Lithium iron phosphate positive electrode material and preparation method thereof

The carbon cladding defects of lithium iron phosphate positive electrode material were repaired through two carbon coating processes, forming a more uniform second carbon cladding layer, solving the problems of poor conductivity and poor processing performance of lithium iron phosphate positive electrode material, significantly improving The cycle life and electrical properties of the material are obtained.

CN119069657APending Publication Date: 2024-12-03NANTONG RESHINE NEW MATERIAL CO LTD

Patent Information

Application Number
CN202310634170.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-31
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

The lithium iron phosphate positive electrode material has poor intrinsic conductivity and large specific surface area, resulting in poor processing performance. The existing carbon coating process is prone to crushing and peeling during the crushing process, resulting in an increase in free carbon and defects, reducing conductivity and cycle life.

Method used

Using two carbon coating processes, the lithium iron phosphate raw material is sintered and crushed to form a first carbon coating layer, and then the second carbon source is evenly wrapped on the surface of the crushed material, and then the second sintered and crushed to form a A second carbon cladding with fewer defects.

Benefits of technology

By repairing the defects of the first carbon cladding layer, more uniform carbon cladding is achieved, the specific surface area is reduced, the conductivity and cycle life are improved, and the processing and electrical performance are improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119069657A_ABST
    Figure CN119069657A_ABST
Patent Text Reader

Abstract

The invention relates to a lithium iron phosphate positive electrode material and a preparation method thereof, and belongs to the technical field of lithium ion battery positive electrode materials. The preparation method comprises the following steps: firstly, sequentially carrying out first sintering and first crushing treatment on a first raw material to obtain a first crushed material; uniformly wrapping the particle surface of the first crushed material with a second carbon source to obtain a coated material; and sequentially carrying out second sintering and second crushing treatment on the coated material to obtain the lithium iron phosphate positive electrode material. Wherein the first crushed material comprises lithium iron phosphate particles with a first carbon coating layer on the surface, the lithium iron phosphate positive electrode material comprises lithium iron phosphate particles with a second carbon coating layer on the surface, and the second carbon coating layer has fewer defects than the first carbon coating layer. Through the secondary carbon coating process, more uniform carbon coating is realized on the surface of the lithium iron phosphate, and the powder resistivity and the specific surface area of the positive electrode material are reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of lithium ion battery positive electrode materials, and in particular to a lithium iron phosphate positive electrode material and a preparation method thereof. Background Art

[0002] Currently, lithium-ion batteries are the most widely used in commercial applications, but as the demand for lithium-ion batteries increases, the problem of lithium scarcity is becoming increasingly prominent.

[0003] Although the ternary cathode materials used in lithium-ion batteries have high energy density and power density, a single ton of ternary cathode materials requires 470kg of lithium hydroxide or 420kg of lithium carbonate. With the rise in lithium salt prices, the cost of raw materials for ternary cathode materials has further increased. The raw materials required for the synthesis of lithium iron phosphate are iron phosphate and lithium carbonate. The synthesis of iron phosphate uses ferrous sulfate, a byproduct of titanium dioxide synthesis, which has a lower cost. The lithium salt consumption required for the synthesis of a single ton of lithium iron phosphate is about 240kg, which is about 57% of the lithium salt consumption of ternary cathode materials. The cost of lithium salt has dropped significantly. In comprehensive comparison, the cost-effectiveness of lithium iron phosphate materials is obvious. Combined with its inherent high safety characteristics, lithium iron phosphate has significant advantages in the fields of power batteries and energy storage batteries.

[0004] Although lithium iron phosphate has the advantages of cost-effectiveness and high safety, it still has the problems of poor intrinsic conductivity and large specific surface area, which leads to poor processing performance. The industry mainly improves these problems by carbon coating on the surface of lithium iron phosphate. Under the existing lithium iron phosphate preparation process conditions, carbon coating is mainly achieved by dissolving a soluble carbon source (such as glucose) and grinding it together with iron phosphate and lithium carbonate, and then quickly drying it through spray drying to achieve uniform liquid phase coating, and then sintering it at high temperature in an inert atmosphere to achieve uniform carbon coating by high-temperature carbonization of the carbon source. However, the sintered material needs to be crushed by high-intensity airflow. During the crushing, there are nanoparticles that are broken and peeled off. Part of the carbon coating layer will peel off from the lithium iron phosphate matrix, resulting in a large amount of free carbon in the positive electrode material, reducing the conductivity of the positive electrode material and increasing the resistivity of the powder. Moreover, due to the destruction of the carbon coating layer, a large number of defects are formed on the surface of lithium iron phosphate, which increases the specific surface area of ​​the positive electrode material, which is not conducive to improving the processing performance and cycle life of the positive electrode material. Summary of the invention

