Positive electrode material and preparation method thereof
By using organic solvent wet mixing method on high nickel positive electrode materials, the problem of high nickel positive electrode materials is solved, and the positive electrode with high energy density and high discharge capacity is achieved Materials, reducing preparation costs and energy consumption.
Patent Information
- Application Number
- CN202310651834.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-06-02
- Publication Date
- 2024-12-03
AI Technical Summary
High nickel positive electrode materials are sensitive to moisture, and the electrical properties of halide solid electrolytes are insufficient when combined with them, making it difficult to improve mechanical properties while reducing the thickness of the electrolyte.
The positive electrode material is prepared by wet mixing method of organic solvents. By forming a solid electrolyte coating of Li3InClxFy type on the surface of lithium metallic acid material, a uniform core-shell structure is formed, and the composition ratio of chlorine and fluorine is controlled to improve electrical performance.
A high energy density and low cost positive electrode material is achieved, which significantly improves the discharge capacity and discharge capacity storage rate, reduces preparation cost and energy consumption, and enhances the mechanical properties of the material.
Smart Images

Figure CN119069663A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a cathode material and a preparation method thereof, and particularly to a cathode material prepared through an organic solvent and having a solid electrolyte coating layer, and a preparation method thereof, so as to improve the electrical performance. Background Art
[0002] Under the considerations of safety and energy density, the development of solid-state batteries has become a mainstream trend in recent years. Compared with traditional lithium batteries, there is still room for improvement in various aspects of solid-state batteries. In terms of cathode materials, high-nickel cathode materials have the defect of high sensitivity to moisture; in terms of solid electrolytes, how to improve the mechanical properties while reducing its thickness is also a challenging topic.
[0003] Among various solid electrolytes, the most promising types for mass production are oxide solid electrolyte, sulfide solid electrolyte, and halide solid electrolyte. Among them, halide solid electrolyte has the characteristics of high stability, high safety, high ionic conductivity, and low interface impedance, and is one of the materials widely discussed in recent years. However, halide solid electrolyte also has the defect of high sensitivity to moisture like high-nickel cathode materials, and Li3InCl6, the most widely used in halide solid electrolytes, also has room for improvement in electrical performance.
[0004] In view of this, it is necessary to provide a cathode material prepared through an organic solvent and having a solid electrolyte coating layer, so as to eliminate the negative impact of moisture on the cathode material and improve the electrical performance, and solve the deficiencies of the prior art. Summary of the Invention
[0005] The object of the present invention is to provide a cathode material and a preparation method thereof. The cathode material is composed of a plurality of particles, and each particle includes a core layer and a coating layer covering the core layer. The core layer is composed of a lithium metal oxide material with the composition of Li[Ni a Co b Mn c Al d O2, and 0.8 < x < 1. Through the high nickel content in the core layer, a cathode material with high energy density and low cost can be realized. The coating layer is composed of a solid electrolyte with the composition of Li3InCl x F y . By forming the solid electrolyte with chlorine and fluorine, a cathode material with high discharge capacity and extremely high discharge capacity retention rate can be obtained. In the composition of the solid electrolyte Li3InCl x F yAmong them, the numerical ranges of the coefficients x and y are more specifically, for example, 4 ≤ x ≤ 5.5 and 0.5 ≤ y ≤ 2. By controlling the composition ratios of chlorine and fluorine in the solid electrolyte, the aforementioned electrical performance can be further improved. The weight ratio of the lithium metal oxide material of the core layer to the solid electrolyte of the coating layer is more specifically, for example, between 1:0.3 and 1:0.6, so as to form a cathode material with a uniform core-shell structure.
[0006] Another object of the present invention is to provide a cathode material and a method for preparing the same. The cathode material is formed by mixing a lithium metal oxide material with the composition of Li[Ni a Co b Mn c Al d O2 and a first raw material including lithium, indium, chlorine and fluorine in an organic solvent, and then through heat treatment. Compared with dry mixing, wet mixing with an organic solvent has low cost and is easy to control. It can also improve the solid dispersion when making electrodes while eliminating the negative impact of moisture. Furthermore, through wet mixing, the first raw material can directly react on the surface of the lithium metal oxide material particles to achieve in-situ synthesis, and then form a cathode material with a uniform core-shell structure to improve the electrical performance. The temperature of the heat treatment is, for example, between 100°C and 250°C, with low energy consumption, saving manufacturing costs and having environmental benefits.
