of the following conditions satisfies the condition "A and / or B": A is true (or exists) and B is false (or does not exist); A is false (or does not exist) and B is true (or exists); or both A and B are true (or exist). If not otherwise specified, all embodiments and optional embodiments of the present application can be combined with each other to form a new technical solution. Unless otherwise specified, all technical features and optional technical features of this application can be combined with each other to form a new technical solution. Unless otherwise specified, the following terms have the following meanings. Any undefined terms have their generally accepted meanings in the art. "Alkyl" refers to a monovalent saturated hydrocarbon group having one or more carbon atoms, optionally with a carbon number of 1 to 20. For example, alkyl includes straight chain hydrocarbon groups and branched hydrocarbon groups, such as methyl (CH3-), ethyl (CH3CH2-), n-propyl (CH3CH2CH2-), isopropyl ((CH3)2CH-), n-butyl (CH3CH2CH2CH2-), isobutyl ((CH3)2CHCH2-), sec-butyl ((CH3)(CH3CH2)CH-), tert-butyl ((CH3)3C-), n-pentyl (CH3CH2CH2CH2CH2-), neopentyl ((CH3)3CCH2-), etc. "Alkenyl" refers to a straight or branched hydrocarbon group having one or more carbon atoms and at least one double bond unsaturated site, optionally with 2 to 20 carbon atoms, such as vinyl (CH2=CH-), propenyl (CH3CH=CH-), allyl (CH2=CH-CH2-), n-butenyl (-CH3CH2CH=CH-), etc. "Aryl" refers to an aromatic compound having a single ring or multiple condensed rings, optionally with 6 to 26 carbon atoms. For example, aryl includes phenyl, naphthyl, indenyl, etc. Aryl also includes a single ring fused to an aryl, for example, tetrahydronaphthyl, 2,3-dihydroindanyl, etc. "Carboxyl" refers to a group having one or more carbon atoms and having a -CO2H functional group, and optionally, the number of carbon atoms is 1 to 20. "Carbonyl" refers to a group having one or more carbon atoms and having a -CO- functional group, and optionally, the number of carbon atoms is 1 to 20. "Aryloxy" refers to a group formed by connecting at least one carbon atom on the aromatic ring of an aryl group to an oxygen atom, and optionally, the number of carbon atoms is 6 to 26. "Sulfonic acid" refers to -SO3H. "Sulfonyl" refers to RS(=O)2-, wherein R includes hydrogen atom, alkyl, alkenyl, alkynyl, aryl, cycloalkyl, cycloalkenyl, heteroaryl, heterocyclic group and the like. A secondary battery is a battery that can be used again after being discharged by recharging the active materials. Usually, a secondary battery includes a positive electrode, a negative electrode, a separator and an electrolyte. During the battery charging and discharging process, active ions are embedded and released back and forth between the positive electrode and the negative electrode. The separator is set between the positive electrode and the negative electrode to play an isolating role. The electrolyte plays the role of conducting ions between the positive electrode and the negative electrode. Due to their high energy density and recyclability, secondary batteries are widely used in energy storage power systems such as hydropower, thermal power, wind power and solar power stations, as well as power tools, electric bicycles, electric motorcycles, electric vehicles, military equipment, aerospace and other fields. With the great development and wide application of secondary batteries, higher requirements are also put forward for their energy density, cycle performance, discharge capacity and other performance. Positive electrode materials are one of the key materials that determine the performance of secondary batteries, mainly including metal oxides and polyanion salts, among which layered metal oxides and spinel metal oxides containing transition metals are widely used as positive electrode materials. The above-mentioned positive electrode materials containing transition metals have the advantages of high energy density and good cycle performance, which are beneficial to improving the performance of secondary batteries. However, transition metal ions will inevitably dissolve in the electrochemical environment of positive electrode materials containing transition metals. On the one hand, the dissolved transition metal ions destroy the structural stability of the original positive electrode materials and thus affect the life of the secondary battery. On the other hand, the dissolved transition metal ions will migrate and deposit on the surface of the negative electrode material, catalyzing the decomposition and regeneration of the electrolyte and the negative electrode interface film, continuously consuming reversible active metals, and ultimately leading to a decline in the performance of the secondary battery. In view of this, the embodiment of the present application provides an electrode plate, which includes a current collector; an active material layer, which is arranged on at least one surface of the current collector; an insulating layer, which is arranged on the active material layer; a coating, which is arranged on the insulating layer, and the coating includes an ion capture agent, the reduction potential of the ion capture agent relative to lithium metal is 0 to 2V, and the reduction potential of transition metal ions relative to lithium metal is generally above 2V, so the ion capture agent can reduce the transition metal ions dissolved in the secondary battery into low-valent ions that are not easily dissolved, or reduce them to metal elements, thereby improving the situation where the transition metal ions catalyze the decomposition of the electrolyte and the negative electrode interface film, thereby improving the cycle performance of the secondary battery. In addition, due to H + The reduction potential of ions relative to lithium metal is higher than that of transition metal ions relative to lithium metal, so the ion scavenger can also convert H in the battery cell into + Reduction, that is, removing acidic substances in the electrolyte (such as HF, organic acid RH+ , H· free radicals, etc.), further improving the performance of the secondary battery. The electrode plate is provided with a coating containing an ion capture agent, and an insulating layer is provided to isolate the active material layer and the coating, reducing the possibility of direct contact between the ion capture agent and the electrode active material, thereby reducing the risk of the ion capture agent losing its redox activity and reducing the risk of the ion capture agent affecting the performance of the electrode active material. [Electrode Plate] Figure 1 FIG. 1 is a schematic diagram of an electrode plate 1 according to an embodiment of the present application. Figure 1 As shown, the electrode plate 1 includes a current collector 11, an active material layer 12, which is disposed on at least one surface of the current collector 11, an insulating layer 14, which is disposed on the active material layer 12, and a coating 13, which is disposed on the insulating layer 14. For example, along the thickness direction of the electrode plate 1 (for example, Figure 1 The current collector 11, the active material layer 12, the insulating layer 14 and the coating layer 13 are sequentially arranged. The coating layer 13 includes an ion trapping agent, and the reduction potential of the ion trapping agent relative to lithium metal is 0 to 2V. The electrode plate provided in the embodiment of the present application can be a positive electrode plate or a negative electrode plate. The ion capture agent mentioned here refers to a class of substances that can consume free transition metal ions in secondary batteries. The reduction potential of the ion capture agent relative