[0005] The present invention aims at solving the problems in the prior art and provides a lithium iron phosphate positive electrode material and a preparation method thereof, which can modify the defects on the surface of the lithium iron phosphate and improve the conductivity of the positive electrode material.

[0006] To achieve the above object, the present invention provides the following technical solution: a method for preparing a lithium iron phosphate positive electrode material, comprising: The first raw material is subjected to a first sintering and a first pulverizing treatment in sequence to obtain a first pulverized material; the first raw material comprises at least iron phosphate, a lithium source, and a first carbon source, and the first pulverized material comprises lithium iron phosphate particles having a first carbon coating layer on the surface; Uniformly coating the second carbon source on the surface of the particles of the first pulverized material to obtain a coated material; The coated material is subjected to a second sintering and a second pulverizing treatment in sequence to obtain a lithium iron phosphate positive electrode material; the lithium iron phosphate positive electrode material includes lithium iron phosphate particles having a second carbon coating layer on the surface, and the second carbon coating layer has a smaller number of defects than the first carbon coating layer.

[0007] Optionally, the step of uniformly coating the second carbon source on the particle surface of the first pulverized material to obtain a coated material comprises: The second carbon source and a corresponding solvent are configured into a carbon source solution; The carbon source solution is atomized into micron-sized droplets and then evenly sprayed onto the particle surface of the first pulverized material; wherein the concentration of the second carbon source in the carbon source solution is 10% to 20%.

[0008] Optionally, the carbon source solution accounts for 1% to 15% by weight of the first pulverized material.

[0009] Optionally, the second carbon source is the same as the first carbon source, which is at least one of polyethylene glycol, polyvinyl alcohol and glucose.

[0010] Optionally, the second pulverization is performed under an inert gas atmosphere.

[0011] Optionally, after the second pulverization treatment, the D50 of the lithium iron phosphate positive electrode material is 0.6 μm to 1.5 μm.

[0012] Optionally, the sintering temperature of the second sintering is 300°C to 750°C.

[0013] Optionally, the sintering temperature of the first sintering is 300°C to 750°C.

[0014] Optionally, after the first pulverizing treatment, the D50 of the first pulverized material is 0.6 μm to 1.5 μm.

[0015] To achieve the above object, the present invention also provides the following technical solution: a lithium iron phosphate positive electrode material, wherein the lithium iron phosphate positive electrode material is prepared according to the preparation method described in the above technical solution.

[0016] The beneficial effects of the present invention are as follows: relative to the prior art, the present invention first performs a first sintering and a first pulverizing treatment on the first raw material in sequence to obtain a first pulverized material; then the second carbon source is uniformly wrapped on the particle surface of the first pulverized material to obtain a coated material; and the coated material is then subjected to a second sintering and a second pulverizing treatment in sequence to obtain a lithium iron phosphate positive electrode material. The first pulverized material includes lithium iron phosphate particles having a first carbon coating layer on the surface, and the lithium iron phosphate positive electrode material includes lithium iron phosphate particles having a second carbon coating layer on the surface, and the second carbon coating layer has a smaller number of defects than the first carbon coating layer. It can be seen that the present invention, through the second carbon coating process, coats the free carbon in the first pulverized material again on the surface of lithium iron phosphate, repairs the defects of the first carbon coating layer, forms a second carbon coating layer with fewer defects, and achieves a more uniform carbon coating on the surface of lithium iron phosphate, reducing the specific surface area of ​​the positive electrode material, thereby improving the processing performance. In addition, the carbon coating with fewer defects and more uniformity can also reduce the powder resistivity of the positive electrode material and improve the cycle life. BRIEF DESCRIPTION OF THE DRAWINGS