[0007] To achieve the aforementioned object, the present invention provides a cathode material composed of a plurality of particles, and each of the plurality of particles includes a core layer and a coating layer. The core layer is composed of a lithium metal oxide material with the composition of Li[Ni a Co b Mn c Al d O2, where a + b + c + d = 1, 0 < a < 1, 0 < b < 1, 0 ≤ c < 1, 0 ≤ d < 1. The coating layer coats the core layer and is composed of a solid electrolyte. The solid electrolyte is formed by reacting a first raw material on the core layer, and the composition of the solid electrolyte is Li3InCl x F y , x + y = 6, 0 < x < 6, 0 < y < 6. The cathode material is formed by heat-treating a precursor, and the precursor is formed by mixing a lithium metal oxide material, a first raw material and a solvent. The first raw material includes lithium, indium, chlorine and fluorine. The weight ratio of the lithium metal oxide material to the solid electrolyte is between 1:0.3 and 1:0.6.
[0008] In one embodiment, 0.9 < a < 1.
[0009] In one embodiment, 4 ≤ x ≤ 5.5, 0.5 ≤ y ≤ 2.
[0010] In one embodiment, the weight ratio of the lithium metal oxide material and the solid electrolyte is between 1:0.4 and 1:0.5.
[0011] In one embodiment, the particles have a particle size, the coating layer has a thickness, and the ratio of the particle size to the thickness is between 6:1 and 40:1.
[0012] In one embodiment, the particle size of the particles is between 5 μm and 20 μm, and the thickness of the coating layer is between 0.5 μm and 3 μm.
[0013] In one embodiment, the first raw material is selected from the group consisting of lithium chloride (LiCl), lithium fluoride (LiF), indium chloride (InCl3), and indium fluoride (InF3).
[0014] In one embodiment, the solvent is a volatile organic solvent
[0015] In one embodiment, the heat treatment is carried out in a vacuum environment or an inert gas atmosphere.
[0016] In one embodiment, the temperature of the heat treatment is between 100 °C and 250 °C.
[0017] To achieve the foregoing object, the present invention further provides a method for preparing a positive electrode material, comprising the steps of: (a) providing a lithium metal oxide material having a composition of Li[Ni a Co b Mn c Al d O2, wherein a + b + c + d = 1, 0.8 < a < 1, 0 < b < 1, 0 ≤ c < 1, 0 ≤ d < 1; (b) mixing the lithium metal oxide material, the first raw material, and the solvent to form a precursor, wherein the first raw material includes lithium, indium, chlorine, and fluorine; and (c) performing a heat treatment on the precursor to form a positive electrode material composed of a plurality of particles. Each of the plurality of particles includes a core layer and a coating layer covering the core layer. The core layer is composed of the lithium metal oxide material, and the coating layer is composed of a solid electrolyte. The solid electrolyte is formed by the reaction of the first raw material on the core layer, and the composition of the solid electrolyte is Li3InCl x F y , x + y = 6, 0 < x < 6, 0 < y < 6. The weight ratio of the lithium metal oxide material and the solid electrolyte is between 1:0.3 and 1:0.6.
[0018] In one embodiment, 0.9 < a < 1.
[0019] In one embodiment, 4 ≤ x ≤ 5.5, 0.5 ≤ y ≤ 2.
[0020] In one embodiment, the weight ratio of the lithium metal oxide material and the solid electrolyte is between 1:0.4 and 1:0.5.
[0021] In one embodiment, the particle has a particle size, the coating layer has a thickness, and the ratio of the particle size to the thickness is between 6:1 and 40:1.
[0022] In one embodiment, the particle size of the particles is between 5 μm and 20 μm, and the thickness of the coating layer is between 0.5 μm and 3 μm.
[0023] In one embodiment, the first raw material is selected from the group consisting of lithium chloride (LiCl), lithium fluoride (LiF), indium chloride (InCl 3 ) and indium fluoride (InF 3 ).
[0024] In one embodiment, the solvent is a volatile organic solvent.
[0025] In one embodiment, the heat treatment is performed in a vacuum environment or an inert gas atmosphere.
[0026] In one embodiment, the temperature of the heat treatment is between 100°C and 250°C. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] Figure 1 It is a schematic structural diagram of a positive electrode material according to an embodiment of the present invention.
[0028] Figure 2 This is a cross-sectional SEM image of a positive electrode material according to an embodiment of the present invention.
[0029] Figure 3 The flowchart is a method for preparing a positive electrode material according to an embodiment of the present invention.
[0030] FIG. 4A to FIG. 4B This is a SEM image of the positive electrode material of the first example of the present invention.
[0031] FIG. 5A to FIG. 5B This is a SEM image of the positive electrode material of the second example of the present invention.
[0032] FIG. 6A to FIG. 6B This is a SEM image of the positive electrode material of the third example of the present invention.
[0033] FIG. 7A to FIG. 7B This is a SEM image of the positive electrode material of the comparative example of the present invention.
[0034] Fig. 8A FIG. 4 is a discharge capacity-cycle number curve diagram of the first exemplary embodiment of the present invention.
