Carbon nanofiber encapsulated sodium alum phosphate flexible self-supporting electrode material and preparation method and application thereof

The carbon nanofiber-encapsulated sodium vanadium phosphate electrode addresses the conductivity and flexibility issues of NVP electrodes by forming a three-dimensional network, enhancing electronic conductivity and flexibility, thus improving sodium ion battery energy density and performance.

CN119069670APending Publication Date: 2024-12-03HUBEI WANRUN NEW ENERGY TECH CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411189516.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-27
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

Sodium vanadium phosphate (NVP) electrodes in sodium-ion batteries suffer from poor electronic conductivity and flexibility, limiting their rate performance and commercialization due to the need for traditional additives and current collectors, which reduce the active material proportion and energy density.

Method used

A carbon nanofiber-encapsulated sodium vanadium phosphate flexible self-supporting electrode material is created by coating sodium vanadium phosphate particles on polyacrylonitrile carbonized nanofibers, forming a three-dimensional network structure through staggered overlapping, enhancing electronic conductivity and flexibility.

Benefits of technology

The electrode material achieves high electronic conductivity and flexibility, increasing the proportion of active materials and energy density without relying on current collectors, resulting in a sodium ion battery with good wearability and charge/discharge performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119069670A_ABST
    Figure CN119069670A_ABST
Patent Text Reader

Abstract

The invention provides a carbon nanofiber encapsulated sodium vanadium phosphate flexible self-supporting electrode material and a preparation method and application thereof, and belongs to the field of sodium batteries, the carbon nanofiber encapsulated sodium vanadium phosphate flexible self-supporting electrode material comprises a plurality of polyacrylonitrile carbonized nanofibers in staggered lap joint, sodium alum phosphate particles are coated in the polyacrylonitrile carbonized nanofibers. According to the preparation method, the prepared carbon nanofiber packaged sodium vanadium phosphate flexible self-supporting electrode material is high in electronic conductivity, and the energy density of a battery prepared from the carbon nanofiber packaged sodium vanadium phosphate flexible self-supporting electrode material can be effectively improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of sodium ion batteries, and in particular to a carbon nanofiber-encapsulated sodium alum phosphate flexible self-supporting electrode material, and a preparation method and application thereof. Background Art

[0002] Currently, lithium-ion batteries (LIBs) have dominated the fields of portable devices and electric vehicles, but due to the uneven geographical distribution of lithium resources and the continuous rise in prices, lithium-ion batteries cannot meet the energy storage requirements of grid scale. Therefore, people are in urgent need of developing new energy storage batteries that can replace lithium-ion batteries. Sodium-ion batteries have become a potential substitute for lithium-ion batteries due to their abundant resources and low cost, especially in large-scale energy storage scenarios. In addition, sodium-ion batteries have similar working principles to lithium-ion batteries, which has attracted widespread attention.

[0003] Since the radius of sodium ions is larger than that of lithium ions, the diffusion kinetics of sodium ions are relatively slow. In order to design high-performance sodium-ion batteries, it is extremely important to choose suitable electrode materials. Sodium superion conductor (NASICON) materials have a well-opened three-dimensional structure, which is suitable for the rapid migration of sodium ions and stands out among many sodium-ion battery positive electrode materials. In the NASICON series, sodium vanadium phosphate (NVP), with the chemical formula Na3V2(PO4)3, shows good advantages in sodium-ion battery positive electrode materials due to its stable structure and large capacity. However, due to the inherent disadvantage of poor electronic conductivity, the rate performance of NVP is not ideal, which hinders the further development of the commercialization of sodium-ion batteries.

[0004] At present, common modification methods for NVP include ion doping, improved conductive agents, carbon coatings, and nano-crystallization, which can provide a fast diffusion path for ions, and are also conducive to improving the conduction path of electrons, thereby improving the rate performance and cycle performance of electrode materials. However, most NVP prepared by existing methods are in the form of granular blocks, and need to be prepared into electrodes with various traditional additives and current collectors, resulting in a low proportion of active electrode materials, low electronic conductivity, and thus too low energy density of the prepared battery. At the same time, the NVP prepared by existing methods has poor flexibility and does not have wearable properties. Summary of the invention

[0005] In view of the technical problems existing in the background technology, the present application provides a carbon nanofiber encapsulated sodium vanadium phosphate flexible self-supporting electrode and its preparation method and application, aiming to solve the problem of how to improve the electronic conductivity and flexibility of the sodium vanadium phosphate electrode material.

