Negative pole piece, preparation method, secondary battery and electric device

By depositing a silicon interface layer on the metal negative electrode layer, the problem of dendrites is solved, the cycle stability and capacity of the battery are improved, and higher battery performance is achieved.

CN119069645AActive Publication Date: 2024-12-03CONTEMPORARY AMPEREX TECHNOLOGY CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202310645748.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-06-01
Publication Date
2024-12-03
Estimated Expiration
2043-06-01

AI Technical Summary

Technical Problem

The metal negative electrode is prone to form dendrites during the circulation process, resulting in safety accidents and degradation of battery performance, and it is difficult for the prior art to effectively inhibit its growth.

Method used

The silicon interface layer, including a material with the general formula SiOx, is deposited on the metal negative electrode layer, and the composition and thickness of the silomide layer are regulated by chemical vapor deposition method, inhibit the growth of dendrites, and improve the cycle stability and capacity of the battery.

Benefits of technology

The silicon interface layer effectively suppresses the formation of dendrites by increasing mechanical strength and negative electrode potential, improves the cycling stability and capacity level of the battery, while avoiding the risk of degradation in conductivity and brittle breakage.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119069645A_ABST
    Figure CN119069645A_ABST
Patent Text Reader

Abstract

The invention provides a negative pole piece which comprises a metal layer and a silicon interface layer located on at least one side of the metal layer, the silicon interface layer comprises a material with the general formula of SiOx, and x is larger than or equal to 0 and smaller than or equal to 2. Compared with a metal layer, the silicon interface layer has higher negative electrode potential, formation and growth of dendritic crystals can be inhibited, and improvement of the cycle performance of the battery is facilitated.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of secondary batteries, and in particular to a negative electrode sheet, a preparation method, a secondary battery and an electrical device. Background Art

[0002] In recent years, as secondary batteries have been widely used in energy storage power systems such as hydropower, thermal, wind and solar power stations, as well as in power tools, electric bicycles, electric motorcycles, electric vehicles, military equipment, aerospace and other fields, the market's performance requirements for secondary batteries have become increasingly higher.

[0003] Compared with the commonly used negative electrode material graphite, metal negative electrodes (such as lithium metal) have lower potential and higher theoretical capacity, and are very promising negative electrode materials. Summary of the invention

[0004] In view of the problems existing in the background technology, the present application provides a negative electrode plate, which aims to inhibit the formation of dendrites on the metal electrode and improve the cycle stability of the battery.

[0005] The first aspect of the present application provides a negative electrode plate, comprising a metal layer and a silicon interface layer located on at least one side of the metal layer, wherein the silicon interface layer comprises a general formula of SiO x of materials, where 0≤x≤2.

[0006] Compared with the metal layer, the silicon interface layer has a higher negative electrode potential, which can inhibit the formation and growth of dendrites and is beneficial to improving the battery cycle performance.

[0007] In any embodiment, the silicon interface layer comprises a silicon oxide having a general formula of SiO x Material, where 0<x<2, optionally 0.7<x<1.5.

[0008] Silicon oxide materials undergo lithiation during the charge and discharge cycle, forming a large amount of irreversible Li4SiO4, which has a Young's modulus of up to 8.81 GPa. It can inhibit the growth of lithium dendrites through its high mechanical strength and improve the cycle stability of the battery. In addition, silicon oxide materials also have a certain capacity, which can improve the capacity level of the battery while improving the cycle stability of the battery.

[0009] In any embodiment, the thickness of the silicon interface layer is 25 nm-1000 nm, and can be optionally 50 nm-200 nm.

[0010] When the thickness of the silicon interface layer is within an appropriate range, it can not only effectively protect the metal layer and inhibit the formation of dendrites, but also reduce the decrease in the conductivity of the negative electrode sheet, the increase in resistance, and the decrease in the unit gram capacity of the battery caused by the excessive thickness of the silicon interface layer. It can also reduce the risk of brittle fracture of the negative electrode sheet due to excessive thickness, thereby improving the overall performance of the battery.

[0011] In any embodiment, in the thickness direction of the silicon interface layer, the oxygen content of the silicon interface layer close to the metal layer is lower than the oxygen content of the silicon interface layer far from the metal layer. In the thickness direction of the silicon interface layer, the oxygen content of the silicon interface layer close to the metal layer is lower than the oxygen content of the silicon interface layer far from the metal layer, which is conducive to giving full play to the characteristics of different materials and achieving comprehensive improvement of battery cycle stability and capacity level.

[0012] In any embodiment, in the thickness direction of the silicon interface layer from close to the metal layer to far away from the metal layer, the silicon interface layer sequentially includes a silicon layer and a silicon oxide layer, the silicon layer includes elemental silicon, and the silicon oxide layer includes a general formula of SiO x material, where 0<x<2.

[0013] The irreversible Li4SiO4 formed by the silicon oxide layer 622 during the battery cycle can effectively solve the problem of large expansion rate of elemental silicon while inhibiting the growth of lithium dendrites, giving full play to the high capacity characteristics of elemental silicon, so that the battery has a higher capacity level while having high cycle performance.

[0014] In any embodiment, in the thickness direction of the silicon interface layer from close to the metal layer to far away from the metal layer, the silicon interface layer includes a silicon oxide layer and a silicon dioxide layer in sequence, and the silicon oxide layer includes a general formula of SiO x material, where 0<x<2.

[0015] Compared with silicon oxide materials, silicon dioxide layers can effectively inhibit the growth of lithium dendrites at low thickness. Providing a silicon dioxide layer on a silicon oxide layer can make full use of the surface pore structure of the silicon oxide layer. Compared with directly depositing a silicon dioxide layer on a metal layer, the surface pore structure of the silicon oxide layer can reduce the density of the silicon dioxide layer, while inhibiting the growth of dendrites, reducing the significant decrease in conductivity caused by excessive density of the silicon dioxide layer, and improving the battery cycle stability without causing a significant attenuation of the battery capacity level.

[0016] In any embodiment, in the thickness direction of the silicon interface layer from close to the metal layer to far away from the metal layer, the silicon interface layer sequentially includes a silicon layer, a silicon oxide layer and a silicon dioxide layer, the silicon layer includes amorphous silicon, and the silicon oxide layer includes a general formula of SiO x material, where 0<x<2.

[0017] The superposition of silicon layer, silicon oxide layer and silicon dioxide layer can not only give full play to the advantages of each layer, but also achieve comprehensive improvement in battery cycle stability and capacity level through the mutual cooperation of each layer.

[0018] In any embodiment, in the thickness direction of the silicon interface layer from close to the metal layer to far away from the metal layer, the silicon interface layer sequentially includes a SiOx1 layer, a SiOx2 layer, ..., SiOx n Layer, where 0<x1<x2<……<x n <2, n≥2.

[0019] The silicon content of the silicon interface layer is high near the metal layer, which can give full play to the high capacity characteristics of the material; the oxygen content is high far away from the metal layer, the negative electrode potential increases, and the content of Li4SiO4 generated increases, which is beneficial to inhibit the growth of dendrites.

[0020] In any embodiment, the negative electrode plate satisfies at least one of the following conditions:

[0021] (i) the ratio of the thickness of the silicon layer to the thickness of the silicon oxide layer is 4-15;

[0022] (ii) the thickness of the silicon layer is 10 nm to 100 nm;

[0023] (iii) the thickness of the silicon oxide layer is 25nm-150nm;

[0024] (iv) The thickness of the silicon dioxide layer is 1 nm-10 nm.

[0025] In any embodiment, the metal layer includes at least one of lithium metal, lithium alloy, sodium metal, and sodium alloy.

[0026] In any embodiment, the silicon interface layer is prepared by at least one of chemical vapor deposition, atomic layer deposition, evaporation, and magnetron sputtering.

[0027] The present application provides a method for preparing a negative electrode sheet, the method comprising: depositing a silicon interface layer on at least one side of a metal layer to prepare the negative electrode sheet, the silicon interface layer comprising a general formula of SiO x of materials, where 0≤x≤2.