to lithium metal is 0 to 2V, while the reduction potential of transition metal ions relative to lithium metal is generally above 2V. Therefore, the reducibility of the ion capture agent is stronger than that of the transition metal ions. The ion capture agent can reduce the free transition metal ions into low-valent ions that are not easily dissolved in the electrolyte, or reduce them into metal elements. The positive electrode material is an important component of the secondary battery and directly affects the performance of the secondary battery. The positive electrode material containing transition metals will inevitably dissolve transition metal ions in the electrochemical environment. On the one hand, the dissolved transition metal ions destroy the structural stability of the original positive electrode material and thus affect the life of the secondary battery. On the other hand, the dissolved transition metal ions will migrate and deposit on the surface of the negative electrode material, catalyzing the decomposition and regeneration of the electrolyte and the negative electrode interface film, continuously consuming reversible active metals, and ultimately leading to a decrease in the performance of the secondary battery. The electrode plate is provided with a coating containing an ion scavenger, and an insulating layer is provided to isolate the active material layer and the coating, reducing the possibility of direct contact between the ion scavenger and the electrode active material, thereby reducing the risk of the ion scavenger losing its redox activity and reducing the risk of the ion scavenger affecting the performance of the electrode active material. For example, the positive electrode material may include a phosphate material with an olivine structure, a material with a spinel structure, and a transition metal oxide with a layered structure. Specifically, for example, lithium iron phosphate (LiFePO4), lithium iron manganese phosphate (LiMnFePO4), lithium manganate (LiMn2O4), ternary materials, etc. The iron ions, nickel ions, manganese ions, etc. in the above positive electrode materials all have the phenomenon of dissolving from the positive electrode materials. The coating of the electrode plate provided in the embodiment of the present application includes an ion capture agent, and the reduction potential of the ion capture agent relative to lithium metal is 0 to 2V, while the reduction potential of transition metal ions relative to lithium metal is generally above 2V. Therefore, the ion capture agent can reduce the transition metal ions dissolved in the secondary battery into low-valent ions that are not easily dissolved, or into metal elements, thereby improving the situation where the transition metal ions catalyze the decomposition of the electrolyte and the negative electrode interface film, thereby improving the cycle performance of the secondary battery. In addition, due to H + The reduction potential of ions relative to lithium metal is higher than that of transition metal ions relative to lithium metal, so the ion scavenger can also convert H in the battery cell into + Reduction, that is, removing acidic substances in the electrolyte (such as HF, organic acid RH + , H· free radicals, etc.), further improving the performance of secondary batteries. It should be understood that in the embodiments of the present application, different types of ion capture agents can be selected according to different types of free transition metal ions dissolved in the secondary battery. Optionally, in some embodiments, the ion capture agent includes at least one of a compound of an active metal and an alkali metal. Specifically, the active metal may include at least one of Li, Na, K, Rb, Cs, Fr, Mg, Ca, Sr, Ba, Al, Ti or V. Optionally, the active metal includes at least one of Li, Na, Mg, Al, Ti or V. Optionally, the alkali metal compound comprises A 1 x B, A 2 y Ti5O 12 , and at least one of the compounds represented by formula (I), formula (II) or formula (III): RA 3 (I) Among them, A 1 , A 2 , A 3 , A 4 , A 5 , A 6Each independently includes at least one of Li, Na or K, B includes C, Si or Sn, x≥0.05, y>4, R, R1, R2, R3, and R4 independently include a hydrogen atom, an alkyl group having 1 to 20 carbon atoms, an alkyl group having 1 to 20 carbon atoms substituted by a sulfonic acid group or a sulfonyl group, an alkenyl group having 2 to 20 carbon atoms, an alkenyl group having 2 to 20 carbon atoms substituted by a sulfonic acid group or a sulfonyl group, an alkenyl group having 6 to 8 carbon atoms, The present invention further comprises at least one of an aryl group having 6 to 26 carbon atoms, an aryl group having 6 to 26 carbon atoms substituted by a sulfonic acid group or a sulfonyl group, a carboxyl group having 1 to 20 carbon atoms, a carboxyl group having 1 to 20 carbon atoms substituted by a sulfonic acid group or a sulfonyl group, a carbonyl group having 1 to 20 carbon atoms, a carbonyl group having 1 to 20 carbon atoms substituted by a sulfonic acid group or a sulfonyl group, an aryloxy group having 6 to 26 carbon atoms, and an aryloxy group having 6 to 26 carbon atoms substituted by a sulfonic acid group or a sulfonyl group. In the embodiments of the present application, the dotted line in formula (II) indicates that R1 and R2 may be connected to form a ring or may not be connected; the dotted line in formula (III) indicates that R3 and R4 may be connected to form a ring or may not be connected. Optionally, A 1 x B includes LiC6, NaC6, KC8, Li 4.4 Si, Li 4.4 Sn or Li 22 At least one of Si5. In the present application embodiment, A 1 x The value of x in B is related to the specific substance selected for B. For example, when B is carbon (C), the upper limit of the value of x is 1 / 6; for another example, when B is silicon (Si) or tin (Sn), the upper limit of the value of x is 4.4. Optionally, 5≤y≤7, A 2 y Ti5O 12 Including Li7Ti5O 12 or Na7Ti5O 12 At least one of . Optionally, the compound represented by formula (I) includes at least one of n-butyllithium, naphthyllithium or biphenyllithium. Optionally, the compound represented by formula (II) comprises At least one of . Optionally, the compound represented by formula (III) comprises At least one of . The current collector 11 is a structure for collecting current of the electrode plate 1. Its main function is to collect the current generated by the electroactive material to form a larger current for external output. Therefore, the current collector 11 should be in full contact with the active material, and the internal resistance should be as small as possible. Alternatively, the current collector 11 may be a metal foil or a composite current collector. For example, the composite current collector may include a polymer material base and a metal layer formed on at least one surface of the polymer material base. The composite current collector may be formed by forming a metal material (aluminum, aluminum alloy, nickel, nickel alloy, titanium, titanium alloy, silver and silver alloy, etc.) on a polymer material substrate (such as a substrate of polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), polyethylene (PE), etc.). For another example, as a metal foil, the positive electrode current collector may be aluminum foil, and the negative electrode current collector may be copper foil. Optionally, the active material provided by the active material layer 12 may adopt active materials for secondary batteries that are well known in the art. For example, in a lithium-ion battery, the positive electrode active material may include at least one of the following materials: lithium-containing phosphates with an olivine structure, lithium transition metal oxides, and their