[0035] Figure 8B FIG. 4 is a discharge capacity-cycle number curve diagram of the second exemplary embodiment of the present invention.
[0036] Figure 8C FIG. 4 is a discharge capacity-cycle number curve diagram of the third example of the present invention.
[0037] Fig.8D The discharge capacity-cycle number curve of the comparative example of the present invention is shown in FIG.
[0038] Fig. 9A FIG. 4 is a discharge capacity retention rate-cycle number curve diagram of the first exemplary embodiment of the present invention.
[0039] Fig. 9B FIG. 4 is a discharge capacity retention rate-cycle number curve diagram of the second exemplary embodiment of the present invention.
[0040] Fig. 9C FIG. 4 is a discharge capacity retention rate-cycle number curve diagram of the third example of the present invention.
[0041] Fig.9D The figure is a curve of discharge capacity retention rate-cycle number of the comparative example of the present invention. DETAILED DESCRIPTION
[0042] Some typical embodiments that embody the features and advantages of the present invention will be described in detail in the following description. It should be understood that the present invention can have various changes in different aspects, all of which do not depart from the scope of the present invention, and the description and drawings therein are essentially used for illustrative purposes rather than for limiting the present invention. For example, if the following content of the present invention describes that a first feature is set on or above a second feature, it means that it includes an embodiment in which the first feature and the second feature are directly in contact, and also includes an embodiment in which an additional feature can be set between the first feature and the second feature, so that the first feature and the second feature may not be in direct contact. In addition, it is understood that although the terms "first", "second", "third" and the like can be used in the scope of the patent application to describe different components, these components should not be limited by these terms, and the components described in the embodiments are represented by different component symbols. These terms are used to distinguish different components, for example: the first component can be called the second component. Similarly, the second component can also be called the first component without departing from the scope of the embodiment. The term "and / or" in the specification includes any or all combinations of one or more related listed items. The term "approximately" refers to an average value within a standard error range generally accepted by those skilled in the art. Unless otherwise specified in the operation / working examples or otherwise explicitly stated, all numerical ranges, quantities, values and percentages (such as angles, lengths of time, temperatures, operating conditions, quantity ratios, etc.) disclosed in the present invention should be understood to be modified by the term "approximately" or "substantially" in all embodiments. Therefore, unless otherwise specified, the numerical parameters stated in the present invention and the accompanying patent claims are approximate values that can be changed as needed. For example, the number of significant digits of each numerical parameter should be interpreted at least by applying ordinary rounding. The range can be expressed herein as from one endpoint to another or between two endpoints. Unless otherwise specified, all ranges disclosed herein include endpoints.
[0043] Figure 1 It is a schematic structural diagram of a positive electrode material according to an embodiment of the present invention. Figure 2 This is a cross-sectional SEM image of a positive electrode material according to an embodiment of the present invention. Figure 2 The results are obtained by focusing ion beam scanning electron microscopy (FIB-SEM). In this embodiment, the positive electrode material is composed of a plurality of particles 1, and each of the plurality of particles 1 includes a core layer 10 and a coating layer 20. The core layer 10 is composed of Li[Ni a Co b Mn c Al dcomposed of a lithium metal acid material, where a + b + c + d = 1, 0 < a < 1, 0 < b < 1, 0 ≤ c < 1, 0 ≤ d < 1. The coating layer 20 wraps the core layer 10 and is composed of a solid electrolyte. The solid electrolyte composition is formed by the reaction of the first raw material on the core layer 10, and the composition of the solid electrolyte is Li3InCl x F y , and x + y = 6, 0 < x < 6, 0 < y < 6. The positive electrode material is formed by heat-treating the precursor, and the precursor is formed by mixing a lithium metal acid material, the first raw material, and a solvent. The first raw material includes lithium, indium, chlorine, and fluorine. The weight ratio of the lithium metal acid material to the solid electrolyte is between 1:0.3 and 1:0.6. By forming the solid electrolyte with chlorine and fluorine, a positive electrode material with high discharge capacity and high discharge capacity retention rate can be obtained. In this embodiment, the lithium metal acid material is, for example, a lithium nickel cobalt manganese oxide (NCM) material with a composition of Li[Ni a Co b Mn c O2, and a = 0.83, b = 0.12, c = 0.05, that is, the ratio of nickel, cobalt, and manganese in the lithium nickel cobalt manganese oxide material is 83:12:5. Preferably, the lithium nickel cobalt manganese oxide material is prepared, for example, by a solid-state synthesis method. In other embodiments, the lithium metal acid material can also be, for example, a lithium nickel cobalt manganese oxide (NCM) material with a different composition ratio, a lithium nickel cobalt aluminate (NCA) material with a composition of Li[Ni a Co b Al d O2 or a lithium nickel cobalt manganese aluminate (NCMA) material with a composition of Li[Ni a Co b Mn c Al d O2, and can be prepared, for example, by a sol-gel process. In a preferred embodiment, the composition of the lithium metal acid material is Li[Ni a Co b Mn c Al d O2, and the value range of the coefficient a is, for example, 0.9 < a < 1, that is, the molar ratio of cobalt among the metal elements other than lithium in the lithium metal acid material is greater than 90%. For example, a composition of Li[Ni a Co b Mn c Al d]O2 nickel cobalt manganese aluminum oxide (NCMA) material, and a = 0.93, b = 0.03, c = 0.03, d = 0.01, that is, the ratio of nickel, cobalt, manganese and aluminum in the nickel cobalt manganese aluminum oxide material is 93:3:3:1. Through the high nickel content in the core layer 10, a high energy density and low-cost positive electrode material is achieved. It should be noted that the type, composition ratio, and process of the metal acid lithium material of the present invention are not limited to this and will not be repeated.