[0028] In any embodiment, the preparation method includes: introducing a gas containing a silicon source or a mixed gas containing an oxygen source and a silicon source, and preparing a silicon interface layer by chemical vapor deposition; optionally, the oxygen source includes N2O, and the silicon source includes SiH4.

[0029] The silicon interface layer is prepared by chemical vapor deposition. The composition of the silicon interface layer can be regulated by adjusting the flow rate of the oxygen source and silicon source at any time, making the battery molding more efficient. Compared with other preparation methods, the flow rate of the input raw materials is controllable, making it easy to achieve precise control of the composition and thickness of the silicon interface layer.

[0030] In any embodiment, the preparation method comprises: the volume flow ratio M of the introduced oxygen source to the silicon source is 0<M<20, and the silicon interface layer comprises a material of the general formula SiOx, wherein 0<x<2.

[0031] In any embodiment, during the preparation of the silicon interface layer, the introduction ratio M of the oxygen source to the silicon source is increased so that in the thickness direction of the silicon interface layer, the oxygen content of the silicon interface layer close to the metal layer is lower than the oxygen content far from the metal layer.

[0032] In any embodiment, the preparation method comprises: introducing a silicon source for deposition; and introducing an oxygen source and a silicon source for further deposition after deposition for a period of time, wherein the volume flow ratio M of the oxygen source and the silicon source is 0<M<20.

[0033] In any embodiment, the preparation method includes: introducing an oxygen source and a silicon source for deposition, wherein the volume flow ratio M of the oxygen source and the silicon source is 0<M<20; after deposition for a period of time, increasing the volume flow ratio M of the oxygen source and the silicon source to not less than 20 for deposition.

[0034] In any embodiment, the preparation method includes: introducing a silicon source for deposition; after a period of deposition, introducing an oxygen source and a silicon source for deposition, wherein the volume flow ratio M of the oxygen source and the silicon source is 0<M<20; after a period of deposition, increasing the ratio M of the oxygen source and the silicon source to not less than 20 for deposition.

[0035] In any embodiment, the preparation method comprises: during the process of introducing the oxygen source and the silicon source for deposition, gradually increasing the volume flow ratio M of the oxygen source and the silicon source.

[0036] A third aspect of the present application provides a secondary battery, comprising the negative electrode sheet of the first aspect or the negative electrode sheet prepared by the preparation method of the second aspect.

[0037] In any embodiment, the secondary battery includes an electrolyte, and the silicon interface layer is located between the electrolyte and the metal layer.

[0038] A fourth aspect of the present application provides an electrical device, comprising the secondary battery of the third aspect. BRIEF DESCRIPTION OF THE DRAWINGS

[0039] Figure 1 is a schematic diagram of a negative electrode sheet according to an embodiment of the present application;

[0040] Figure 2 is a schematic diagram of a negative electrode sheet according to an embodiment of the present application;

[0041] Figure 3 is a schematic diagram of a negative electrode sheet according to an embodiment of the present application;

[0042] Figure 4 is a schematic diagram of a negative electrode sheet according to an embodiment of the present application;

[0043] Figure 5 is a schematic diagram of a negative electrode sheet according to an embodiment of the present application;

[0044] Figure 6 is a schematic diagram of a secondary battery according to an embodiment of the present application;

[0045] Figure 7 yes Figure 6 An exploded view of a secondary battery according to an embodiment of the present application is shown;

[0046] Figure 8 It is a schematic diagram of an electrical device according to one embodiment of the present application.

[0047] Reference numerals:

[0048] 1 battery pack; 2 upper box; 3 lower box; 4 battery module; 5 sodium ion battery; 51 shell; 52 electrode assembly; 53 cover plate; 6, 6-1, 6-2, 6-3, 6-4 negative electrode plate; 61 metal layer; 62, 62-1, 62-2, 62-3, 62-4 silicon interface layer; 621 silicon layer; 622 silicon oxide layer; 6221SiO x1 Layer; 6222SiO x2 Layer: 623 silicon dioxide layer. DETAILED DESCRIPTION

[0049] Below, the embodiments of the negative electrode sheet, preparation method, secondary battery and electrical device of the present application are specifically disclosed with appropriate reference to the drawings. However, there may be cases where unnecessary detailed descriptions are omitted. For example, there are cases where detailed descriptions of well-known matters and repeated descriptions of actually the same structure are omitted. This is to avoid the following description from becoming unnecessarily lengthy and to facilitate the understanding of those skilled in the art. In addition, the drawings and the following descriptions are provided for those skilled in the art to fully understand the present application and are not intended to limit the subject matter described in the claims.

[0050] "Scope" disclosed in the present application is limited in the form of lower limit and upper limit, and a given range is limited by selecting a lower limit and an upper limit, and the selected lower limit and upper limit define the boundary of a special range. The scope limited in this way can be including end values ​​or not including end values, and can be arbitrarily combined, that is, any lower limit can be combined with any upper limit to form a scope. For example, if the scope of 60-120 and 80-110 is listed for a specific parameter, it is understood that the scope of 60-110 and 80-120 is also expected. In addition, if the minimum range values ​​1 and 2 are listed, and if the maximum range values ​​3, 4 and 5 are listed, the following scope can be all expected: 1-3, 1-4, 1-5, 2-3, 2-4 and 2-5. In the present application, unless otherwise specified, the numerical range "ab" represents the abbreviation of any real number combination between a and b, wherein a and b are real numbers. For example, the numerical range "0-5" means that all real numbers between "0-5" are listed in this document, and "0-5" is just an abbreviation of these numerical combinations. In addition, when a parameter is expressed as an integer ≥ 2, it is equivalent to disclosing that the parameter is, for example, an integer of 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, etc.

[0051] If not otherwise specified, all embodiments and optional embodiments of the present application can be combined with each other to form a new technical solution.

[0052] Unless otherwise specified, all technical features and optional technical features of this application can be combined with each other to form a new technical solution.

[0053] If there is no special explanation, all steps of the present application can be performed sequentially or randomly, preferably sequentially. For example, the method includes steps (a) and (b), which means that the method may include steps (a) and (b) performed sequentially, or may include steps (b) and (a) performed sequentially. For example, the method may further include step (c), which means that step (c) may be added to the method in any order. For example, the method may include steps (a), (b) and (c), or may include steps (a), (c) and (b), or may include steps (c), (a) and (b), etc.

[0054] If there is no special explanation, the "include" and "comprising" mentioned in this application are open-ended or closed-ended. For example, the "include" and "comprising" may mean that other components not listed may also be included or only the listed components may be included or only the listed components may be included.

[0055] If not specifically stated, in this application, the term "or" is inclusive. For example, the phrase "A or B" means "A, B, or both A and B". More specifically, any of the following conditions satisfies the condition "A or B": A is true (or exists) and B is false (or does not exist); A is false (or does not exist) and B is true (or exists); or both A and B are true (or exist).

[0056] Metal anodes are very promising anode materials. For example, lithium metal has the lowest voltage and a theoretical capacity of 3860 mAh / g, which is 10 times that of graphite anode materials. However, during the cycle, metal anodes are prone to form a large number of dendrites on the surface of the electrode, causing puncture of the diaphragm, resulting in direct contact between the positive and negative electrodes and short circuits, causing serious safety accidents.

[0057] [Negative electrode]

[0058] Based on this, Figure 1 As shown, the present application provides a negative electrode plate 6, comprising a metal layer 61 and a silicon interface layer 62 located on at least one side of the metal layer 61, wherein the silicon interface layer 62 comprises a general formula of SiO x of materials, where 0≤x≤2.

[0059] The structure of the negative electrode sheet can be characterized by any known method in the art. As an example, the ion polished cross-sectional morphology of the negative electrode sheet can be observed by a scanning electron microscope, and the material composition on the cross-sectional surface of the negative electrode sheet can be tested by an energy dispersive spectrometer.

[0060] In some embodiments, the metal layer 61 includes at least one of lithium metal, lithium alloy, sodium metal, and sodium alloy.