respective modified compounds. However, the present application is not limited to these materials, and other traditional materials that can be used as positive electrode active materials for lithium-ion batteries may also be used. These positive electrode active materials may be used alone or in combination of two or more. Among them, examples of lithium transition metal oxides may include, but are not limited to, lithium cobalt oxide (such as LiCoO2), lithium nickel oxide (such as LiNiO2), lithium manganese oxide (such as LiMnO2, LiMn2O4), lithium nickel cobalt oxide, lithium manganese cobalt oxide, lithium nickel manganese oxide, lithium nickel cobalt manganese oxide (such as LiNi 1 / 3 Co 1 / 3 Mn 1 / 3 O2 (also referred to as NCM333), LiNi 0.5 Co 0.2 Mn 0.3 O2 (also referred to as NCM523), LiNi 0.5 Co 0.25 Mn 0.25 O2 (also referred to as NCM211), LiNi 0.6 Co 0.2 Mn 0.2 O2 (also referred to as NCM622), LiNi 0.8 Co 0.1 Mn 0.1 O2 (also referred to as NCM811), lithium nickel cobalt aluminum oxide (such as LiNi 0.85 Co 0.15 Al 0.05O2) and its modified compounds, etc. Examples of lithium-containing phosphates with an olivine structure may include, but are not limited to, at least one of lithium iron phosphate (such as LiFePO4 (also referred to as LFP)), a composite material of lithium iron phosphate and carbon, lithium manganese phosphate (such as LiMnPO4), a composite material of lithium manganese phosphate and carbon, lithium iron manganese phosphate, and a composite material of lithium iron manganese phosphate and carbon. For another example, in a lithium-ion battery, the negative electrode active material may include at least one of the following materials: artificial graphite, natural graphite, soft carbon, hard carbon, silicon-based materials, tin-based materials, lithium titanate, etc. The silicon-based material may be selected from at least one of elemental silicon, silicon oxide compounds, silicon-carbon composites, silicon-nitrogen composites, and silicon alloys. The tin-based material may be selected from at least one of elemental tin, tin oxide compounds, and tin alloys. However, the present application is not limited to these materials, and other traditional materials that can be used as negative electrode active materials for batteries may also be used. These negative electrode active materials may be used alone or in combination of two or more. The current collector 11 has two surfaces arranged along its thickness direction. Figure 1 As shown, active material layers 12 are provided on both surfaces of the current collector 11. On both sides of the current collector 11, along the thickness direction of the electrode plate 1 (for example, Figure 1 (z direction in the drawing) the active material layer 12, the insulating layer 14 and the coating layer 13 are arranged in sequence. Figure 2 Schematic diagram of an electrode plate of an embodiment of the present application. In some other embodiments, such as Figure 2 As shown, one of the two surfaces of the current collector 11 opposite to each other in the thickness direction is provided with an active material layer 12. On one side of the current collector 11, along the thickness direction of the electrode plate 1 (for example, Figure 2 (z direction in the figure) the active material layer 12, the insulating layer 14 and the coating layer 13 are arranged in sequence. Optionally, in some embodiments, the mass proportion of the ion capture agent in the coating 13 is 50% to 99%. Optionally, the mass proportion of the ion capture agent in the coating 13 is 80% to 98%. Specifically, the mass proportion of the ion capture agent in the coating 13 can be 50%, 60%, 70%, 80%, 90%, 96%, 98%, 99%, or a value between any two of the above values. The mass proportion of the ion capture agent in the porous coating is within the given range, and the ion capture agent can play a good role in reducing transition metal ions, thereby further improving the cycle performance of the battery. Optionally, in some embodiments, Figure 1-2 As shown, the thickness d2 of the insulating layer 14 is 0.01 μm to 20 μm, and optionally, d2 is 0.1 μm to 10 μm. Specifically, the thickness d2 of the insulating layer 14 may be 0.01 μm, 0.05 μm, 0.1 μm, 0.5 μm, 1 μm, 5 μm, 10 μm, 15 μm, 20 μm, or a value between any two of the above values. If the thickness of the insulating layer is too small, it cannot play a good role in isolating the ion capture agent and the electrode active material; if the thickness of the insulating layer is too large, it will hinder the migration of active metal ions in the active material of the electrode plate 1, deteriorating the performance of the secondary battery, for example, affecting the cycle performance of the secondary battery. Therefore, setting the thickness of the insulating layer 14 to 0.01μm to 20μm is conducive to improving the performance of the secondary battery. Optionally, in some embodiments, the coating 13 may be disposed on at least one side of the current collector 11. Figure 3 As shown, both surfaces of the current collector 11 are provided with a coating 13, and the active material layer 12 is provided on the coating 13. For example, along the thickness direction of the electrode plate 1 ( Figure 3 The current collector 11, the coating layer 13 and the active material layer 12 are arranged in sequence. Optionally, in some embodiments, Figure 1-3 As shown, the thickness d1 of the coating 13 is 0.01 μm to 20 μm, and optionally, d1 is 0.1 μm to 10 μm. Specifically, the thickness d1 of the coating 13 may be 0.01 μm, 0.05 μm, 0.1 μm, 0.5 μm, 1 μm, 5 μm, 10 μm, 15 μm, 20 μm, or a value between any two of the above values. If the thickness of the coating 13 is too small, the content of the ion capture agent in the electrode plate 1 is too small, and the ion capture agent cannot play a good role in reducing the transition metal ions through chemical reactions; if the thickness of the coating 13 is too large, it will hinder the migration of active metal ions in the active material of the electrode plate 1, and deteriorate the performance of the secondary battery, for example, affecting the cycle performance of the secondary battery. Therefore, setting the thickness of the coating 13 to 0.01 μm to 20 μm is conducive to improving the performance of the secondary battery. As mentioned above, the thickness of the material can be measured by a micrometer. The thickness of the material at multiple different positions is measured using the micrometer, and the average value of the multiple measurement results is recorded as the final thickness. The material thickness in the embodiment of the present application can be measured by the above method, but is not limited to the above method. For example, it can also be measured by spectroscopy. The specific detection method can refer to the well-known method of measuring thickness by spectroscopy. Optionally, in some embodiments, the coating 13 further includes a binder. Optionally, the binder includes at least one of polyacrylate, polyacrylic acid, polytetrafluoroethylene, polyvinylidene fluoride, vinylidene fluoride-trichloroethylene copolymer, polyvinyl pyrrolidone, polyvinyl acetate, ethylene-vinyl acetate copolymer, polyethylene oxide, polyarylate, carboxymethyl cellulose, hydroxypropyl cellulose, regenerated cellulose, cellulose acetate, cellulose acetate propionate, cellulose acetate butyrate, polyacrylonitrile, polyvinyl alcohol, polyethylene, polypropylene, starch, or cyanoethyl pullulan. Optionally, in some embodiments, the insulating layer 14 includes at least one of inorganic particles, organic particles, or an organic-metal framework material; Optionally, the inorganic particles include at least one of inorganic particles having a