[0044] In this embodiment, the composition of the solid electrolyte is Li3InCl x F y The range of the coefficients x and y is, for example, 4≤x≤5.5, 0.5≤y≤2, that is, the ratio of chlorine to fluorine is between 5.5:0.5 and 4:2. By controlling the composition ratio of chlorine and fluorine in the solid electrolyte, the electrical performance of the positive electrode material can be improved. Preferably, the ratio of chlorine to fluorine is, for example, between 5.3:0.7 and 4.5:1.5, but the present invention is not limited thereto.
[0045] In a preferred embodiment, the weight ratio of the lithium metal oxide material to the solid electrolyte is between 1:0.4 and 1:0.5 to form a positive electrode material with a uniform core-shell structure. Figure 2 As shown, the particle 1 of the positive electrode material has a particle size T1, the coating layer 20 has a thickness T2, and the ratio of the particle size T1 to the thickness T2 is between 6:1 and 40:1. The particle size T1 of the particle 1 is between 5 μm and 20 μm. The thickness T2 of the coating layer 20 is between 0.5 μm and 3 μm.
[0046] In this embodiment, the first raw material is selected from the group consisting of lithium chloride (LiCl), lithium fluoride (LiF), indium chloride (InCl3), and indium fluoride (InF3), and the solvent is a volatile organic solvent. Compared with dry mixing, wet mixing with an organic solvent is low in cost and easy to control, and can further eliminate the negative impact of moisture while improving the solid dispersion during the fabrication of the electrode. Furthermore, through wet mixing, the first raw material can directly react on the surface of the lithium metal oxide material particles to achieve in-situ synthesis, thereby forming a cathode material with a uniform core-shell structure and improving the electrical performance. The first raw material includes, for example, lithium chloride (LiCl), lithium fluoride (LiF), and indium chloride (InCl3), and the molar ratio of lithium, indium, and halogen elements (the sum of chlorine and fluorine) in the first raw material is 3:1:6. In this embodiment, the volatile organic solvent is, for example, ethanol. Of course, other volatile organic solvents that do not react with the lithium metal oxide material and the first raw material are also applicable and will not be elaborated herein. In this embodiment, the precursor is formed by mixing the lithium metal oxide material, the first raw material, a conductive agent, a binder, and a solvent together and reacting in a vacuum environment or an inert gas atmosphere. The conductive agent is, for example, carbon nanotubes, conductive graphite, conductive carbon black, acetylene black, or vapor grown carbon fiber (VGCF), etc., and the binder is, for example, polyvinylidene difluoride (PVDF) or polytetrafluoroethene (PTFE), etc. The vacuum environment is, for example, a vacuum reaction flask with a pressure less than or equal to 10 -3 torr. The inert gas atmosphere is, for example, an argon atmosphere or a nitrogen atmosphere, and the present invention is not limited thereto.