[0017] In order to more clearly illustrate the technical solutions in the embodiments of the present invention, the following briefly introduces the drawings required for describing the embodiments. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without creative work. Among them: Figure 1 It is a schematic diagram of a process for preparing a lithium iron phosphate positive electrode material according to an embodiment of the present invention; Figure 2 is the XRD pattern of the comparative example; Figure 3 is the XRD pattern of Example 1; Figure 4 The SEM images of the comparative example and embodiment 1 are compared. DETAILED DESCRIPTION

[0018] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0019] See also Figure 1 , Figure 1 1 is a flow chart of an embodiment of a method for preparing a lithium iron phosphate positive electrode material of the present invention. The method comprises the following steps S11-S13.

[0020] Step S11, performing a first sintering and a first pulverizing process on the first raw material in sequence to obtain a first pulverized material, wherein the first pulverized material includes lithium iron phosphate particles having a first carbon coating layer on the surface.

[0021] The first raw material includes at least iron phosphate, a lithium source, and a first carbon source, and may also include additives for other improvement purposes. The lithium source is a common lithium source in the prior art, such as lithium carbonate, lithium hydroxide, etc. The first carbon source is a soluble carbon source such as polyethylene glycol, polyvinyl alcohol and glucose. This step is to achieve carbon coating on its surface while forming lithium iron phosphate. Specifically, the carbon coating is mainly achieved by sand grinding with iron phosphate and lithium source after the carbon source is dissolved, and then the liquid phase is uniformly coated by rapid drying by spray drying, and then the carbon source is carbonized at high temperature to achieve uniform carbon coating after high temperature sintering in an inert atmosphere. The first crushed material obtained in this step includes lithium iron phosphate particles having a first carbon coating layer on the surface. The first crushing treatment damages the first carbon coating layer, so that there are a large number of defects in the first carbon coating layer, and there is a large amount of free carbon in the first crushed material.

[0022] Specifically, the sintering temperature of the first sintering is 300° C. to 750° C., for example, 350° C., 400° C., 450° C., 500° C., 550° C., 600° C., 650° C., 700° C., etc. After the first pulverization process, the parameter D50 representing the particle size distribution of the first pulverized material is 0.6 μm to 1.5 μm, for example, 0.7 μm, 0.8 μm, 0.9 μm, 1.0 μm, 1.1 μm, 1.2 μm, 1.3 μm, 1.4 μm, etc.

[0023] Step S12, uniformly coating the second carbon source on the particle surface of the first pulverized material to obtain a coated material.

[0024] Specifically, the coated material can be obtained by the following steps: Step 1: Prepare a carbon source solution by mixing a second carbon source and a corresponding solvent. The second carbon source is the same as the first carbon source, and is at least one of polyethylene glycol, polyvinyl alcohol and glucose. The concentration of the second carbon source in the carbon source solution is 10% to 20%, such as 12%, 14%, 16%, 18%, etc.

[0025] Step 2: atomize the carbon source solution into micron-sized droplets and then evenly spray them onto the particle surface of the first pulverized material.

[0026] The weight percentage of the carbon source solution to the first pulverized material is 1% to 10%, such as 2%, 4%, 6%, 8%, etc. This is a wet coating process, and this embodiment limits the carbon source solution. In other embodiments, a dry coating process can also be used, using a fluidized bed to mix the second carbon source and the first pulverized material to achieve coating.

[0027] Step S13, performing a second sintering and a second pulverizing treatment on the coated material in sequence to obtain a lithium iron phosphate positive electrode material, wherein the lithium iron phosphate positive electrode material includes lithium iron phosphate particles having a second carbon coating layer on the surface, and the second carbon coating layer has fewer defects than the first carbon coating layer.

[0028] The sintering temperature of the second sintering is 300°C to 750°C, such as 350°C, 400°C, 450°C, 500°C, 550°C, 600°C, 650°C, 700°C, etc. The second pulverization is performed under an inert gas atmosphere. After the second pulverization, the parameter D50 representing the particle size distribution of the lithium iron phosphate positive electrode material is 0.6μm to 1.5μm, such as 0.7μm, 0.8μm, 0.9μm, 1.0μm, 1.1μm, 1.2μm, 1.3μm, 1.4μm, etc.