dielectric constant of 5 or more or inorganic particles having ion conductivity but not storing ions; Optionally, the organic particles include at least one of polycarbonate, polythiophene, polypyridine, polystyrene, polyacrylic wax, polyethylene, polypropylene, cellulose, cellulose modifier, melamine resin, phenolic resin, polyester, silicone resin, polyimide, polyamideimide, polyaramid, polyphenylene sulfide, polysulfone, polyethersulfone, polyetheretherketone, polyaryletherketone, or a copolymer of butyl acrylate and ethyl methacrylate; Optionally, the organic-metal framework material includes at least one of a nitrogen-containing heterocyclic ligand building structure, an organic carboxylic acid ligand building structure, and a nitrogen-oxygen mixed ligand building structure. The insulating materials provided by the above technical solutions all have good insulating properties and can play a good role in electronic insulation and isolating ion capture agents and electrode active materials. Optionally, in some embodiments, the coating 13 further includes a filler. For example, when the ion capture agent added to the coating 13 is a non-particulate matter, a filler may be added to the coating 13 to provide pores in the coating for ions to pass through. Optionally, the filler comprises at least one of inorganic particles, organic particles, or organic-metal framework materials; Optionally, the inorganic particles include at least one of inorganic particles having a dielectric constant of 5 or more or inorganic particles having ion conductivity but not storing ions; Optionally, the organic particles include at least one of polycarbonate, polythiophene, polypyridine, polystyrene, polyacrylic wax, polyethylene, polypropylene, cellulose, cellulose modifier, melamine resin, phenolic resin, polyester, silicone resin, polyimide, polyamideimide, polyaramid, polyphenylene sulfide, polysulfone, polyethersulfone, polyetheretherketone, polyaryletherketone, or a copolymer of butyl acrylate and ethyl methacrylate; Optionally, the organic-metal framework material includes at least one of a nitrogen-containing heterocyclic ligand building structure, an organic carboxylic acid ligand building structure, and a nitrogen-oxygen mixed ligand building structure. Fillers are added to the coating layer 13 to provide pores in the coating layer 13 for ions to pass through, so as to improve the cycle performance of the secondary battery. Optionally, in some embodiments, the active material layer may further include a binder. For example, the binder in the positive electrode active material layer may include at least one of polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), vinylidene fluoride-tetrafluoroethylene-propylene terpolymer, vinylidene fluoride-hexafluoropropylene-tetrafluoroethylene terpolymer, tetrafluoroethylene-hexafluoropropylene copolymer and fluorine-containing acrylate resin. For another example, the binder in the negative electrode active material layer may include at least one of styrene-butadiene rubber (SBR), polyacrylic acid (PAA), sodium polyacrylate (PAAS), polyacrylamide (PAM), polyvinyl alcohol (PVA), sodium alginate (SA), polymethacrylic acid (PMAA) and carboxymethyl chitosan (CMCS). Optionally, in some embodiments, the active material layer may further include a conductive agent. As an example, the conductive agent may include at least one of superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene and carbon nanofibers. [Method for preparing electrode sheet] Figure 4 This is a method for preparing an isolation film according to an embodiment of the present application. Figure 4 As shown, the preparation method 500 includes the following steps. Step 510, providing a current collector; Step 520, providing active material slurry, and coating the active material slurry on at least one surface of the current collector to form an active material layer; Step 530, providing an insulating slurry, and coating the insulating slurry on the active material layer to form an insulating layer; Step 540, providing a coating slurry, and coating the coating slurry on the insulating layer to obtain an electrode plate. The coating layer includes an ion capture agent, and the reduction potential of the ion capture agent relative to lithium metal is 0 to 2V. The electrode plate prepared by the above method, when applied to a secondary battery, can improve the cycle performance of the secondary battery. [Electrolytes] The electrolyte plays the role of conducting ions between the positive electrode and the negative electrode. The present application has no specific restrictions on the type of electrolyte, which can be selected according to needs. For example, the electrolyte can be liquid, gel or all-solid. In some embodiments, the electrolyte is an electrolyte solution, which includes an electrolyte salt and a solvent. In some embodiments, the electrolyte salt can be selected from at least one of lithium hexafluorophosphate, lithium tetrafluoroborate, lithium perchlorate, lithium hexafluoroarsenate, lithium bis(fluorosulfonyl)imide, lithium bis(trifluoromethanesulfonyl)imide, lithium trifluoromethanesulfonate, lithium difluorophosphate, lithium difluorooxalatoborate, lithium dioxalatoborate, lithium difluorodioxalatophosphate, and lithium tetrafluorooxalatophosphate. In some embodiments, the solvent can be selected from at least one of ethylene carbonate, propylene carbonate, ethyl methyl carbonate, diethyl carbonate, dimethyl carbonate, dipropyl carbonate, methyl propyl carbonate, ethyl propyl carbonate, butylene carbonate, fluoroethylene carbonate, methyl formate, methyl acetate, ethyl acetate, propyl acetate, methyl propionate, ethyl propionate, propyl propionate, methyl butyrate, ethyl butyrate, 1,4-butyrolactone, cyclopentane sulfone, dimethyl sulfone, methyl ethyl sulfone and diethyl sulfone. In some embodiments, the electrolyte may further include additives, such as negative electrode film-forming additives, positive electrode film-forming additives, and additives that can improve certain battery properties, such as additives that improve battery overcharge performance, additives that improve battery high or low temperature performance, etc. In some embodiments, the positive electrode sheet, the negative electrode sheet, and the separator may be formed into an electrode assembly by a winding process or a lamination process. In some embodiments, the battery cell may include an outer packaging, which may be used to encapsulate the electrode assembly and the electrolyte. In some embodiments, the outer packaging of the battery cell may be a hard shell, such as a hard plastic shell, an aluminum shell, a steel shell, etc. The outer packaging of the battery cell may also be a soft package, such as a bag-type soft package. The material of the soft package may be plastic, and examples of the plastic include polypropylene, polybutylene terephthalate, and polybutylene succinate. The present application has no particular limitation on the shape of the battery cell, which may be cylindrical, square or any other shape. Figure 5 The secondary battery 20 is a square structure as an example. In some embodiments, reference Figure 6 , the outer packaging may include a shell 21 and a cover plate 23. Among them, the shell 21 may include a bottom plate and a side plate connected to the bottom plate, and the bottom plate and the side plate enclose a receiving cavity. The shell 21 has an opening connected to the receiving cavity, and the cover plate 23 can be covered on the opening to close the receiving cavity. The positive electrode sheet, the negative electrode sheet and the isolation membrane can form an electrode assembly 22 through a winding process or a lamination