[0006] In a first aspect, an embodiment of the present application provides a carbon nanofiber-encapsulated sodium aluminate phosphate flexible self-supporting electrode material, which includes a plurality of staggered overlapping polyacrylonitrile carbonized nanofibers, and the polyacrylonitrile carbonized nanofibers are coated with sodium aluminate phosphate particles.

[0007] In the technical solution of the embodiment of the present application, polyacrylonitrile (PAN) can be used to adsorb VO 2+ , sodium vanadium phosphate (NVP) is uniformly coated on polyacrylonitrile carbonized nanofibers to form a composite material of NVP and carbon nanofibers (NVP@CNF), and NVP@CNF is formed into a three-dimensional network structure by staggered overlapping, that is, a flexible self-supporting electrode material of carbon nanofiber-encapsulated sodium vanadium phosphate is obtained, which can promote the embedding of sodium ions into the cross-linked electrode material of NVP fibers. At the same time, since the polyacrylonitrile carbonized nanofiber coating layer is conductive, it is beneficial to improve the electronic conductivity of the material; on the other hand, the carbonized polyacrylonitrile fibers have good flexibility, which improves the flexibility of the material, and finally a flexible self-supporting electrode material with good flexibility and high electronic conductivity is obtained.

[0008] In some embodiments, the polyacrylonitrile carbon nanofibers include a coated region coated with sodium vanadium phosphate particles and an uncoated region not coated with sodium vanadium phosphate particles, wherein the cross-sectional diameter of the uncoated region is 300-500 nm, and the cross-sectional diameter of the coated region is 400-600 nm.

[0009] In this embodiment, in the coating area, the cross-sectional diameter of the sodium aluminate phosphate particles is matched with the cross-sectional diameter of the polyacrylonitrile carbonized nanofibers to achieve the coating of the sodium aluminate phosphate particles within the polyacrylonitrile carbonized nanofibers, and the carbon layer is not too thick. If the cross-sectional diameter of the coating area is too large and the cross-sectional diameter of the uncoated area is too small, the sodium aluminate phosphate particles are easy to leak and good coating cannot be achieved, resulting in reduced material flexibility and low electronic conductivity. If the cross-sectional diameter of the coating area is too small and the cross-sectional diameter of the uncoated area is too large, the carbonized nanofiber layer is too thick, resulting in reduced electronic conductivity.

[0010] In a second aspect, the present invention provides a method for preparing a flexible self-supporting electrode material of sodium aluminate phosphate encapsulated by carbon nanofibers, comprising the following steps:

[0011] preparing a precursor solution containing sodium vanadium phosphate particles and polyacrylonitrile;

[0012] Electrospinning the spinning precursor solution to obtain a precursor film;

[0013] The precursor film is sequentially dried, pre-sintered and secondary-sintered to obtain a flexible self-supporting electrode material of carbon nanofiber-encapsulated sodium alum phosphate.

[0014] In the technical solution of the embodiment of the present application, the polyacrylonitrile solution has high viscosity and can absorb VO 2+ , so that sodium vanadium phosphate is evenly dispersed in the polyacrylonitrile solution, and then the NVP is encapsulated in the polyacrylonitrile carbonized fiber through electrospinning and heat treatment to obtain an electrode material with high electronic conductivity and good flexibility.

[0015] In some embodiments, the step of preparing a precursor solution containing sodium vanadium phosphate particles and polyacrylonitrile comprises:

[0016] dissolving polyacrylonitrile in a first solvent to obtain a polyacrylonitrile solution;

[0017] A vanadium source, a sodium source, a phosphorus source, a reducing agent, a carbon source and a second solvent are mixed and stirred to obtain a black gel;

[0018] The black gel is calcined and ground to obtain sodium sulfate phosphate precursor particles;

[0019] Dispersing sodium vanadium phosphate precursor particles into a polyacrylonitrile solution to obtain a precursor solution containing sodium vanadium phosphate particles and polyacrylonitrile;

[0020] The first solvent includes at least one of dimethylformamide and N-methylpyrrolidone, and the second solvent includes at least one of deionized water, anhydrous ethanol, acetic acid, and tetrahydrofuran.