[0061] Lithium alloy refers to an alloy including lithium and at least one other metal. In some embodiments, the content of lithium in the lithium alloy can be 90 wt% or more, 95 wt% or more, 99 wt% or more. For example, the content of lithium in the lithium alloy can be 97wt%, 97.5wt%, 98wt%, 98.5wt%, 99.1wt%, 99.3wt%, 99.5wt%, 99.7wt% or 99.9wt%, etc. The lithium alloy can optionally include one or more of lithium copper alloy, lithium indium alloy, lithium zinc alloy, lithium magnesium alloy, lithium tin alloy and lithium silver alloy.

[0062] Sodium alloy refers to an alloy including sodium and at least one other metal. As a non-limiting example, the sodium alloy can be sodium and cesium, sodium and rubidium, or a mixture thereof.

[0063] In some embodiments, the silicon interface layer 62 includes silicon, silicon dioxide, a general formula of SiO xAt least one of the silicon-oxygen materials with a thickness of (0<x<2). It can be understood that the above-mentioned multiple materials can be located in the same layer, or can be arranged in layers to form a silicon interface layer together.

[0064] In some embodiments, the silicon interface layer 62 includes silicon. In some embodiments, the silicon is amorphous silicon. Silicon has a higher electrode potential than lithium, and the probability of lithium dendrite formation can be reduced by increasing the potential. Moreover, silicon has a larger negative electrode capacity than lithium, which can further increase the battery capacity.

[0065] In some embodiments, the silicon interface layer 62 includes a general formula of SiO x In some embodiments, the silicon interface layer includes a silicon-oxygen material of the general formula SiO x For silicon oxide material, x can be selected as 0.1, 0.2, 0.3, 0.4, 0.5, 0.6, 0.7, 0.8, 0.9, 1, 1.1, 1.2, 1.3, 1.4, 1.5, 1.6, 1.7, 1.8, 1.9 or any value therebetween.

[0066] Silicon oxide materials undergo lithiation during the charge and discharge cycle, forming a large amount of irreversible Li4SiO4, which has a Young's modulus of up to 8.81 GPa. It can inhibit the growth of lithium dendrites through its high mechanical strength and improve the cycle stability of the battery. In addition, silicon oxide materials also have a certain capacity, which can improve the capacity level of the battery while improving the cycle stability of the battery.

[0067] In some embodiments, the silicon interface layer 62 includes a general formula of SiO x Silicon oxide material, wherein 0.7<x<1.5.

[0068] When the ratio of oxygen to silicon in the silicon-oxygen material is between 0.7 and 1.5, the silicon-oxygen material has both high specific capacity and low expansion rate, which is conducive to further improving the battery cycle stability and capacity level.

[0069] In some embodiments, silicon interface layer 62 includes silicon dioxide.

[0070] Silicon dioxide is a high-strength insulating material that provides almost no capacity. The Li4SiO4 generated during the battery cycle is denser and has higher mechanical strength. Compared with silicon oxide materials, it can more effectively inhibit dendrite growth, stabilize the negative electrode structure, and improve the overall mechanical strength at a low addition amount.

[0071] In summary, the silicon interface layer has a higher negative electrode potential than metallic lithium, which can inhibit the formation and growth of dendrites and is beneficial to improving the battery cycle performance.

[0072] In some embodiments, the thickness of the silicon interface layer 62 is 25 nm-1000 nm, and may be 50 nm-200 nm.

[0073] In some embodiments, the thickness of the silicon interface layer 62 may be 25 nm, 50 nm, 75 nm, 100 nm, 125 nm, 150 nm, 175 nm, 200 nm, or any value therein.

[0074] The thickness of the silicon interface layer 62 is within an appropriate range, which can not only effectively protect the metal layer 61 and inhibit the formation of dendrites, but also reduce the decrease in the conductivity of the negative electrode plate 6 caused by the excessive thickness of the silicon interface layer 62, the increase in resistance, and the decrease in the unit gram capacity of the battery. It can also reduce the risk of brittle fracture of the negative electrode plate 6 due to excessive thickness, thereby improving the overall performance of the battery.

[0075] In some embodiments, in the thickness direction of the silicon interface layer, the oxygen content of the silicon interface layer close to the metal layer is lower than the oxygen content of the silicon interface layer far from the metal layer.

[0076] The oxygen content at different positions of the silicon interface layer can be measured by combining a scanning electron microscope with an energy spectrometer. As an example, a cross-sectional view in the thickness direction of the electrode piece is obtained by a scanning electron microscope, and the relative distribution of oxygen at different positions of the negative electrode piece is measured by a line scan, surface scan or point scan module of the energy spectrometer, thereby determining the oxygen content at different positions of the negative electrode piece.

[0077] In the thickness direction of the silicon interface layer, the oxygen content of the silicon interface layer close to the metal layer is lower than the oxygen content far from the metal layer, which is beneficial to bring out the characteristics of different materials and achieve a comprehensive improvement in battery cycle stability and capacity level.

[0078] In some embodiments, Figure 2 As shown, in the negative electrode sheet 6-1, in the thickness direction of the silicon interface layer from close to the metal layer 61 to far away from the metal layer 61, the silicon interface layer 62-1 includes a silicon layer 621 and a silicon oxide layer 622 in sequence, the silicon layer 621 includes single substance silicon, and the silicon oxide layer 622 includes a general formula of SiO x material, where 0<x<2.

[0079] In some embodiments, the elemental silicon includes crystalline silicon and amorphous silicon.

[0080] Crystalline silicon includes single crystal silicon and polycrystalline silicon. The atomic arrangement structure of crystalline silicon is similar to the diamond structure, forming a long-range ordered structure. The constituent atoms of amorphous silicon are short-range ordered and long-range disordered, and the bonding between atoms is very similar to crystalline silicon, forming a covalent irregular network structure.

[0081] The irreversible Li4SiO4 formed by the silicon oxide layer 622 during the battery cycle can effectively solve the problem of large expansion rate of elemental silicon while inhibiting the growth of lithium dendrites, giving full play to the high capacity characteristics of elemental silicon, so that the battery has a higher capacity level while having high cycle performance.

[0082] In some embodiments, Figure 3 As shown, in the negative electrode sheet 6-2, in the thickness direction of the silicon interface layer from close to the metal layer 61 to far away from the metal layer 61, the silicon interface layer 62-2 includes a silicon oxide layer 622 and a silicon dioxide layer 623 in sequence, and the silicon oxide layer 622 includes a general formula of SiO x material, where 0<x<2.

[0083] In some embodiments, silicon dioxide layer 623 includes silicon dioxide.

[0084] Compared with silicon oxide materials, the silicon dioxide layer 623 can effectively inhibit the growth of lithium dendrites at a low thickness. The silicon dioxide layer 623 is arranged on the silicon oxide layer 622, and the surface pore structure of the silicon oxide layer 622 can be fully utilized. Compared with directly depositing the silicon dioxide layer 623 on the metal layer 61, the surface pore structure of the silicon oxide layer 622 can reduce the density of the silicon dioxide layer 623, while inhibiting the growth of dendrites, reducing the significant decrease in conductivity caused by the excessive density of the silicon dioxide layer 623, and improving the battery cycle stability without causing a significant attenuation of the battery capacity level.

[0085] In some embodiments, Figure 4 As shown, in the negative electrode sheet 6-3, in the thickness direction of the silicon interface layer from close to the metal layer 61 to far away from the metal layer 61, the silicon interface layer 62-3 includes a silicon layer 621, a silicon oxide layer 622 and a silicon dioxide layer 623 in sequence, the silicon layer 621 includes elemental silicon, the silicon oxide layer 622 includes a general formula of SiO x material, where 0<x<2.

[0086] The stacking arrangement of the silicon layer 621, the silicon oxide layer 622 and the silicon dioxide layer 623 can not only give full play to the advantages of each layer, but also achieve comprehensive improvement in battery cycle stability and capacity level through the mutual cooperation of each layer.