[0047] According to the foregoing cathode material, the present invention further provides a method for preparing a cathode material. Figure 3 The flowchart of the method for preparing the cathode material according to an embodiment of the present invention is shown. First, as shown in step S1, a lithium metal oxide material having a composition of Li[Ni a Co b Mn c Al d O2 is provided, where a + b + c + d = 1, 0 < a < 1, 0 < b < 1, 0 ≤ c < 1, 0 ≤ d < 1. In this embodiment, the lithium metal oxide material is, for example, a composition of Li[Ni a Co b Mn cLithium nickel cobalt manganese oxide (NCM) material with O2, where a = 0.83, b = 0.12, c = 0.05, that is, the ratio of nickel, cobalt, and manganese in the lithium nickel cobalt manganese oxide material is 83:12:5. Preferably, the lithium nickel cobalt manganese oxide material is obtained, for example, by solid-state synthesis. In other embodiments, the lithium metal oxide material can also be, for example, a lithium nickel cobalt manganese oxide (NCM) material with different composition ratios, or a lithium nickel cobalt aluminate (NCA) material with the composition Li[Ni a Co b Al d O2 or a lithium nickel cobalt manganese aluminate (NCMA) material with the composition Li[Ni a Co b Mn c Al d O2, and can be obtained, for example, by a sol-gel process. In a preferred embodiment, the composition of the lithium metal oxide material is Li[Ni a Co b Mn c Al d O2, and the numerical range of the coefficient a is, for example, 0.9 < a < 1, that is, the molar ratio of cobalt among the metal elements other than lithium in the lithium metal oxide material is greater than 90%. For example, a lithium nickel cobalt manganese aluminate (NCMA) material with the composition Li[Ni a Co b Mn c Al d O2, where a = 0.93, b = 0.03, c = 0.03, d = 0.01, that is, the ratio of nickel, cobalt, manganese, and aluminum in the lithium nickel cobalt manganese aluminate material is 93:3:3:1. Through the high nickel content in the core layer 10, a cathode material with high energy density and low cost is achieved. It should be noted that the type, composition ratio, and manufacturing process of the lithium metal oxide material of the present invention are not limited to this, and will not be elaborated further. Through the high nickel content in the core layer 10, a cathode material with high energy density and low cost is achieved.
[0048] Furthermore, as shown in step S2, a metal acid lithium material, a first raw material and a solvent are mixed to form a precursor. The first raw material includes lithium, indium, chlorine and fluorine. The first raw material is selected from the group consisting of lithium chloride (LiCl), lithium fluoride (LiF), indium chloride (InCl3) and indium fluoride (InF3), and the solvent is a volatile organic solvent. Compared with dry mixing, wet mixing with an organic solvent is low in cost and easy to control, and can also improve the solid dispersion when making an electrode while eliminating the negative impact of moisture. Furthermore, through wet mixing, the first raw material can directly react on the surface of the metal acid lithium material particles to achieve in situ synthesis (In situ synthesis), thereby forming a positive electrode material with a uniform core-shell structure and improving electrical performance. In this embodiment, the weight ratio of the metal acid lithium material and the first raw material is, for example, between 1:0.3 and 1:0.6, preferably between 1:0.4 and 1:0.5. The first raw material includes, for example, lithium chloride (LiCl), lithium fluoride (LiF) and indium chloride (InCl3), and the molar ratio of lithium, indium and halogen elements (the sum of chlorine and fluorine) in the first raw material is 3:1:6. In the present embodiment, the volatile organic solvent is, for example, ethanol. Of course, other volatile organic solvents that do not react with the metal acid lithium material and the first raw material are also applicable, and are not described in detail here. In the present embodiment, the precursor is, for example, a mixture of metal acid lithium material, the first raw material, a conductive agent, a binder and a solvent, and reacts in a vacuum environment or an inert gas atmosphere to form. The conductive agent is, for example, carbon nanotubes, conductive graphite, conductive carbon black, acetylene black or vapor-grown carbon fiber (Vaporgrown carbon fiber, VGCF), etc., and the binder is, for example, polyvinylidene difluoride (PVDF) or polytetrafluoroethylene (PTFE), etc. A vacuum environment is, for example, a pressure less than or equal to 10 -3 The inert gas atmosphere is, for example, an argon atmosphere or a nitrogen atmosphere, but the present invention is not limited thereto.
[0049] Finally, as shown in step S3, the precursor is heat treated to form a positive electrode material composed of a plurality of particles 1. Each of the plurality of particles 1 includes a core layer 10 and a coating layer 20 that covers the core layer 10. The core layer 10 is composed of a lithium metal oxide material, and the coating layer 20 is composed of a solid electrolyte. The solid electrolyte assembly is formed by reacting a first raw material on the core layer 10, and the composition of the solid electrolyte is Li3InCl x F y, x + y = 6, 0 < x < 6, 0 < y < 6. The weight ratio of the lithium metal oxide material to the solid electrolyte is between 1:0.3 and 1:0.6. In this embodiment, the heat treatment is carried out in a vacuum environment or an inert gas atmosphere. The vacuum environment is, for example, a vacuum reaction flask with a pressure less than or equal to 10 -3 torr. The inert gas atmosphere is, for example, an argon atmosphere or a nitrogen atmosphere. The heat treatment temperature is between 100°C and 250°C, preferably between 160°C and 200°C, so that the energy consumption of the preparation method of the present invention is low, the manufacturing cost is saved and it has environmental benefits. In this embodiment, the precursor is, for example, uniformly coated on a metal foil for heat treatment, and then cut to form a positive electrode sheet.