[0021] In this embodiment, the process of first preparing black gel and then calcining to obtain sodium alum phosphate precursor particles is simple, the particle size is controllable, and the sodium alum phosphate precursor particles can be evenly dispersed in the polyacrylonitrile solution.

[0022] In some embodiments, in the precursor mixed solution, the mass ratio of sodium vanadium phosphate particles to polyacrylonitrile is 1:(0.5-1.5).

[0023] In this embodiment, if too much sodium alum phosphate particles are added, agglomeration will occur, and if too little sodium alum phosphate particles are added, it will be unfavorable to improve the electronic conductivity.

[0024] In some embodiments, the drying temperature is 60-100°C and the drying time is 8-24h; and / or the pre-sintering temperature is 200-220°C and the pre-sintering heating rate is 0.5-0.6°C min -1 ; and / or, the secondary sintering temperature is 500-800°C, and the secondary sintering time is 1-15h.

[0025] In this embodiment, drying is performed within a limited range to remove the solvent. If the temperature is too high, energy is wasted, and if the temperature is too low, the solvent evaporation time is too long. In air, the purpose of pre-sintering is pre-oxidation treatment and solidification spinning, which can avoid structural collapse and increase oxygen-containing functional groups. In an inert atmosphere, the purpose of secondary sintering is annealing to synthesize sodium vanadium phosphate@polyacrylonitrile carbonized nanofiber composite materials.

[0026] In some embodiments, the calcination temperature is 300-350°C, and the calcination heating rate is 5-6°C min -1 .

[0027] In this embodiment, the water in the gel-like mixture is removed by calcination. Under the calcination conditions of the present application, the particle size of the sodium alum phosphate can be controlled at 400-600nm, and then the sodium alum phosphate particles are loosened by grinding to facilitate subsequent dispersion in the polyacrylonitrile solution. If the calcination temperature is too high, the particle size of the sodium alum phosphate particles increases, which is not conducive to electron transmission. If the calcination temperature is too low, the purity of the sodium alum phosphate particles is reduced.

[0028] In some embodiments, the molar ratio of the vanadium source to the reducing agent is 1:(1-4); and / or, the molar ratio of the vanadium source to the carbon source is (0.05-5):1; and / or, the molar ratio of the vanadium source to the sodium source is 2:(3-5), and the molar ratio of the vanadium source to the phosphorus source is 2:(3-5).

[0029] In this embodiment, within the specified range, the obtained product is sodium vanadium phosphate. If it exceeds the above specified range, the obtained sodium vanadium phosphate has a high impurity content.

[0030] In some embodiments, the vanadium source includes one or more of vanadium pentoxide, ammonium metavanadate, vanadium dioxide, and sodium metavanadate; and / or, the sodium source includes one or more of sodium oxalate, disodium hydrogen phosphate, sodium carbonate, sodium bicarbonate, sodium hydroxide, and sodium citrate; and / or, the phosphorus source includes one or more of diammonium hydrogen phosphate, ammonium dihydrogen phosphate, diammonium phosphate, and phosphoric acid; and / or, the reducing agent is one or more of citric acid, oxalic acid, oxalic acid, malonic acid, and ascorbic acid; and / or, the carbon source includes at least one of citric acid, sucrose, and glucose.

[0031] In this embodiment, the synthesis reaction of sodium sulfate phosphate is finally achieved under stirring conditions by combining the raw materials.

[0032] In a third aspect, an embodiment of the present application provides a positive electrode plate, comprising the aforementioned carbon nanofiber-encapsulated sodium vanadium phosphate flexible self-supporting electrode material, or comprising the carbon nanofiber-encapsulated sodium vanadium phosphate flexible self-supporting electrode material prepared by the aforementioned preparation method.