process. The electrode assembly 22 is encapsulated in the receiving cavity. The electrolyte is infiltrated in the electrode assembly 22. The number of electrode assemblies 22 contained in the secondary battery 20 can be one or more, and those skilled in the art can select according to specific actual needs. Figure 7 30 is an example of a battery module. Figure 7In the battery module 30, a plurality of secondary batteries 20 may be included. The plurality of secondary batteries 20 may be arranged in sequence along the length direction of the battery module 30. Of course, they may also be arranged in any other manner. Further, the plurality of secondary batteries 20 may be fixed by fasteners. The battery module 30 may further include a housing having an accommodation space in which the plurality of secondary batteries 20 are accommodated. In some embodiments, the battery modules described above may also be assembled into a battery pack, and the number of battery modules contained in the battery pack may be adjusted according to the application and capacity of the battery pack. Figure 8 40 is an example of a battery pack. Figure 8 The battery pack 40 may include a box body 41, the inside of the box body 41 is a hollow structure, and the plurality of battery modules 30 are accommodated in the box body 41. The plurality of battery modules 30 may be arranged in the box body 41 in any manner. In addition, the present application also provides an electric device, which includes at least one of the battery cells, battery modules or batteries provided in the present application. The battery cells, battery modules or batteries can be used as the power source of the electric device, and can also be used as the energy storage unit of the electric device. The electric device may include mobile devices (such as mobile phones, laptops, etc.), electric vehicles (such as pure electric vehicles, hybrid electric vehicles, plug-in hybrid electric vehicles, electric bicycles, electric scooters, electric golf carts, electric trucks, etc.), electric trains, ships and satellites, energy storage systems, etc., but are not limited thereto. As the electrical device, a battery cell, a battery module or a battery can be selected according to its usage requirements. Fig. 9 The power consumption device is taken as an example. The power consumption device is a pure electric vehicle, a hybrid electric vehicle, or a plug-in hybrid electric vehicle. In order to meet the high power and high energy density requirements of the power consumption device for battery cells, batteries or battery modules can be used. As another example, the device may be a mobile phone, a tablet computer, a notebook computer, etc. The device is usually required to be light and thin, and a battery cell may be used as a power source. [Example] Hereinafter, the embodiments of the present application will be described. The embodiments described below are exemplary and are only used to explain the present application, and should not be construed as limiting the present application. If no specific techniques or conditions are indicated in the embodiments, the techniques or conditions described in the literature in this area or the product specifications are used. If the manufacturer is not indicated in the reagents or instruments used, they are all conventional products that can be obtained commercially. 1. Preparation of positive electrode sheet Positive electrode 1: Providing active material slurry: dissolving active material lithium manganese oxide (LiMn2O4), conductive agent acetylene black, and binder polyvinylidene fluoride (PVDF) in a solvent N-methylpyrrolidone (NMP) at a mass ratio of 90%:5%:5%, stirring and mixing well, coating on Al foil, drying, and cold pressing to obtain a positive electrode sheet 1. Positive electrode 2: Providing insulating slurry: dissolving insulating material aluminum oxide (Al2O3) and binder PVDF in solvent NMP at a mass ratio of 90%:10%, stirring and mixing thoroughly, coating on the active material layer of the positive electrode plate 1 to form an insulating layer, and then drying to obtain a positive electrode plate 2, wherein the insulating layer thickness is 2μm. Positive electrode 3: Provide coating slurry: add ion capture agent Li7Ti5O 12 , the binder PVDF is dissolved in the solvent NMP at a mass ratio of 90%:10%, and after being fully stirred and mixed, it is coated on the insulating layer of the positive electrode plate 2 to form a coating to obtain the positive electrode plate 3, wherein the coating thickness is 2 μm. Positive electrode sheet 4: The preparation of positive electrode sheet 4 is similar to that of positive electrode sheet 3, except that the coating thickness in positive electrode sheet 4 is 0.01 μm. Positive electrode sheet 5: The preparation of positive electrode sheet 5 is similar to that of positive electrode sheet 3, except that the coating thickness in positive electrode sheet 5 is 0.1 μm. Positive electrode sheet 6: The preparation of positive electrode sheet 7 is similar to that of positive electrode sheet 3, except that the coating thickness in positive electrode sheet 6 is 10 μm. Positive electrode sheet 7: The preparation of positive electrode sheet 7 is similar to that of positive electrode sheet 3, except that the coating thickness in positive electrode sheet 7 is 20 μm. Positive electrode sheet 8: The preparation of positive electrode sheet 8 is similar to that of positive electrode sheet 3, except that the thickness of the insulating layer in positive electrode sheet 8 is 0.01 μm. Positive electrode sheet 9: The preparation of positive electrode sheet 9 is similar to that of positive electrode sheet 3, except that the thickness of the insulating layer in positive electrode sheet 9 is 0.1 μm. Positive electrode sheet 10: The preparation of the positive electrode sheet 10 is similar to that of the positive electrode sheet 3, except that the thickness of the insulating layer in the positive electrode sheet 10 is 10 μm. Positive electrode sheet 11: The preparation of the positive electrode sheet 11 is similar to that of the positive electrode sheet 3, except that the thickness of the insulating layer in the positive electrode sheet 11 is 20 μm. Positive electrode sheet 12: The preparation of positive electrode sheet 12 is similar to that of positive electrode sheet 3, except that the coating thickness in positive electrode sheet 12 is 30 μm. Positive electrode sheet 13: The preparation of the positive electrode sheet 13 is similar to that of the positive electrode sheet 3, except that the thickness of the insulating layer in the positive electrode sheet 13 is 30 μm. Positive electrode sheet 14: The preparation of the positive electrode sheet 14 is similar to that of the positive electrode sheet 3, except that the ion capture agent in the coating of the positive electrode sheet 14 is Li powder. Positive electrode sheet 15: The preparation of positive electrode sheet 15 is similar to that of positive electrode sheet 3, except that the ion capture agent in the coating of positive electrode sheet 15 is Li 1 / 6 C. Positive electrode plate 16: The preparation of positive electrode plate 16 is similar to that of positive electrode plate 3, except that the ion capture agent in the coating of positive electrode plate 16 is n-butyl lithium. Positive electrode sheet 17: The preparation of positive electrode sheet 17 is similar to that of positive electrode sheet 3, except that the ion capture agent in the coating of positive electrode sheet 17 is Positive electrode sheet 18: The preparation of positive electrode sheet 18 is similar to that of positive electrode sheet 3, except that the ion capture agent in the coating of positive electrode sheet 18 is