[0087] In some embodiments, in the thickness direction of the silicon interface layer from close to the metal layer 61 to far away from the metal layer 61, the silicon interface layer 62 includes SiOx1 layer, SiOx2 layer, SiOx n Layer, where 0<x1<x2<……<x n<2, n≥2. It can be understood that the oxygen content in the silicon-oxygen material can change continuously or increase in stages. The silicon content of the silicon interface layer 62 is high near the metal layer 61, which can give full play to the high capacity characteristics of the material; the oxygen content is high at a position far from the metal layer 61, the negative electrode potential increases, and the content of Li4SiO4 generated increases, which is conducive to inhibiting the growth of dendrites.

[0088] In some embodiments, Figure 5 As shown, in the negative electrode plate 6-4, in the thickness direction of the silicon interface layer from close to the metal layer 61 to far away from the metal layer 61, the silicon interface layer 62-4 sequentially includes a silicon layer 621, a SiOx1 layer 6221, a SiOx2 layer 6222 and a silicon dioxide layer 623, and the silicon layer 621 includes elemental silicon, 0<x1<x2<2.

[0089] In some embodiments, the ratio of the thickness of the silicon layer to the thickness of the silicon oxide layer is 4-15.

[0090] In some embodiments, the ratio of the thickness of the silicon layer to the thickness of the silicon oxide layer may be 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15 or any value therebetween.

[0091] Controlling the ratio of the thickness of the silicon layer to the thickness of the silicon oxide layer within the above range can increase the battery capacity while suppressing the growth of lithium dendrites and the expansion of the silicon material through the high modulus of the silicon oxide layer, thereby improving the cycle stability and electrochemical performance of the battery.

[0092] In some embodiments, the silicon layer has a thickness of 10 nm to 100 nm.

[0093] In some embodiments, the thickness of the silicon layer can be selected to be 10 nm, 20 nm, 30 nm, 40 nm, 50 nm, 60 nm, 70 nm, 80 nm, 90 nm, 100 nm, or any value therebetween.

[0094] By controlling the thickness of the silicon layer within this range, the high capacity characteristics of single-element silicon can be fully utilized and the negative impact of the expansion of single-element silicon on the battery cycle performance can be reduced.

[0095] In some embodiments, the thickness of the silicon oxide layer is 25 nm to 150 nm.

[0096] In some embodiments, the thickness of the silicon oxide layer may be 25 nm, 30 nm, 40 nm, 50 nm, 60 nm, 70 nm, 80 nm, 90 nm, 100 nm, 110 nm, 120 nm, 130 nm, 140 nm, 150 nm, 160 nm, 170 nm, 180 nm, 190 nm, 200 nm, or any value therebetween.

[0097] Controlling the thickness of the silicon oxide layer within this range can effectively suppress dendrites without sacrificing capacity or causing excessive negative impact on the conduction of lithium ions in the negative electrode.

[0098] In some embodiments, the silicon dioxide layer has a thickness of 1 nm to 10 nm.

[0099] In some embodiments, the thickness of the silicon dioxide layer is 1 nm, 2 nm, 3 nm, 4 nm, 5 nm, 6 nm, 7 nm, 8 nm, 9 nm, 10 nm, or any value therebetween.

[0100] Controlling the thickness of the silicon dioxide layer within this range can effectively suppress dendrites without bringing excessive negative impact on the battery capacity and the conduction of lithium ions in the negative electrode.

[0101] In some embodiments, the silicon interface layer is prepared by at least one of chemical vapor deposition, atomic layer deposition, evaporation, and magnetron sputtering.

[0102] Chemical vapor deposition is a chemical vapor reaction growth method. Under different temperature fields and different vacuum degrees, the compound or single substance reaction source gas containing the elements constituting the thin film material is concentrated and introduced into the reaction chamber containing the metal layer, and decomposition, desorption, combination and other reactions are carried out at the interface between the metal layer and the gas phase to generate new solid substances that are deposited on the surface of the metal layer to form a uniform film. By controlling the reaction temperature, reaction source gas composition, concentration, pressure and other parameters, the organizational structure and composition of the film can be easily controlled, its mechanical properties and chemical properties can be changed, and the requirements for the performance of the electrode under different conditions can be met. Chemical vapor deposition methods include but are not limited to electron cyclotron resonance microwave, plasma chemical vapor deposition, hot wire plasma chemical vapor deposition and radio frequency plasma chemical vapor deposition.

[0103] Atomic layer deposition is a method that can deposit materials layer by layer on the surface of a substrate in the form of a single atomic film.

[0104] Evaporation refers to a method of heating the raw material to be formed into a thin film in an evaporation container so that its atoms or molecules vaporize and escape from the surface to form a vapor flow, which is incident on the surface of the material to be deposited and condenses to form a solid thin film.

[0105] Magnetron sputtering is a DC diode sputtering method performed under the control of a magnetic field and is a physical coating method.

[0106] The second aspect of the present application provides a method for preparing a negative electrode sheet, the method comprising: depositing a silicon interface layer on at least one side of a metal layer to prepare a negative electrode sheet, the silicon interface layer comprising a general formula of SiO x of materials, where 0≤x≤2.

[0107] In some embodiments, the preparation method includes: introducing a gas containing a silicon source or a mixed gas containing an oxygen source and a silicon source, and preparing a silicon interface layer by chemical vapor deposition; optionally, the oxygen source includes N2O, and the silicon source includes SiH4.

[0108] In some embodiments, during the preparation of the silicon interface layer, only the silicon source is introduced, and the volume flow ratio M of the oxygen source to the silicon source is 0, so as to prepare the silicon layer.

[0109] In some embodiments, the volume flow ratio M of the oxygen source to the silicon source is 0<M<20 to prepare a silicon oxide layer, wherein the silicon oxide layer comprises a general formula of SiO x material, where 0<x<2.

[0110] In some embodiments, the volume flow ratio M of the introduced oxygen source to the silicon source is greater than 20 to prepare the silicon dioxide layer.

[0111] The silicon interface layer is prepared by chemical vapor deposition. The composition of the silicon interface layer can be regulated by adjusting the flow rate of the oxygen source and silicon source at any time, making the battery molding more efficient. Compared with other preparation methods, the flow rate of the input raw materials is controllable, making it easy to achieve precise control of the composition and thickness of the silicon interface layer.

[0112] In some embodiments, the preparation method includes: the volume flow ratio M of the introduced oxygen source to the silicon source is 0<M<20, and the silicon interface layer includes a material with a general formula of SiOx, wherein 0<x<2.

[0113] In some embodiments, during the preparation of the silicon interface layer, the introduction ratio M of the oxygen source to the silicon source is increased so that in the thickness direction of the silicon interface layer, the oxygen content of the silicon interface layer close to the metal layer is lower than the oxygen content far from the metal layer.

[0114] It can be understood that the oxygen source to silicon source introduction ratio M can be continuously increased to deposit a silicon interface layer with continuously changing components; the oxygen source to silicon source introduction ratio M can also be increased in stages so that a certain fixed component material has a certain thickness.

[0115] In some embodiments, the preparation method includes: introducing a silicon source for deposition; and introducing an oxygen source and a silicon source for deposition after a period of deposition, wherein the volume flow ratio M of the oxygen source and the silicon source is 0<M<20.

[0116] In some embodiments, the preparation method includes: introducing an oxygen source and a silicon source for deposition, wherein the volume flow ratio M of the oxygen source and the silicon source is 0<M<20; after deposition for a period of time, increasing the volume flow ratio M of the oxygen source and the silicon source to not less than 20 for deposition.

[0117] In some embodiments, the preparation method includes: introducing a silicon source for deposition; after a period of deposition, introducing an oxygen source and a silicon source for deposition, wherein the volume flow ratio M of the oxygen source and the silicon source is 0<M<20; after a period of deposition, increasing the ratio M of the oxygen source and the silicon source to greater than 20 for deposition.

[0118] In some embodiments, during the process of introducing the oxygen source and the silicon source for deposition, the volume flow ratio M of the oxygen source and the silicon source is gradually increased to prepare multilayer SiO x layer.