[0033] In this embodiment, the positive electrode plate includes the aforementioned carbon nanofiber-encapsulated sodium vanadium phosphate flexible self-supporting electrode material, thereby having the advantages of high electronic conductivity and good flexibility brought by the material.

[0034] In a fourth aspect, an embodiment of the present application provides a sodium ion battery, comprising the aforementioned positive electrode plate.

[0035] In this embodiment, the sodium ion battery includes the aforementioned positive electrode plate, and thus has the advantage of high energy density.

[0036] The beneficial effects of this application are as follows:

[0037] The carbon nanofiber encapsulated sodium alum phosphate flexible self-supporting electrode material of the present application combines the advantages of carbon nanofiber encapsulation and flexible self-support. On the one hand, its conductivity is increased and the electrochemical properties of the electrode material are improved. On the other hand, the prepared electrode does not need to rely on current collectors, binders and additional conductive agents, which greatly increases the proportion of electrode active materials. The material has good electrical conductivity, high electronic conductivity and good flexibility.

[0038] Therefore, the sodium ion battery prepared by using the flexible self-supporting electrode material of sodium alum phosphate encapsulated by carbon nanofibers in the present application not only has good wearability, but also has high energy density and good charge and discharge performance.

[0039] The above description is only an overview of the technical solution of the present application. In order to more clearly understand the technical means of the present application, it can be implemented in accordance with the contents of the specification. In order to make the above and other purposes, features and advantages of the present application more obvious and easy to understand, the specific implementation methods of the present application are listed below. BRIEF DESCRIPTION OF THE DRAWINGS

[0040] In order to more clearly illustrate the technical solution of the present application, the following is a brief introduction to the drawings used in the present application. Obviously, the drawings described below are only some embodiments of the present application, and for ordinary technicians in this field, other drawings can be obtained based on these drawings without creative work.

[0041] Figure 1 A schematic diagram of the process for preparing the flexible self-supporting electrode material of sodium vanadium phosphate encapsulated by carbon nanofibers of the present application;

[0042] Figure 2 This is a SEM image of the carbon nanofiber encapsulated sodium vanadium phosphate flexible self-supporting electrode material prepared in Example 2;

[0043] Figure 3 This is a SEM image of the sodium vanadium phosphate positive electrode material prepared in Comparative Example 1;

[0044] Figure 4The XRD patterns of the materials obtained in Example 2 and Comparative Example 1 are shown in FIG.

[0045] Figure 5 This is a high-resolution TEM image of the carbon nanofiber-encapsulated sodium vanadium phosphate flexible self-supporting electrode material prepared in Example 2;

[0046] Figure 6 This is a performance diagram of the charge and discharge curves of a sodium ion battery assembled with the carbon nanofiber-encapsulated sodium vanadium phosphate flexible self-supporting electrode material prepared in Example 2 at different rates. DETAILED DESCRIPTION

[0047] The following embodiments of the technical solution of the present application are described in detail in conjunction with the accompanying drawings. The following embodiments are only used to more clearly illustrate the technical solution of the present application, and are therefore only used as examples, and cannot be used to limit the scope of protection of the present application.

[0048] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by technicians in the technical field to which this application belongs; the terms used herein are only for the purpose of describing specific embodiments and are not intended to limit this application; the terms "including" and "having" in the specification and claims of this application and the above-mentioned figure descriptions and any variations thereof are intended to cover non-exclusive inclusions.

[0049] In the description of the embodiments of the present application, the technical terms "first", "second", etc. are only used to distinguish different objects, and cannot be understood as indicating or implying relative importance or implicitly indicating the number, specific order or primary and secondary relationship of the indicated technical features. In the description of the embodiments of the present application, the meaning of "multiple" is more than two, unless otherwise clearly and specifically defined.

[0050] Reference to "embodiments" herein means that a particular feature, structure, or characteristic described in conjunction with the embodiments may be included in at least one embodiment of the present application. The appearance of the phrase in various locations in the specification does not necessarily refer to the same embodiment, nor is it an independent or alternative embodiment that is mutually exclusive with other embodiments. It is explicitly and implicitly understood by those skilled in the art that the embodiments described herein may be combined with other embodiments.