[0050] In this embodiment, the composition of the solid electrolyte is Li3InCl x F y In the formula, the ranges of the coefficients x and y are, for example, 4 ≤ x ≤ 5.5, 0.5 ≤ y ≤ 2, that is, the ratio of chlorine to fluorine is between 5.5:0.5 and 4:2. By controlling the composition ratio of chlorine and fluorine in the solid electrolyte, the electrical performance of the positive electrode material can be improved. Preferably, the ratio of chlorine to fluorine is more, for example, between 5.3:0.7 and 4.5:1.5, but the present invention is not limited thereto. In a preferred embodiment, the weight ratio of the lithium metal oxide material to the solid electrolyte is between 1:0.4 and 1:0.5 to form a positive electrode material with a uniform core-shell structure. The particle 1 of the positive electrode material has a particle size T1, the coating layer 20 has a thickness T2, and the ratio of the particle size T1 to the thickness T2 is between 6:1 and 40:1. The particle size T1 of the particle 1 is between 5 μm and 20 μm. The thickness T2 of the coating layer 20 is between 0.5 μm and 3 μm.
[0051] The following details the process and efficacy of the present invention through comparative examples and demonstration examples.
[0052] First demonstration example:
[0053] The first demonstration example is a positive electrode material prepared in the following manner. First, a lithium metal oxide material is provided. The composition of the lithium metal oxide material is Li[Ni a Co b Mn c Al d O2, and a = 0.82, b = 0.13, c = 0.05. In other words, the lithium metal oxide material is a lithium nickel cobalt manganese oxide material with a molar ratio of nickel, cobalt, and manganese of 82:13:5.
[0054] Furthermore, 0.68 g of lithium metal oxide material, 0.3 g of the first raw material, 0.02 g of vapor grown carbon fiber (VGCF) and 0.01 g of polytetrafluoroethene (PTFE) were added to 3 ml of alcohol and ground at 120° C. to mix the materials evenly to form a precursor. The first raw material of the first example includes 0.083 g of lithium chloride (LiCl), 0.0189 g of lithium fluoride (LiF) and 0.199 g of indium chloride (InCl3), that is, the molar ratio of lithium, indium, chlorine and fluorine in the first raw material is about 3:1:5.19:0.81.
[0055] Finally, the precursor is heat-treated to form the positive electrode material. The heat treatment is performed in an argon atmosphere at a temperature of 180° C. for 2 hours.
[0056] Second example:
[0057] The preparation method of the second example is substantially the same as that of the first example, except that the first raw material of the second example includes 0.068 g of lithium chloride (LiCl), 0.029 g of lithium fluoride (LiF) and 0.203 g of indium chloride (InCl3), that is, the molar ratio of lithium, indium, chlorine and fluorine in the first raw material is approximately 3:1:4.77:1.23.
[0058] The third example:
[0059] The preparation method of the third example is substantially the same as that of the first example, except that the first raw material of the third example includes 0.053 g of lithium chloride (LiCl), 0.04 g of lithium fluoride (LiF) and 0.207 g of indium chloride (InCl3), that is, the molar ratio of lithium, indium, chlorine and fluorine in the first raw material is approximately 3:1:4.35:1.65.
[0060] Comparative Example:
[0061] The preparation method of the comparative example is substantially the same as the preparation method of the first exemplary embodiment, except that the first raw material of the comparative example only includes 0.11 g of lithium chloride (LiCl) and 0.19 g of indium chloride (InCl3), that is, the first raw material does not include fluorine, and the molar ratio of lithium, indium and chlorine is approximately 3:1:6.