[0001] Positive electrode sheet 19: The preparation of positive electrode sheet 19 is similar to that of positive electrode sheet 3, except that the coating in positive electrode sheet 19 contains inorganic Al2O3 ceramic particles, wherein the ion capture agent Li7Ti5O 12 The mass ratio of inorganic Al2O3 ceramic particles and binder PVDF is 50%:40%:10%. 2. Preparation of negative electrode sheet Negative electrode sheet 1: The active material artificial graphite, the conductive agent acetylene black, and the binder PVDF are dissolved in the solvent NMP at a mass ratio of 90%:5%:5%, and after being fully stirred and mixed, they are coated on Cu foil, dried, and cold pressed to obtain the negative electrode sheet 1. Negative electrode sheet 2: The insulating material Al2O3 and the binder PVDF are dissolved in the solvent NMP in a mass ratio of 90%:10%, stirred and mixed thoroughly, and then coated on the negative electrode sheet 1 to obtain the negative electrode sheet 2, wherein the thickness of the insulating layer is 2 μm. Negative electrode 3: Ion capture agent Li7Ti5O 12 , the binder PVDF is dissolved in the solvent NMP at a mass ratio of 90%:10%, fully stirred and mixed, and then coated on the negative electrode sheet 2 to obtain the negative electrode sheet 3, wherein the coating thickness is 2 μm. 2. Preparation of secondary batteries [Example 1] (1) Positive electrode The positive electrode sheet adopts the positive electrode sheet 3 prepared as described above. (2) Negative electrode The negative electrode sheet adopts the negative electrode sheet 1 prepared as above. (3) Preparation of electrolyte Ethylene carbonate (EC) and ethyl methyl carbonate (EMC) were mixed at a mass ratio of 30:70, and 1 M lithium hexafluorophosphate (LiPF6) electrolyte salt was dissolved to obtain an electrolyte solution. (4) Preparation of isolation membrane A conventional polypropylene film was used as the isolation film. (5) Assembly of lithium-ion secondary battery: stack the positive electrode sheet 3, the separator, and the negative electrode sheet 1 in order, so that the separator is between the positive electrode sheet 3 and the negative electrode sheet 1 to play an isolating role, and then wind them to obtain an electrode assembly; place the electrode assembly in a battery casing, inject electrolyte after drying, and then obtain a lithium-ion battery 1 through processes such as formation and standing, as Example 1. [Example 2-17, Comparative Example 1-2] The preparation methods of the secondary batteries of Examples 2-17 and Comparative Examples 1-2 are similar to those of the secondary battery of Example 1, except that different positive electrode sheets are used (Example 1-17 uses positive electrode sheet 3-19, and Comparative Example 1-2 uses positive electrode sheet 1-2), as shown in Table 1 for details. [Example 18] The preparation method of the secondary battery of Example 18 is similar to that of the secondary battery of Example 1, except that different positive and negative electrode sheets are used (wherein Example 1 uses positive electrode sheet 3 and negative electrode sheet 1, and Example 18 uses positive electrode sheet 1 and negative electrode sheet 3), see Table 1 for details. [Example 19] The preparation method of the secondary battery of Example 19 is similar to that of the secondary battery of Example 1, except that different negative electrode sheets are used (wherein, Example 1 uses negative electrode sheet 1, and Example 19 uses negative electrode sheet 3), as shown in Table 1 for details. [Comparative Example 3] The preparation method of the secondary battery of comparative example 3 is similar to that of the secondary battery of embodiment 18, except that different negative electrode sheets are used (among which, embodiment 18 uses negative electrode sheet 3, and comparative example 3 uses negative electrode sheet 2), as shown in Table 1 for details. 3. Battery performance test (1) Battery capacity retention test At 45°C, the lithium-ion secondary battery is charged to 4.2V at 1C constant current, then charged to less than 0.05C at 4.2V constant voltage, and then discharged to 2.8V at 1C constant current. This is a charge and discharge process. Repeat the charge and discharge process and calculate the capacity retention rate of the lithium-ion secondary battery after 500 cycles. The capacity retention rate (%) of the lithium ion secondary battery after 500 cycles at 45° C.=(discharge capacity at the 500th cycle / discharge capacity at the first cycle)×100%. Please refer to Table 1 for product parameters of different embodiments and comparative examples, as well as test results of battery performance tests conducted on comparative examples 1-3 and embodiments 1-19 prepared according to the above method. Table 1: Product parameters and test results of comparative examples and different embodiments From the comparison of the results of comparative examples 1-3 and examples 1-19, it can be seen that the coating of the electrode plate includes an ion scavenger, and the corresponding cycle performance of the lithium manganese oxide battery is significantly improved. From the comparison of the results of Examples 1-5 and 10, it can be seen that when the coating thickness is set within an appropriate range, the corresponding cycle performance improvement effect of the lithium manganese oxide battery is better. In the embodiment of the present application, when other conditions are the same, the coating thickness is in the range of 0.01 μm to 20 μm, and the cycle performance of the lithium manganese oxide battery is better. From the comparison of the results of Examples 1, 6-9, and 11, it can be seen that when the thickness of the insulating layer is set within an appropriate range, the corresponding cycle performance improvement effect of the lithium manganese oxide battery is better. In the embodiments of the present application, when other conditions are the same, the thickness of the insulating layer is in the range of 0.01 μm to 20 μm, and the cycle performance of the lithium manganese oxide battery is better. From the comparison of the results of Comparative Examples 1-2 and Examples 1, 12-17, it can be seen that the ion capture agent Li7Ti5O provided in the examples of the present application 12 , Metal Li (powder), Li 1 / 6 C. n-Butyl lithium, When added to lithium manganese oxide batteries respectively, the cycle performance of lithium manganese oxide batteries is significantly improved. Although the present application has been described with reference to preferred embodiments, various modifications may be made thereto and parts thereof may be replaced with equivalents without departing from the scope of the present application. In particular, the various technical features mentioned in the various embodiments may be combined in any manner as long as there are no structural conflicts. The present application is not limited to the specific embodiments disclosed herein, but includes all technical solutions falling within the scope of the claims.