[0029] In this embodiment, the free carbon in the first crushed material is coated again on the surface of lithium iron phosphate through the second carbon coating process, the defects of the first carbon coating layer are repaired, and a second carbon coating layer with fewer defects is formed, which achieves more uniform carbon coating on the surface of lithium iron phosphate, reduces the specific surface area of ​​the positive electrode material, and thus improves the processing performance. In addition, the more uniform carbon coating with fewer defects can also reduce the powder resistivity of the positive electrode material and improve the cycle life.

[0030] Based on the same inventive concept, the present invention also provides a lithium iron phosphate positive electrode material, which is prepared by the preparation method described in the above embodiment and has the same beneficial effects as the above embodiment, which will not be repeated here.

[0031] The beneficial effects of the present invention are described below by means of specific comparative examples and embodiments.

[0032] Comparative Example The lithium iron phosphate positive electrode material prepared by the following steps is recorded as a comparative example: (1) Weigh 50 kg of iron phosphate, 12.36 kg of lithium carbonate, 5.07 kg of glucose, 87.46 g of TiO2 and 187.14 g of V2O5 as additives, add the above raw materials into 90 kg of pure water, and stir with a paddle stirrer for 30 minutes; (2) The slurry after stirring and dispersing was ground to D50 = 1.45 μm using a sand mill (coarse grinding, zirconium bead diameter 0.6 mm) to obtain slurry J1, and then 79.2 kg (accounting for 50% of the total volume of the slurry) was taken out from the J1 slurry and transferred to the fine grinding system for fine grinding to D50 = 0.35-0.40 μm to obtain slurry J2, and then the remaining J1 slurry and J2 slurry were transferred to a mixing tank for stirring and mixing for 30 minutes to obtain slurry J3, and the D50 of slurry J3 was 1.0 μm; (3) The slurry J3 is dried using a spray dryer. The material after drying has a D50 of 10-25 μm and a moisture content of about 2%, thereby obtaining a first raw material. (4) placing the first raw material into a graphite crucible for the first sintering, heating to 740° C. at a heating rate of 5° C. / min under a nitrogen atmosphere, and keeping the temperature for 8 h; (5) The material after the first sintering is subjected to a first pulverization treatment using a jet mill to obtain a lithium iron phosphate positive electrode material of a comparative example. Example

[0033] The lithium iron phosphate positive electrode material prepared by the following steps is recorded as Example 1: (1) Obtain the first raw material according to the same process as in the comparative example; (2) placing the first raw material into a graphite crucible for the first sintering, heating to 600° C. at a heating rate of 5° C. / min under a nitrogen atmosphere, and keeping the temperature for 5 h; (3) The first sintered material is subjected to a first pulverization process using a jet mill to obtain a first pulverized material S1; (4) preparing a glucose solution with a concentration of 20%, atomizing the glucose solution into micron-sized droplets through a high-pressure atomizing nozzle, and then evenly spraying the droplets onto the particle surface of the first pulverized material S1 to obtain a coated material C1; wherein the weight of the glucose solution accounts for 10% of the total weight of the first pulverized material S1; (5) The coated material C1 was placed in a graphite crucible for the second sintering, and heated to 740°C at a heating rate of 5°C / min under a nitrogen atmosphere for the first time, and kept at this temperature for 5 h; (6) The material after the second sintering is subjected to a second pulverization treatment using a jet mill to obtain the lithium iron phosphate positive electrode material of Example 1. Example

[0034] The difference from Example 1 is that during the first sintering, the material is heated to 500° C. for the first time, and the remaining processes are the same to obtain the lithium iron phosphate positive electrode material of Example 2. Example

[0035] The difference from Example 1 is that during the first sintering, the material is heated to 400° C. for the first time, and the remaining processes are the same to obtain the lithium iron phosphate positive electrode material of Example 3.

[0036] The comparative examples and embodiments 1-3 of the present invention are characterized. Figure 2 and Figure 3 They are the XRD spectra of the comparative example and embodiment 1, and it can be seen from the characteristic peaks of the phase that the phases under the two processes are pure lithium iron phosphate. Figure 4The SEM images of the comparative example and Example 1 show that the surface of the lithium iron phosphate positive electrode material of Example 1 prepared by the method of the present invention is smoother and rounder. After the second carbon coating, the second carbon coating layer on the surface of the lithium iron phosphate particles has a smaller number of defects, and the carbon coating effect is better.