[0051] In the description of the embodiments of the present application, the term "and / or" is only a description of the association relationship of the associated objects, indicating that there may be three relationships. For example, A and / or B can represent: A exists alone, A and B exist at the same time, and B exists alone. In addition, the character " / " in this article generally indicates that the associated objects before and after are in an "or" relationship.

[0052] In the description of the embodiments of the present application, the term "multiple" refers to more than two (including two). Similarly, "multiple groups" refers to more than two groups (including two groups), and "multiple pieces" refers to more than two pieces (including two pieces).

[0053] In the description of the embodiments of the present application, the technical terms "center", "longitudinal", "lateral", "length", "width", "thickness", "up", "down", "front", "back", "left", "right", "vertical", "horizontal", "top", "bottom", "inside", "outside", "clockwise", "counterclockwise", "axial", "radial", "circumferential", etc. indicate orientations or positional relationships based on the orientations or positional relationships shown in the accompanying drawings, which are only for the convenience of describing the embodiments of the present application and simplifying the description, and do not indicate or imply that the referred device or element must have a specific orientation, be constructed and operated in a specific orientation, and therefore should not be understood as a limitation on the embodiments of the present application.

[0054] In the description of the embodiments of the present application, unless otherwise clearly specified and limited, technical terms such as "installed", "connected", "connected", "fixed" and the like should be understood in a broad sense. For example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection or an indirect connection through an intermediate medium, and it can be the internal connection of two elements or the interaction relationship between two elements. For those of ordinary skill in the art, the specific meanings of the above terms in the embodiments of the present application can be understood according to the specific circumstances.

[0055] Common modification methods for sodium vanadium phosphate include ion doping, improved conductive agents, carbon coating and nano-crystallization, which can provide a fast diffusion path for ions, and are also conducive to improving the conduction path of electrons, and improving the rate performance and cycle performance of electrode materials. However, most of these synthesized materials are in the form of granular blocks, and need to be combined with various traditional additives and current collectors to prepare electrodes. The proportion of active materials in the prepared electrodes is not high, and the electronic conductivity is low, resulting in too low battery energy density. The materials modified by carbon coating have poor flexibility and do not have wearable properties.

[0056] In order to solve the technical problems of low electronic conductivity and low flexibility of sodium vanadium phosphate electrode materials, the present application provides a carbon nanofiber-encapsulated sodium vanadium phosphate flexible self-supporting electrode material, which includes a plurality of staggered overlapping polyacrylonitrile carbonized nanofibers, and the polyacrylonitrile carbonized nanofibers are coated with sodium vanadium phosphate particles.

[0057] Suitable but not restrictive, a plurality of staggered overlapping polyacrylonitrile carbonized nanofibers refers to a number of polyacrylonitrile carbonized nanofibers greater than or equal to 2 being staggered overlapping.

[0058] In the technical solution of the embodiment of the present application, polyacrylonitrile (PAN) can be used to adsorb VO2+ , sodium vanadium phosphate (NVP) is uniformly coated on polyacrylonitrile carbonized nanofibers to form a composite material of NVP and carbon nanofibers (NVP@CNF), and NVP@CNF is formed into a three-dimensional network structure by staggered overlapping, that is, a flexible self-supporting electrode material of carbon nanofiber-encapsulated sodium vanadium phosphate is obtained. The electrode material provides a large number of sodium ion adsorption sites, which can promote the embedding of sodium ions into the cross-linked electrode material of the NVP fiber. At the same time, since the polyacrylonitrile carbonized nanofiber coating layer is conductive, it is beneficial to improve the electronic conductivity of the material; on the other hand, the carbonized polyacrylonitrile fiber has good flexibility, which improves the flexibility of the material, and finally a flexible self-supporting electrode material with good flexibility and high electronic conductivity is obtained.

[0059] Furthermore, in the present application, the advantage of selecting PAN for forming NVP@CNF is that NVP has strong solubility, high dielectric constant, and a high carbonization rate of about 50%, making it easier to form NVP@CNF.