Claims

1. An electrode plate, comprising: current collector; an active material layer disposed on at least one surface of the current collector; an insulating layer, disposed on the active material layer; The coating layer is disposed on the insulating layer, and the coating layer includes an ion capture agent, wherein the reduction potential of the ion capture agent relative to lithium metal is 0 to 2V.

2. The electrode plate according to claim 1, wherein: The ion capture agent includes at least one of active metal and alkali metal compounds; Optionally, the active metal includes at least one of Li, Na, K, Rb, Cs, Fr, Mg, Ca, Sr, Ba, Al, Ti or V. Optionally, the active metal includes at least one of Li, Na, Mg, Al, Ti or V. Optionally, the alkali metal compound comprises A 1 x B. A 2 y Ti5O 12 , at least one of the compounds represented by formula (I), formula (II) or formula (III): RA 3 (I)、 Among them, A 1 , A 2 , A 3 , A 4 , A 5 , A 6 Each independently includes at least one of Li, Na, or K, B includes C, Si, or Sn, x≥0.05, y>4, R, R1, R2, R3, and R4 each independently include a hydrogen atom, an alkyl group having 1 to 20 carbon atoms, an alkyl group having 1 to 20 carbon atoms substituted by a sulfonic acid group or a sulfonyl group, an alkenyl group having 2 to 20 carbon atoms, an alkenyl group having 2 to 20 carbon atoms substituted by a sulfonic acid group or a sulfonyl group, an alkenyl group having 6 to 8 carbon atoms, The present invention further comprises at least one of an aryl group having 6 to 26 carbon atoms, an aryl group having 6 to 26 carbon atoms substituted by a sulfonic acid group or a sulfonyl group, a carboxyl group having 1 to 20 carbon atoms, a carboxyl group having 1 to 20 carbon atoms substituted by a sulfonic acid group or a sulfonyl group, a carbonyl group having 1 to 20 carbon atoms, a carbonyl group having 1 to 20 carbon atoms substituted by a sulfonic acid group or a sulfonyl group, an aryloxy group having 6 to 26 carbon atoms, and an aryloxy group having 6 to 26 carbon atoms substituted by a sulfonic acid group or a sulfonyl group.