[0062] FIG. 4A to FIG. 4B This is a SEM image of the positive electrode material of the first example of the present invention. FIG. 5A to FIG. 5B This is a SEM image of the positive electrode material of the second example of the present invention. FIG. 6A to FIG. 6B This is a SEM image of the positive electrode material of the third example of the present invention. FIG. 7A to FIG. 7B This is a SEM image of the positive electrode material of the comparative example of the present invention. FIG. 8A to FIG. 8D The following is a discharge capacity-cycle number curve obtained by testing the button batteries prepared in the first example, the second example, the third example and the comparative example. Table 1 below shows the discharge capacity of the button batteries prepared in the first example, the second example, the third example and the comparative example at the 1st cycle and the 45th cycle. The positive electrode of the button battery is the positive electrode material of the first example, the second example, the third example and the comparative example, and the negative electrode is lithium metal. The voltage window is 2.5V to 4.4V, the charge and discharge rate (C-rate) is 0.1C, and it is charged in a constant current (CC) mode and discharged in a constant current constant voltage (CCCV) mode. The constant current constant voltage discharge method is to maintain the current constant during the discharge process, and then maintain the voltage constant until the discharge is completed after reaching the upper limit voltage. The temperature condition of the charge and discharge test is 55°C. FIG. 8A to FIG. 8D As shown in Table 1, at the first cycle, the discharge capacity of the second example with a chlorine:fluorine ratio of 4.77:1.23 was 196.18 mAh / g, slightly higher than the discharge capacity of the comparative example, while the discharge capacity of the first example with a chlorine:fluorine ratio of 5.19:0.81 was 189.49 mAh / g, slightly lower than the discharge capacity of the comparative example, but the difference was not obvious. At the 45th cycle, the discharge capacity of the first example was 160.21 mAh / g, which was 8.31% higher than the discharge capacity of the comparative example of 147.91 mAh / g; the discharge capacity of the second example was 166.90 mAh / g, which was 12.83% higher than the discharge capacity of the comparative example of 147.91 mAh / g. It can be seen that the use of a solid electrolyte composed of chlorine and fluorine can significantly improve the discharge capacity of the positive electrode material, and the solid electrolyte with a chlorine:fluorine ratio between 5.3:0.7 and 4.5:1.5 has a better effect.
[0063] Table 1
[0064]
[0065] 9A to 9D The following table 2 shows the discharge capacity retention rate-cycle number curves obtained by testing the button batteries made in the first example, the second example, the third example and the comparative example. The following table 2 shows the discharge capacity retention rate of the button batteries made in the first example, the second example, the third example and the comparative example at the 45th cycle. 9A to 9DAs shown in Table 2, at the 45th cycle, the discharge capacity retention rate of the first exemplary embodiment is 84.55%, showing a 10.31% increase compared to the 76.65% of the comparative example; the discharge capacity retention rate of the second exemplary embodiment is 85.07%, showing a 10.98% increase compared to the 76.65% of the comparative example; the discharge capacity retention rate of the third exemplary embodiment is 78.44%, showing a 2.34% increase compared to the 76.65% of the comparative example. It can be seen that using a solid electrolyte composed of chlorine and fluorine together can significantly improve the discharge capacity retention rate of the cathode material, and the solid electrolyte with the chlorine and fluorine ratio between 5.3:0.7 and 4.5:1.5 has better effects.
[0066] Table 2
[0067] Discharge capacity retention rate at the 45th cycle First example 84.55% Second example 85.07% The third example 78.44% Comparative Example 76.65%
[0068] In summary, the present invention provides a cathode material prepared through an organic solvent and having a solid electrolyte coating layer and a preparation method thereof to improve electrical performance. The cathode material is composed of a plurality of particles, and each particle includes a core layer and a coating layer covering the core layer. The core layer is composed of a lithium metal oxide material with the composition of Li[Ni a Co b Mn c Al d O2, and 0.8 < x < 1. Through the high nickel content in the core layer, a cathode material with high energy density and low cost is achieved. The coating layer is composed of a solid electrolyte including lithium, indium, chlorine, and fluorine. By using chlorine and fluorine to form the solid electrolyte, a cathode material with high discharge capacity and high discharge capacity retention rate can be obtained. The composition of the solid electrolyte is, for example, Li3InCl x F y , and 4 ≤ x ≤ 5.5, 0.5 ≤ y ≤ 2. By controlling the composition ratio of chlorine and fluorine in the solid electrolyte, the aforementioned electrical performance can be further improved. The weight ratio of the lithium metal oxide material of the core layer to the solid electrolyte of the coating layer is more, for example, between 1:0.3 and 1:0.6 to form a cathode material with a uniform core-shell structure. The preparation method of the cathode material is to use a composition of Li[Ni a Co b Mn c Al d]O2 lithium metal oxide material, a first raw material including lithium, indium, chlorine and fluorine are mixed in an organic solvent, and then heat treated to form a positive electrode material. Compared with dry mixing, wet mixing with an organic solvent is low-cost and easy to control, and can improve the solid dispersion when making electrodes while eliminating the negative effects of moisture. Furthermore, through wet mixing, the first raw material can directly react on the surface of the lithium metal oxide material particles to achieve in situ synthesis (In situssynthesis), thereby forming a positive electrode material with a uniform core-shell structure and improving electrical performance. The temperature of the heat treatment is, for example, between 100°C and 250°C, with low energy consumption, saving manufacturing costs and environmental benefits.
[0069] The present invention may be modified in various ways by those skilled in the art, but all modifications are within the scope of the attached patent application.