[0119] The chemical vapor deposition method can achieve efficient preparation of silicon interface layers with different buffer potentials in a one-step process, reduce the probability of dendrite formation by increasing the negative electrode potential, and adjust the mechanical strength of the silicon interface layer by regulating its composition to further inhibit the growth of dendrites. It can also simultaneously deposit high-specific capacity negative electrode materials, thereby improving the battery cycle performance while taking into account the electrochemical performance of the battery.

[0120] [Positive electrode]

[0121] The positive electrode sheet includes a positive electrode current collector and a positive electrode film layer arranged on at least one surface of the positive electrode current collector, wherein the positive electrode film layer includes the positive electrode active material of the first aspect of the present application.

[0122] As an example, the positive electrode current collector has two surfaces opposite to each other in its thickness direction, and the positive electrode film layer is disposed on any one or both of the two opposite surfaces of the positive electrode current collector.

[0123] In some embodiments, the positive electrode current collector may be a metal foil or a composite current collector. For example, aluminum foil may be used as the metal foil. The composite current collector may include a polymer material base and a metal layer formed on at least one surface of the polymer material base. The composite current collector may be formed by forming a metal material (aluminum, aluminum alloy, nickel, nickel alloy, titanium, titanium alloy, silver and silver alloy, etc.) on a polymer material substrate (such as a substrate of polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), polyethylene (PE), etc.).

[0124] In some embodiments, the positive electrode active material may adopt a positive electrode active material for a battery that is well known in the art. As an example, the positive electrode active material may include at least one of the following materials: a lithium-containing phosphate with an olivine structure, a lithium transition metal oxide, and their respective modified compounds. However, the present application is not limited to these materials, and other traditional materials that can be used as positive electrode active materials for batteries may also be used. These positive electrode active materials may be used alone or in combination of two or more. Among them, examples of lithium transition metal oxides may include, but are not limited to, lithium cobalt oxide (such as LiCoO2), lithium nickel oxide (such as LiNiO2), lithium manganese oxide (such as LiMnO2, LiMn2O4), lithium nickel cobalt oxide, lithium manganese cobalt oxide, lithium nickel manganese oxide, lithium nickel cobalt manganese oxide (such as LiNi 1 / 3 Co 1 / 3 Mn 1 / 3 O2 (also referred to as NCM 333 )、LiNi 0.5 Co 0.2 Mn 0.3 O2 (also referred to as NCM 523 )、LiNi 0.5 Co 0.25 Mn 0.25 O2 (also referred to as NCM 211 )、LiNi 0.6 Co 0.2 Mn 0.2 O2 (also referred to as NCM 622 )、LiNi 0.8 Co 0.1 Mn 0.1 O2 (also referred to as NCM 811 ), lithium nickel cobalt aluminum oxide (such as LiNi 0.85 Co 0.15 Al 0.05 O2) and its modified compounds, etc. Examples of lithium-containing phosphates with an olivine structure may include, but are not limited to, at least one of lithium iron phosphate (such as LiFePO4 (also referred to as LFP)), a composite material of lithium iron phosphate and carbon, lithium manganese phosphate (such as LiMnPO4), a composite material of lithium manganese phosphate and carbon, lithium iron manganese phosphate, and a composite material of lithium iron manganese phosphate and carbon.

[0125] In some embodiments, the positive electrode film layer may further optionally include a binder. As an example, the binder may include at least one of polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), vinylidene fluoride-tetrafluoroethylene-propylene terpolymer, vinylidene fluoride-hexafluoropropylene-tetrafluoroethylene terpolymer, tetrafluoroethylene-hexafluoropropylene copolymer, and fluorine-containing acrylate resin.

[0126] In some embodiments, the positive electrode film layer may further include a conductive agent, which may include, for example, at least one of superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers.

[0127] In some embodiments, the positive electrode sheet can be prepared in the following manner: the components for preparing the positive electrode sheet, such as the positive electrode active material, the conductive agent, the binder and any other components are dispersed in a solvent (such as N-methylpyrrolidone) to form a positive electrode slurry; the positive electrode slurry is coated on the positive electrode collector, and after drying, cold pressing and other processes, the positive electrode sheet can be obtained.

[0128] [Electrolytes]

[0129] The electrolyte plays the role of conducting ions between the positive electrode and the negative electrode. The present application has no specific restrictions on the type of electrolyte, which can be selected according to needs. For example, the electrolyte can be liquid, gel or all-solid.

[0130] In some embodiments, the electrolyte is an electrolyte solution, which includes an electrolyte salt and a solvent.

[0131] In some embodiments, the electrolyte salt can be selected from at least one of lithium hexafluorophosphate, lithium tetrafluoroborate, lithium perchlorate, lithium hexafluoroarsenate, lithium bis(fluorosulfonyl)imide, lithium bis(trifluoromethanesulfonyl)imide, lithium trifluoromethanesulfonate, lithium difluorophosphate, lithium difluorooxalatoborate, lithium dioxalatoborate, lithium difluorodioxalatophosphate, and lithium tetrafluorooxalatophosphate.

[0132] In some embodiments, the solvent can be selected from at least one of ethylene carbonate, propylene carbonate, ethyl methyl carbonate, diethyl carbonate, dimethyl carbonate, dipropyl carbonate, methyl propyl carbonate, ethyl propyl carbonate, butylene carbonate, fluoroethylene carbonate, methyl formate, methyl acetate, ethyl acetate, propyl acetate, methyl propionate, ethyl propionate, propyl propionate, methyl butyrate, ethyl butyrate, 1,4-butyrolactone, cyclopentane sulfone, dimethyl sulfone, methyl ethyl sulfone and diethyl sulfone.

[0133] In some embodiments, the electrolyte may further include additives, such as negative electrode film-forming additives, positive electrode film-forming additives, and additives that can improve certain battery properties, such as additives that improve battery overcharge performance, additives that improve battery high or low temperature performance, etc.

[0134] [Isolation film]

[0135] In some embodiments, the secondary battery further includes a separator. The present application has no particular limitation on the type of separator, and any known porous separator with good chemical stability and mechanical stability can be selected.

[0136] In some embodiments, the material of the isolation membrane can be selected from at least one of glass fiber, non-woven fabric, polyethylene, polypropylene and polyvinylidene fluoride. The isolation membrane can be a single-layer film or a multi-layer composite film, without particular limitation. When the isolation membrane is a multi-layer composite film, the materials of each layer can be the same or different, without particular limitation.

[0137] In some embodiments, the positive electrode sheet, the negative electrode sheet, and the separator may be formed into an electrode assembly by a winding process or a lamination process.

[0138] A second aspect of the present application provides a secondary battery, comprising a negative electrode sheet according to any embodiment, and / or a negative electrode sheet prepared by a preparation method according to any embodiment.

[0139] In some embodiments, the secondary battery includes an electrolyte, and the silicon interface layer is located between the electrolyte and the metal layer.

[0140] In some embodiments, the secondary battery may include an outer package, which may be used to encapsulate the electrode assembly and the electrolyte.

[0141] In some embodiments, the outer packaging of the secondary battery may be a hard shell, such as a hard plastic shell, an aluminum shell, a steel shell, etc. The outer packaging of the secondary battery may also be a soft package, such as a bag-type soft package. The material of the soft package may be plastic, and examples of the plastic include polypropylene, polybutylene terephthalate, and polybutylene succinate.

[0142] The present application has no particular limitation on the shape of the secondary battery, which may be cylindrical, square or any other shape. Figure 6 The secondary battery 5 is a square structure as an example.

[0143] In some embodiments, reference Figure 7 , the outer packaging may include a shell 51 and a cover plate 53. Among them, the shell 51 may include a bottom plate and a side plate connected to the bottom plate, and the bottom plate and the side plate enclose a receiving cavity. The shell 51 has an opening connected to the receiving cavity, and the cover plate 53 can be covered on the opening to close the receiving cavity. The positive electrode sheet, the negative electrode sheet and the isolation membrane can form an electrode assembly 52 through a winding process or a lamination process. The electrode assembly 52 is encapsulated in the receiving cavity. The electrolyte is infiltrated in the electrode assembly 52. ​​The number of electrode assemblies 52 contained in the secondary battery 5 can be one or more, and those skilled in the art can select according to specific actual needs.