[0060] In some embodiments, the polyacrylonitrile carbon nanofiber includes a coated region coated with sodium vanadium phosphate particles and an uncoated region not coated with sodium vanadium phosphate particles, wherein the cross-sectional diameter of the uncoated region is 300-500nm, including but not limited to 300nm, 350nm, 400nm, 450nm, 500nm, and the cross-sectional diameter of the coated region is 400-600nm, including but not limited to 400nm, 450nm, 500nm, 550nm, and 600nm.

[0061] It can be understood that in the coating area, the cross-sectional diameter of the sodium aluminate phosphate particles is matched with the cross-sectional diameter of the polyacrylonitrile carbonized nanofibers to achieve the coating of the sodium aluminate phosphate particles within the polyacrylonitrile carbonized nanofibers, and the carbon layer is not too thick. If the cross-sectional diameter of the coating area is too large and the cross-sectional diameter of the uncoated area is too small, the sodium aluminate phosphate particles are easy to leak and good coating cannot be achieved, resulting in reduced material flexibility and low electronic conductivity. If the cross-sectional diameter of the coating area is too small and the cross-sectional diameter of the uncoated area is too large, the carbonized nanofiber layer is too thick, resulting in reduced electronic conductivity.

[0062] like Figure 1 As shown, the present application embodiment provides a method for preparing a flexible self-supporting electrode material of sodium aluminate phosphate encapsulated by carbon nanofibers, comprising the following steps:

[0063] S1, preparing a precursor solution containing sodium vanadium phosphate particles and polyacrylonitrile;

[0064] S2, electrospinning the spinning precursor solution to obtain a precursor film;

[0065] S3. The precursor film is dried, pre-sintered, and then subjected to secondary sintering treatments in sequence to obtain a flexible self-supporting electrode material of carbon nanofiber-encapsulated sodium alum phosphate.

[0066] In the technical solution of the embodiment of the present application, the polyacrylonitrile solution has high viscosity and can absorb VO 2+ , so that the raw materials in the spinning precursor solution are evenly dispersed in the polyacrylonitrile solution, and then the NVP is encapsulated in the polyacrylonitrile carbonized fiber through electrospinning and heat treatment, which accelerates the rapid migration of sodium ions and obtains an electrode material with high electronic conductivity and good flexibility.

[0067] In some embodiments, the step of preparing a precursor solution containing sodium vanadium phosphate particles and polyacrylonitrile in step S1 includes:

[0068] dissolving polyacrylonitrile in the first solvent to obtain a polyacrylonitrile solution;

[0069] A vanadium source, a sodium source, a phosphorus source, a reducing agent, a carbon source and a second solvent are mixed and stirred to obtain a black gel;

[0070] The black gel is calcined and ground to obtain sodium sulfate phosphate precursor particles;

[0071] Dispersing sodium vanadium phosphate precursor particles into a polyacrylonitrile solution to obtain a precursor solution containing sodium vanadium phosphate particles and polyacrylonitrile;

[0072] The first solvent includes at least one of dimethylformamide and N-methylpyrrolidone, and the second solvent includes at least one of deionized water, anhydrous ethanol, acetic acid, and tetrahydrofuran.

[0073] In this embodiment, the molar ratio of the vanadium source to the reducing agent is 1:(1-4); and / or, the molar ratio of the vanadium source to the carbon source is (0.05-5):1; and / or, the molar ratio of the vanadium source to the sodium source is 2:(3-5); and / or, the molar ratio of the vanadium source to the phosphorus source is 2:(3-5).

[0074] Within the limited range, the obtained product is sodium vanadium phosphate. If the above limited range is exceeded, the obtained sodium vanadium phosphate has a high impurity content. Specifically, the molar ratio of the vanadium source to the reducing agent can be 1:1, 1:2, 1:3, 1:4 or any value in the range of 1:(1-4); the molar ratio of the vanadium source to the carbon source can be 0.05:1, 0.1:1, 1:1, 2:1, 3:1, 4:1, 5:1 or any value in the range of (0.05-5):1; the molar ratio of the vanadium source to the sodium source can be 2:3, 2:4, 2:5 or any value in the range of 2:(3-5); the molar ratio of the vanadium source to the phosphorus source can be 2:3, 2:4, 2:5 or any value in the range of 2:(3-5).