[0070]
Explanation of symbols
[0071] 1: Particles
[0072] 10: Core layer
[0073] 20: Cladding layer
[0074] S1, S2, S3: Steps
[0075] T1: Particle size
[0076] T2: Thickness
Claims
1. A positive electrode material, comprising a plurality of particles, wherein each of the plurality of particles comprises: A core layer, composed of a metal acid lithium material, wherein the composition of the metal acid lithium material is Li[Ni a Co b Mn c Al d ]O2, and a+b+c+d=1,0.8 <a<1,0<b<1,0≤c<1,0≤d<1; as well as A cladding layer coats the core layer, wherein the cladding layer is composed of a solid electrolyte, and the solid electrolyte is formed by reacting a first raw material on the core layer, and the composition of the solid electrolyte is Li3InCl x F y , x + y = 6, 0 < x < 6, 0 < y < 6, wherein the positive electrode material is formed by performing a heat treatment on a precursor, and the precursor is formed by mixing the lithium metal oxide material, the first raw material, and a solvent, wherein the first raw material includes lithium, indium, chlorine, and fluorine, and the weight ratio of the lithium metal oxide material to the solid electrolyte is between 1:0.3 and 1:0.
6.
2. The positive electrode material as claimed in claim 1, wherein 0.9 <a<1。 3. The positive electrode material as claimed in claim 1, wherein 4≤x≤5.5, 0.5≤y≤2.
4. The positive electrode material as claimed in claim 1, wherein the weight ratio of the lithium metal oxide material to the solid electrolyte is between 1:0.4 and 1:0.
5. 5 . The positive electrode material as claimed in claim 1 , wherein the particle has a particle size, the coating layer has a thickness, and a ratio of the particle size to the thickness is between 6:1 and 40:
1. 6 . The positive electrode material as claimed in claim 5 , wherein the particle size of the particle is between 5 μm and 20 μm, and the thickness of the coating layer is between 0.5 μm and 3 μm.
7. The positive electrode material as claimed in claim 1, wherein the first raw material is selected from the group consisting of lithium chloride (LiCl), lithium fluoride (LiF), indium chloride (InCl3) and indium fluoride (InF3). The positive electrode material as claimed in claim 1 , wherein the solvent is a volatile organic solvent.
9. The positive electrode material as claimed in claim 1, wherein the heat treatment is performed in a vacuum environment or an inert gas atmosphere.
10. The positive electrode material as claimed in claim 1, wherein the temperature of the heat treatment is between 100°C and 250°C.
11. A method for preparing a positive electrode material, comprising the steps of: (a) providing a lithium metal oxide material, wherein the composition of the lithium metal oxide material is Li[Ni a Co b Mn c Al d ]O2, and a+b+c+d=1,0.8 <a<1,0<b<1,0≤c<1,0≤d<1; (b) mixing the lithium metal oxide material, a first raw material and a solvent to form a precursor, wherein the first raw material includes lithium, indium, chlorine and fluorine; and (c) Perform a heat treatment on the precursor to form the cathode material composed of a plurality of particles, wherein each of the plurality of particles includes a core layer and a coating layer coating the core layer. The core layer is composed of the lithium metal acid material, and the coating layer is composed of a solid electrolyte. The solid electrolyte is formed by the reaction of the first raw material on the core layer, and the composition of the solid electrolyte is Li3InCl x F y , x + y = 6, 0 < x < 6, 0 < y < 6, wherein the weight ratio of the lithium metal acid material to the solid electrolyte is between 1:0.3 and 1:0.
6.
12. The method for preparing the positive electrode material according to claim 11, wherein 0.9 <a<1。 13. The method for preparing a positive electrode material as claimed in claim 11, wherein 4≤x≤5.5, 0.5≤y≤2. 14 . The method for preparing the positive electrode material as claimed in claim 11 , wherein the weight ratio of the lithium metal oxide material to the solid electrolyte is between 1:0.4 and 1:0.
5. 15 . The method for preparing a positive electrode material as claimed in claim 11 , wherein the particle has a particle size, the coating layer has a thickness, and a ratio of the particle size to the thickness is between 6:1 and 40:
1. 16 . The method for preparing the positive electrode material as claimed in claim 15 , wherein the particle size of the particle is between 5 μm and 20 μm, and the thickness of the coating layer is between 0.5 μm and 3 μm.
17. The method for preparing a positive electrode material as claimed in claim 11, wherein the first raw material is selected from the group consisting of lithium chloride (LiCl), lithium fluoride (LiF), indium chloride (InCl3) and indium fluoride (InF3).
18. The method for preparing a positive electrode material as claimed in claim 11, wherein the solvent is a volatile organic solvent.
19. The method for preparing a positive electrode material as claimed in claim 11, wherein the heat treatment is performed in a vacuum environment or an inert gas atmosphere.
20. The method for preparing the positive electrode material as claimed in claim 11, wherein the temperature of the heat treatment is between 100°C and 250°C.