[0144] In addition, the present application also provides an electrical device, which includes at least one of the secondary battery, battery module, or battery pack provided in the present application. The secondary battery, battery module, or battery pack can be used as a power source for the electrical device, and can also be used as an energy storage unit for the electrical device. The electrical device may include mobile devices (such as mobile phones, laptops, etc.), electric vehicles (such as pure electric vehicles, hybrid electric vehicles, plug-in hybrid electric vehicles, electric bicycles, electric scooters, electric golf carts, electric trucks, etc.), electric trains, ships and satellites, energy storage systems, etc., but are not limited thereto.

[0145] As the electrical device, a secondary battery, a battery module or a battery pack may be selected according to its usage requirements.

[0146] Figure 8 The power consumption device is taken as an example, and the power consumption device is a pure electric vehicle, a hybrid electric vehicle, or a plug-in hybrid electric vehicle.

[0147] Another example of a device may be a mobile phone, a tablet computer, a notebook computer, etc. Such a device is usually required to be thin and light, and a secondary battery may be used as a power source.

[0148] Example

[0149] Hereinafter, the embodiments of the present application will be described. The embodiments described below are exemplary and are only used to explain the present application, and should not be construed as limiting the present application. If no specific techniques or conditions are indicated in the embodiments, the techniques or conditions described in the literature in this area or the product specifications are used. If the manufacturer is not indicated in the reagents or instruments used, they are all conventional products that can be obtained commercially.

[0150] 1. Preparation method

[0151] Example 1

[0152] 1) Preparation of positive electrode

[0153] The positive electrode active material lithium nickel cobalt manganese oxide, the binder polyvinylidene fluoride (PVDF), and the conductive agent conductive carbon black (Super-P) were mixed uniformly in N-methylpyrrolidone (NMP) solvent at a mass ratio of 96%:2%:2% to prepare the positive electrode slurry, and the positive electrode slurry was coated on the surface of aluminum foil according to the unit area mass requirement of the positive electrode active material by an extrusion coater and dried, and then the coated electrode was cold pressed by a cold press to prepare the final positive electrode electrode, and the surface density of the positive electrode film layer was 0.224g / 1540.25mm 2 .

[0154] 2) Preparation of negative electrode sheet

[0155] A silicon interface layer was prepared on a 20um thick lithium metal layer using plasma enhanced chemical vapor deposition (PECVD) technology to serve as the negative electrode.

[0156] Ar, SiH4 and N2O are introduced to perform chemical vapor deposition on the lithium metal layer, wherein the volume flow ratio of N2O to SiH4 is 1:2, the deposition time is 1.25 min, the thickness is 25 nm, and the deposited layer is a silicon oxide layer including SiOx, where the x value is 1.

[0157] 3) Preparation of electrolyte

[0158] In an argon atmosphere glove box with a water content of <10ppm, ethylene carbonate (EC), carbonate (PC) and dimethyl carbonate (DMC) were mixed in a mass ratio of EC:PC:DMC=3:3:3, and then LiPF6 was added to the mixed organic solvent and stirred evenly to obtain an electrolyte, wherein the concentration of LiPF6 in the electrolyte was 1 mol / L.

[0159] 4) Isolation film

[0160] A polyethylene film (PE membrane) is used as the isolation membrane.

[0161] 5) Preparation of batteries

[0162] The positive electrode sheet, the separator, and the negative electrode sheet are stacked in order, so that the separator is between the positive and negative electrodes to play a role of isolation, and then wound to obtain a bare cell. The bare cell is placed in an outer package, injected with a prepared electrolyte, and packaged for formation to obtain a lithium-ion battery.

[0163] The preparation method of Example 2 is similar to that of Example 1, except that the preparation method of the negative electrode sheet in Example 2 is:

[0164] Ar, SiH4 and N2O are introduced to perform chemical vapor deposition on the lithium metal layer, wherein the volume flow ratio of N2O to SiH4 is 1:2, the deposition time is 2.5 min, the thickness is 50 nm, and the deposited layer is a silicon oxide layer including SiOx, where the x value is 1.

[0165] The preparation method of Example 3 is similar to that of Example 1, except that the preparation method of the negative electrode sheet in Example 3 is:

[0166] Ar, SiH4 and N2O are introduced to perform chemical vapor deposition on the lithium metal layer, wherein the volume flow ratio of N2O to SiH4 is 1:2, the deposition time is 7.5 min, the thickness is 150 nm, and the deposited layer is a silicon oxide layer including SiOx, where the x value is 1.

[0167] The preparation method of Example 4 is similar to that of Example 1, except that the preparation method of the negative electrode sheet in Example 4 is:

[0168] A silicon interface layer was prepared on a 20um thick lithium metal layer using plasma enhanced chemical vapor deposition (PECVD) technology to serve as the negative electrode.

[0169] Ar, SiH4 and N2O were introduced for deposition on the lithium metal layer, wherein the volume flow ratio of N2O to SiH4 was 1:2, the deposition time was 10 min, and the thickness was 200 nm.

[0170] The preparation method of Example 5 is similar to that of Example 1, except that the preparation method of the negative electrode sheet in Example 5 is:

[0171] A silicon interface layer was prepared on a 20um thick lithium metal layer using plasma enhanced chemical vapor deposition (PECVD) technology to serve as the negative electrode.

[0172] Ar, SiH4 and N2O were introduced for deposition on the lithium metal layer, wherein the volume flow ratio of N2O to SiH4 was 1:2, the deposition time was 50 min, and the thickness was 1000 nm.

[0173] The preparation method of Example 6 is similar to that of Example 1, except that the preparation method of the negative electrode sheet in Example 6 is:

[0174] A silicon interface layer was prepared on a 20um thick lithium metal layer using plasma enhanced chemical vapor deposition (PECVD) technology to serve as the negative electrode.

[0175] Ar, SiH4, and N2O were introduced to deposit on the lithium metal layer, wherein the gas flow ratio of N2O to SiH4 was 20:1, the deposition time was 0.5 min, the thickness was 5 nm, and the deposit included silicon dioxide.

[0176] The preparation method of Example 7 is similar to that of Example 1, except that the preparation method of the negative electrode sheet in Example 7 is:

[0177] A silicon interface layer was prepared on a 20um thick lithium metal layer using plasma enhanced chemical vapor deposition (PECVD) technology to serve as the negative electrode.

[0178] Ar, SiH4, and N2O were introduced to deposit on the lithium metal layer, wherein the gas flow ratio of N2O to SiH4 was 1:2, the deposition time was 7.5 min, the thickness was 150 nm, and the x value was 1;

[0179] The ventilation volume of N2O was increased so that the gas flow ratio of N2O to SiH4 was 20:1, the deposition time was 0.5 min, the thickness was 5 nm, and the deposits included silicon dioxide.

[0180] The preparation method of Example 8 is similar to that of Example 1, except that the preparation method of the negative electrode sheet in Example 8 is:

[0181] A silicon interface layer was prepared on a 20um thick lithium metal layer using plasma enhanced chemical vapor deposition (PECVD) technology to serve as the negative electrode.

[0182] In the initial deposition stage, only SiH4 and Ar are introduced, and the amorphous Si film is directly deposited on the lithium metal negative electrode through the dissociation of SiH4 by plasma in a high vacuum. The deposition time is 1 min and the thickness is 10 nm.

[0183] Ar, SiH4, and N2O were introduced to deposit on the lithium metal layer, where the gas flow ratio of N2O to SiH4 was 1:2, the deposition time was 7.5 min, the thickness was 150 nm, and the deposited SiO x Material, x value is 1;

[0184] The ventilation volume of N2O was increased so that the gas flow ratio of N2O to SiH4 was 20:1, the deposition time was 0.5 min, the deposition layer was a silicon dioxide layer, and the deposition thickness was 5 nm.