3. The electrode plate according to claim 2, wherein: The A 1 x B includes Li 1 / 6 C. Na 1 / 6 C.K 1 / 8 C. Li 4.4 Si or Li 4.4 At least one of Sn.

4. The electrode plate according to claim 2 or 3, wherein: 5≤y≤7; Optionally, the A 2 y Ti5O 12 Including Li7Ti5O 12 or Na7Ti5O 12 At least one of .

5. The electrode sheet according to any one of claims 2 to 4, wherein: The compound represented by formula (I) includes at least one of n-butyllithium, naphthyllithium or biphenyllithium.

6. The electrode sheet according to any one of claims 2 to 5, wherein: The compounds represented by formula (II) include At least one of .

7. The electrode sheet according to any one of claims 2 to 6, wherein: The compounds represented by formula (III) include At least one of .

8. The electrode sheet according to any one of claims 1 to 7, wherein: The mass proportion of the ion capture agent in the coating is 50% to 99%. Optionally, the mass proportion of the ion capture agent in the coating is 80% to 98%.

9. The electrode sheet according to any one of claims 1 to 8, wherein: The thickness d1 of the coating is 0.01 μm to 20 μm, and optionally, d1 is 0.1 μm to 10 μm.

10. The electrode sheet according to any one of claims 1 to 9, wherein: The thickness d2 of the insulating layer is 0.01 μm to 20 μm, and optionally, d2 is 0.1 μm to 10 μm.

11. The electrode sheet according to any one of claims 1 to 10, wherein: The coating also includes a binder; Optionally, the binder includes at least one of polyacrylate, polyacrylic acid, polytetrafluoroethylene, polyvinylidene fluoride, vinylidene fluoride-trichloroethylene copolymer, polyvinyl pyrrolidone, polyvinyl acetate, ethylene-vinyl acetate copolymer, polyethylene oxide, polyarylate, carboxymethyl cellulose, hydroxypropyl cellulose, regenerated cellulose, cellulose acetate, cellulose acetate propionate, cellulose acetate butyrate, polyacrylonitrile, polyvinyl alcohol, polyethylene, polypropylene, starch, or cyanoethyl pullulan.

12. The electrode sheet according to any one of claims 1 to 11, wherein: The coating further comprises a filler; Optionally, the filler includes at least one of inorganic particles, organic particles, or organic-metal framework materials; Optionally, the inorganic particles include at least one of inorganic particles having a dielectric constant of 5 or more or inorganic particles having ion conductivity but not storing ions; Optionally, the organic particles include at least one of polycarbonate, polythiophene, polypyridine, polystyrene, polyacrylic wax, polyethylene, polypropylene, cellulose, cellulose modifier, melamine resin, phenolic resin, polyester, silicone resin, polyimide, polyamideimide, polyaramid, polyphenylene sulfide, polysulfone, polyethersulfone, polyetheretherketone, polyaryletherketone, or a copolymer of butyl acrylate and ethyl methacrylate; Optionally, the organic-metal framework material includes at least one of a nitrogen-containing heterocyclic ligand building structure, an organic carboxylic acid ligand building structure, and a nitrogen-oxygen mixed ligand building structure.

13. The electrode sheet according to any one of claims 1 to 12, wherein: The insulating layer comprises at least one of inorganic particles, organic particles or organic-metal framework materials; Optionally, the inorganic particles include at least one of inorganic particles having a dielectric constant of 5 or more or inorganic particles having ion conductivity but not storing ions; Optionally, the organic particles include at least one of polycarbonate, polythiophene, polypyridine, polystyrene, polyacrylic wax, polyethylene, polypropylene, cellulose, cellulose modifier, melamine resin, phenolic resin, polyester, silicone resin, polyimide, polyamideimide, polyaramid, polyphenylene sulfide, polysulfone, polyethersulfone, polyetheretherketone, polyaryletherketone, or a copolymer of butyl acrylate and ethyl methacrylate; Optionally, the organic-metal framework material includes at least one of a nitrogen-containing heterocyclic ligand building structure, an organic carboxylic acid ligand building structure, and a nitrogen-oxygen mixed ligand building structure.

14. A method for preparing an electrode sheet, comprising: providing a current collector; Providing an active material slurry, and coating the active material slurry on at least one surface of the current collector to form an active material layer; Providing an insulating slurry, and coating the insulating slurry on the active material layer to form an insulating layer; A coating slurry is provided, wherein the coating slurry includes an ion capture agent, and the reduction potential of the ion capture agent relative to lithium metal is 0-2V. The coating slurry is coated on the insulating layer to obtain an electrode plate.

15. A secondary battery comprising the electrode sheet according to any one of claims 1 to 13.

16. An electric device comprising the secondary battery according to claim 15.

Citation Information

Patent Citations

  • Non-aqueous electrolyte solution secondary battery

    CN104508869A

  • Coating material improving safety of lithium ion battery and preparation method and battery application thereof

    CN106848225A

  • Negative pole piece and preparation method thereof, secondary battery and preparation method thereof, battery module, battery pack and power utilization device

    CN115832640A

  • Non-aqueous electrolyte secondary cell containing scavenger

    WO2013108841A1