[0037] The lithium iron phosphate positive electrode materials obtained in the above comparative example and Examples 1-3 were made into batteries and then tested for key technical indicators such as charge and discharge capacity. The test results are shown in Table 1 below.

[0038] From the data in Table 1, it can be seen that the lithium iron phosphate positive electrode material prepared by the second carbon coating process of the present invention, especially Example 1, has a higher compaction density and a discharge capacity retention rate at a high rate. In addition, at the same level of carbon content, the material prepared by the secondary carbon coating process has a smaller specific surface area, which is about 73% of the conventional process, and the powder resistivity of the material is significantly reduced. Therefore, the technical solution provided by the present invention significantly improves the processing performance and electrical properties of the material, and has significant performance advantages.

[0039]

[0040] The above description is only an implementation mode of the present invention, and does not limit the patent scope of the present invention. Any equivalent structure or equivalent process transformation made by using the contents of the present invention specification and drawings, or directly or indirectly applied in other related technical fields, are also included in the patent protection scope of the present invention.

Claims

1. A method for preparing a lithium iron phosphate positive electrode material, characterized in that: include: The first raw material is subjected to a first sintering and a first pulverizing treatment in sequence to obtain a first pulverized material; the first raw material comprises at least iron phosphate, a lithium source, and a first carbon source, and the first pulverized material comprises lithium iron phosphate particles having a first carbon coating layer on the surface; Uniformly coating the second carbon source on the surface of the particles of the first pulverized material to obtain a coated material; The coated material is subjected to a second sintering and a second pulverizing treatment in sequence to obtain a lithium iron phosphate positive electrode material; the lithium iron phosphate positive electrode material includes lithium iron phosphate particles having a second carbon coating layer on the surface, and the second carbon coating layer has a smaller number of defects than the first carbon coating layer.

2. The preparation method according to claim 1, characterized in that: The step of uniformly coating the second carbon source on the particle surface of the first pulverized material to obtain the coated material comprises: The second carbon source and a corresponding solvent are configured into a carbon source solution; The carbon source solution is atomized into micron-sized droplets and then evenly sprayed onto the particle surface of the first pulverized material; wherein the concentration of the second carbon source in the carbon source solution is 10% to 20%.

3. The preparation method according to claim 2, characterized in that: The weight percentage of the carbon source solution to the first pulverized material is 1% to 15%.

4. The preparation method according to claim 2, characterized in that: The second carbon source is the same as the first carbon source and is at least one of polyethylene glycol, polyvinyl alcohol and glucose.

5. The preparation method according to any one of claims 1 to 4, characterized in that: The second pulverization is performed under an inert gas atmosphere.

6. The preparation method according to claim 5, characterized in that: After the second pulverization process, the D50 of the lithium iron phosphate positive electrode material is 0.6 μm to 1.5 μm.

7. The preparation method according to any one of claims 1 to 4, characterized in that: The sintering temperature of the second sintering is 300°C to 750°C.

8. The preparation method according to claim 1, characterized in that: The sintering temperature of the first sintering is 300°C to 750°C.

9. The preparation method according to claim 8, characterized in that: After the first pulverization process, D50 of the first pulverized material is 0.6 μm to 1.5 μm.

10. A lithium iron phosphate positive electrode material, characterized in that: The lithium iron phosphate positive electrode material is prepared according to the preparation method according to any one of claims 1-9.

Citation Information

Patent Citations

  • Method for industrially producing lithium-iron-phosphate positive pole material

    CN102881902A

  • Method for preparing lithium iron phosphate material by adopting cold-rolled byproduct iron oxide

    CN104269553A

  • Synthetic method capable of increasing low-temperature performance of lithium iron phosphate

    CN106554003A

  • Preparation method and application of lithium iron phosphate positive electrode material

    CN112897491A

  • Lithium iron phosphate composite material and preparation method thereof

    CN113130899A

Cited By

  • Preparation method of low-resistance lithium iron phosphate

    CN120553665A