[0185] The preparation method of Example 9 is similar to that of Example 1, except that the preparation method of the negative electrode sheet in Example 9 is:

[0186] A silicon interface layer was prepared on a 20um thick lithium metal layer using plasma enhanced chemical vapor deposition (PECVD) technology to serve as the negative electrode.

[0187] In the initial deposition stage, only SiH4 and Ar are introduced, and the amorphous Si film is directly deposited on the lithium metal negative electrode through the dissociation of SiH4 by plasma in a high vacuum. The deposition time is 1 min and the thickness is 10 nm.

[0188] Continue to introduce Ar, SiH4 and N2O for deposition, wherein the volume flow rate of N2O and SiH4 is introduced at a ratio of 1:2 for deposition for 1 minute, increase the N2O ventilation rate so that the volume flow rate of N2O and SiH4 is 2:1, and deposit for 1 minute; increase the N2O ventilation rate so that the volume flow rate of N2O and SiH4 is 5:1 for deposition for 1 minute; increase the N2O ventilation rate so that the volume flow rate of N2O and SiH4 is 8:1 for deposition for 1 minute; increase the N2O ventilation rate so that the volume flow rate of N2O and SiH4 is 11:1 for deposition for 1 minute; increase the N2O ventilation rate so that the volume flow rate of N2O and SiH4 is 14:1 for deposition for 1 minute; increase the N2O ventilation rate so that the volume flow rate of N2O and SiH4 is 17:1 for deposition for 1 minute; increase the N2O ventilation rate so that the volume flow rate of N2O and SiH4 is 18:1 for deposition for 0.5 minute.

[0189] Increase the N2O ventilation volume so that the gas flow ratio of N2O to SiH4 is 20:1 and the deposition time is 0.5 min.

[0190] The preparation method of Example 10 is similar to that of Example 1, except that the preparation method of the negative electrode sheet in Example 10 is:

[0191] A silicon interface layer was prepared on a 20um thick lithium metal layer using plasma enhanced chemical vapor deposition (PECVD) technology to serve as the negative electrode.

[0192] Ar, SiH4, and N2O were introduced for deposition, wherein the gas flow ratio of N2O to SiH4 was 1:2, the deposition time was 2.5 min, and a 50 nm SiOx film was prepared on the upper foundation, and the value of X was 1;

[0193] Increase the N2O ventilation volume so that the gas flow ratio of N2O to SiH4 is greater than 20:1, ensuring that the generated substance is SiO2. The deposition time is 0.5 min, and a 5 nm SiO2 film is deposited on the outermost layer.

[0194] The preparation method of Example 11 is similar to that of Example 1, except that the preparation method of the negative electrode sheet in Example 11 is:

[0195] A silicon interface layer was prepared on a 20um thick lithium metal layer using plasma enhanced chemical vapor deposition (PECVD) technology to serve as the negative electrode.

[0196] In the initial deposition stage, only SiH4 and Ar were introduced, and the amorphous Si film was directly deposited on the lithium metal negative electrode through the dissociation of SiH4 by plasma in a high vacuum. The deposition time was 10 min and the thickness was 100 nm.

[0197] Ar, SiH4, and N2O were introduced to deposit on the lithium metal layer, where the gas flow ratio of N2O to SiH4 was 1:2, the deposition time was 2.5 min, the thickness was 50 nm, and the deposited SiO x Material, x value is 1;

[0198] The ventilation volume of N2O was increased so that the gas flow ratio of N2O to SiH4 was 20:1, the deposition time was 0.5 min, the deposition layer was a silicon dioxide layer, and the deposition thickness was 5 nm.

[0199] The preparation method of Example 12 is similar to that of Example 1, except that the preparation method of the negative electrode sheet in Example 12 is:

[0200] A silicon interface layer was prepared on a 20um thick lithium metal layer using plasma enhanced chemical vapor deposition (PECVD) technology to serve as the negative electrode.

[0201] In the initial deposition stage, only SiH4 and Ar were introduced, and the amorphous Si film was directly deposited on the lithium metal negative electrode through the dissociation of SiH4 by plasma in a high vacuum. The deposition time was 10 min and the thickness was 100 nm.

[0202] Ar, SiH4, and N2O were introduced to deposit on the lithium metal layer, where the gas flow ratio of N2O to SiH4 was 1:2, the deposition time was 2.5 min, the thickness was 50 nm, and the deposited SiO x Material, x value is 1.

[0203] Comparative Example 1

[0204] In Comparative Example 1, the lithium metal layer is used as the negative electrode plate, and the rest is the same as in Example 1. The negative electrode gram capacity of the battery is 3860 mAh / g.

[0205] 2. Test Method

[0206] 1) Normal temperature cycle capacity retention rate

[0207] At 25°C, the lithium secondary battery is first charged at a constant current of 1C (i.e., the current value that completely discharges the theoretical capacity within 1 hour) to a voltage of 3.65V, then charged at a constant voltage of 3.65V to a current of 0.05C. After standing for 5 minutes, the lithium secondary battery is discharged at a constant current of 1C to a voltage of 2.5V. This is a charge and discharge cycle process, and the discharge capacity this time is the discharge capacity of the first cycle. The lithium ion secondary battery is subjected to multiple cycle charge and discharge tests according to the above method, and the discharge capacity of the 500th cycle is detected.

[0208] Capacity retention rate of lithium secondary battery after 500 cycles = (discharge capacity at 500th cycle / discharge capacity at first cycle) × 100%.

[0209] 2) Negative electrode potential

[0210] The test method of the negative electrode potential refers to CN115825765A. The brief test method includes:

[0211] Prepare the reference electrode.

[0212] The copper wire was soaked in concentrated sulfuric acid for 50 minutes (min), then rinsed with deionized water three times, rinsed with ethanol three times and dried to remove the oxide layer on the surface of the copper wire. After that, the surface oxide layer of the copper wire was observed under CCD to see if it was completely removed. If not, the above process of removing the oxide layer was repeated until the surface oxide layer of the copper wire was completely removed. The diameter of the copper wire was about 6 microns (μm).

[0213] Preparation of three electrodes

[0214] The materials prepared in the above steps are assembled into a laminated battery in the order of positive electrode sheet, separator, negative electrode sheet, separator, reference electrode, separator and positive electrode sheet.

[0215] Lithium plating of the reference electrode

[0216] Connect the positive electrode of the battery to the reference electrode, and use a current of 20 microamperes (μA) to charge the battery for two hours, so that lithium is plated on the side of the reference electrode close to the positive electrode. Similarly, connect the negative electrode of the battery to the reference electrode, and use a current of 20μA to charge the battery for two hours, so that lithium is plated on the side of the reference electrode close to the negative electrode. The entire lithium plating process is completed.

[0217] Calibration of three electrodes

[0218] Use a multimeter to detect the positive and negative electrode voltage V1, the positive electrode and reference voltage V2, and the reference electrode and negative electrode voltage V3. If V1 = V2 + V3, the three electrodes of the battery cell are normal and continue to the next step of testing. Otherwise, re-prepare the three electrodes.

[0219] A first potential of the negative electrode and a second potential of the reference electrode are monitored.

[0220] During the battery charging and discharging process, the first potential of the negative electrode and the second potential of the reference electrode are monitored. At 25 degrees Celsius (℃), the battery cell is charged to 4.2V at a constant current of 1 / 3C, left for 5 minutes, and then discharged to 2.8V at 1 / 3C. During this process, the first potential of the negative electrode and the second potential of the reference electrode are detected in real time, thereby achieving real-time monitoring of the negative electrode potential of the battery cell.

[0221] 3) Negative electrode capacity test

[0222] Punch the prepared lithium metal negative electrode into a 14mm original sheet in the glove box. The water and oxygen content in the glove box is less than 0.5ppm, and a CR2025 positive electrode shell is used to assemble the button battery. After the successfully assembled button battery is left to stand for 24 hours, the Xinwei test platform is used to set the charge and discharge voltage range to 2.5V-4.2V, and the test temperature is controlled at 25°C. Set the theoretical gram capacity to 3860mAh / g, then discharge to 2.5V at 0.05C, stand for 5 minutes, charge to 4.2V at 0.05C, and then charge at a constant voltage until the current is 0.01C cutoff. After standing for 30 minutes, discharge to 2.5V at 0.05C. The capacity at this step is the battery capacity. Divide the mass of the negative electrode active material by this capacity to get the negative electrode gram capacity.

[0223] III. Analysis of test results of various embodiments and comparative examples

[0224] The batteries of the embodiments and comparative examples were prepared according to the above method, and various performance parameters were measured. The results are shown in Table 1 below.

[0225] Table 1

[0226]

[0227] As can be seen from Examples 1-5, when the thickness of the silicon interface layer is 25nm-1000nm, lithium metal has a higher negative electrode potential, can inhibit dendrite growth, and further improves the cycle stability of the battery. When the thickness of the silicon interface layer is 50nm-200nm, the battery has both high cycle stability and gram capacity.

[0228] From the comparison of Examples 3, 8-9, and Examples 2, 10-12, it can be seen that in the thickness direction of the silicon interface layer, the oxygen content of the silicon interface layer close to the metal layer is lower than the oxygen content far from the metal layer. Compared with the silicon interface layer containing a single component, the comprehensive performance of the battery including cycle stability and gram capacity can be further optimized.

[0229] From the comparison between Example 9 and Example 8, it can be seen that the gradual change of the content of the silicon oxide layer can further improve the cycle stability and gram capacity of the battery.

[0230] It should be noted that the present application is not limited to the above-mentioned embodiments. The above-mentioned embodiments are only examples, and the embodiments having the same structure as the technical idea and exerting the same effect within the scope of the technical solution of the present application are all included in the technical scope of the present application. In addition, without departing from the scope of the main purpose of the present application, various modifications that can be thought of by those skilled in the art to the embodiments and other methods of combining some of the constituent elements in the embodiments are also included in the scope of the present application.

Claims

1. A negative electrode plate, characterized in that: It includes a metal layer and a silicon interface layer located on at least one side of the metal layer, wherein the silicon interface layer includes a general formula of SiO x of materials, where 0≤x≤2.

2. The negative electrode sheet according to claim 1, characterized in that: The silicon interface layer comprises a general formula of SiO x Material, where 0<x<2, optionally 0.7<x<1.

5.

3. The negative electrode sheet according to claim 1 or 2, characterized in that: The thickness of the silicon interface layer is 25nm-1000nm, and can be optionally 50nm-200nm.

4. The negative electrode sheet according to any one of claims 1 to 3, characterized in that: In the thickness direction of the silicon interface layer, the oxygen content of the silicon interface layer close to the metal layer is lower than the oxygen content of the silicon interface layer far from the metal layer.

5. The negative electrode sheet according to any one of claims 1 to 4, characterized in that: In the thickness direction of the silicon interface layer from close to the metal layer to far away from the metal layer, the silicon interface layer sequentially includes a silicon layer and a silicon oxide layer, the silicon layer includes elemental silicon, and the silicon oxide layer includes a general formula of SiO x material, where 0<x<2.

6. The negative electrode sheet according to any one of claims 1 to 4, characterized in that: In the thickness direction of the silicon interface layer from close to the metal layer to far away from the metal layer, the silicon interface layer includes a silicon oxide layer and a silicon dioxide layer in sequence, and the silicon oxide layer includes a general formula of SiO x material, where 0<x<2.

7. The negative electrode sheet according to any one of claims 1 to 4, characterized in that: In the thickness direction of the silicon interface layer from close to the metal layer to far away from the metal layer, the silicon interface layer sequentially includes a silicon layer, a silicon oxide layer and a silicon dioxide layer, the silicon layer includes amorphous silicon, the silicon oxide layer includes a general formula of SiO x material, where 0<x<2.

8. The negative electrode sheet according to any one of claims 1 to 7, characterized in that: In the thickness direction of the silicon interface layer from close to the metal layer to far away from the metal layer, the silicon interface layer includes SiOx1 layer, SiOx2 layer, SiOx n Layer, where 0<x1<x2<……<x n <2, n≥2.

9. The negative electrode sheet according to any one of claims 1 to 8, characterized in that: The negative electrode plate satisfies at least one of the following conditions: (i) the ratio of the thickness of the silicon layer to the thickness of the silicon oxide layer is 4-15; (ii) the thickness of the silicon layer is 10 nm to 100 nm; (iii) the thickness of the silicon oxide layer is 25nm-150nm; (iv) The thickness of the silicon dioxide layer is 1 nm-10 nm.

10. The negative electrode sheet according to any one of claims 1 to 9, characterized in that: The metal layer includes at least one of lithium metal, lithium alloy, sodium metal, and sodium alloy.

11. The negative electrode sheet according to any one of claims 1 to 10, characterized in that: The silicon interface layer is prepared by at least one of chemical vapor deposition, atomic layer deposition, evaporation and magnetron sputtering.

12. A method for preparing a negative electrode sheet, characterized in that: The preparation method comprises: depositing a silicon interface layer on at least one side of a metal layer to prepare the negative electrode plate, wherein the silicon interface layer comprises a general formula of SiO x of materials, where 0≤x≤2.

13. The preparation method according to claim 12, characterized in that: The preparation method comprises: A gas containing a silicon source or a mixed gas containing an oxygen source and a silicon source is introduced to prepare the silicon interface layer by chemical vapor deposition; optionally, the oxygen source includes N2O, and the silicon source includes SiH4.

14. The preparation method according to claim 13, characterized in that: The preparation method comprises: The volume flow ratio M of the oxygen source and the silicon source is 0<M<20, and the silicon interface layer includes a material of the general formula SiOx, wherein 0<x<2.

15. The preparation method according to any one of claims 13 or 14, characterized in that: During the preparation of the silicon interface layer, the introduction ratio M of the oxygen source to the silicon source is increased so that the oxygen content of the silicon interface layer close to the metal layer is lower than the oxygen content far from the metal layer in the thickness direction of the silicon interface layer.

16. The preparation method according to any one of claims 12 to 15, characterized in that: The preparation method comprises: introducing the silicon source for deposition; After a period of deposition, the oxygen source and the silicon source are introduced to perform deposition, wherein the volume flow ratio M of the oxygen source to the silicon source is 0<M<20.

17. The preparation method according to any one of claims 12 to 15, characterized in that: The preparation method comprises: Passing the oxygen source and the silicon source into the deposition, wherein the volume flow ratio M of the oxygen source to the silicon source is 0<M<20; After a period of deposition, the volume flow ratio M of the oxygen source to the silicon source is increased to not less than 20 for deposition.

18. The preparation method according to any one of claims 12 to 15, characterized in that: The preparation method comprises: introducing the silicon source for deposition; After a period of deposition, the oxygen source and the silicon source are introduced for deposition, wherein the volume flow ratio M of the oxygen source and the silicon source is 0<M<20; After a period of deposition, the ratio M of the oxygen source to the silicon source is increased to not less than 20 for deposition.

19. The preparation method according to any one of claims 12 to 18, characterized in that: The preparation method comprises: During the process of introducing the oxygen source and the silicon source for deposition, the volume flow ratio M of the oxygen source and the silicon source is gradually increased.

20. A secondary battery, characterized in that: A negative electrode sheet comprising the negative electrode sheet according to any one of claims 1 to 12, and / or a negative electrode sheet prepared by the preparation method according to any one of claims 13 to 19.

21. The secondary battery according to claim 20, characterized in that: The secondary battery includes an electrolyte, and the silicon interface layer is located between the electrolyte and the metal layer.

22. An electrical device, characterized in that: Includes the secondary battery according to claim 20 or 21.

Citation Information

Patent Citations

  • Negative plate, lithium-sulfur battery and preparation method of lithium-sulfur battery

    CN113314708A

  • Negative pole piece and metal lithium battery

    CN114512674A

  • Production method of negative electrode for lithium ion secondary battery

    KR1020060069295A

  • The Method of Manufacturing Ice Cream using Corn and Honey

    KR1020220119196A

  • Negative electrode for lithium-ion battery, production method therefor, and lithium-ion battery

    US20120107684A1