[0075] Furthermore, the vanadium source includes one or more of vanadium pentoxide, ammonium metavanadate, vanadium dioxide, and sodium metavanadate; the sodium source includes one or more of sodium oxalate, disodium hydrogen phosphate, sodium carbonate, sodium bicarbonate, sodium hydroxide, and sodium citrate; the phosphorus source includes one or more of diammonium hydrogen phosphate, ammonium dihydrogen phosphate, diammonium phosphate, and phosphoric acid; the reducing agent is one or more of citric acid, oxalic acid, oxalic acid, malonic acid, and ascorbic acid; and the carbon source includes at least one of citric acid, sucrose, and glucose.

[0076] The stirring temperature for mixing the vanadium source, the sodium source, the phosphorus source, the reducing agent, the carbon source and the second solvent is 60-80° C., which is conducive to uniform mixing of the materials.

[0077] Furthermore, in this embodiment, the black gel is calcined to remove the solvent, and the obtained sodium phosphate has high purity. Specifically, the calcination temperature of the black gel is 300-350°C, for example, the calcination temperature can be 300°C, 330°C, 350°C or any value within the range of 300-350°C, and the calcination heating rate is 5-6°C min -1 Under the calcination conditions, the sodium alum phosphate particle size can be controlled within the range of 400-600 nm by adjusting the amount of each raw material, including but not limited to 400 nm, 500 nm, and 600 nm. Thereafter, the sodium alum phosphate particles are loosened by grinding to facilitate subsequent dispersion in the polyacrylonitrile solution. If the calcination temperature is too high, the particle size of the sodium alum phosphate particles increases, which is not conducive to electron transmission. If the calcination temperature is too low, the purity of the sodium alum phosphate particles is reduced.

[0078] Further, the mass ratio of sodium alum phosphate particles to polyacrylonitrile is 1:(0.5-1.5). Specifically, the mass ratio of sodium alum phosphate particles to polyacrylonitrile can be 1:0.5, 1:1, 1:1.5 or any value within the range of 1:(0.5-1.5).

[0079] Understandably, if too much sodium alum phosphate particles are added, agglomeration will occur, and if too little sodium alum phosphate particles are added, it will be detrimental to the improvement of electronic conductivity.

[0080] Further, in this embodiment, when polyacrylonitrile is dissolved in the first solvent, the usage ratio of polyacrylonitrile to the first organic solvent is (0.01-1) mg:1 mL, including but not limited to 0.01 g:1 mL, 0.05 g:1 mL, 0.1 g:1 mL, 0.15 g:1 mL, 0.17 g:1 mL, 0.19 g:1 mL, 0.21 g:1 mL, 0.25 g:1 mL, 0.3 g:1 mL, 0.4 g:1 mL, 0.5 g:1 mL, 0.6 g:1 mL, 0.7 g:1 mL, 0.8 g:1 mL, 0.9 g:1 mL, and 1 g:1 mL, any one of the point values ​​or the range values ​​between any two of them.

[0081] In some embodiments, in step S2, the temperature of electrospinning is 20-30°C, the humidity is 20-30%, the positive voltage of electrospinning is 13KV, the negative voltage is -3KV, and the injection speed is set to 0.16cm min -1 After 5 hours, you will get a sheet of about 15×20cm 2 The spun film is the precursor film.

[0082] It can be understood that during the electrospinning process, under the action of the electric field, the droplet at the needle tip will change from a spherical shape to a conical shape, and then be ejected to form fiber filaments, and finally obtain a precursor film.

[0083] In some embodiments, in step S3, the drying temperature is 60-100°C and the drying time is 8-24h; and / or the pre-sintering temperature is 200-220°C and the pre-sintering heating rate is 0.5-0.6°C min -1 ; and / or, the secondary sintering temperature is 500-800°C, and the secondary sintering time is 1-15h.

[0084] Specifically, the drying temperature of the precursor film can be 60℃, 70℃, 80℃, 90℃, 100℃ or any value between 60-100℃; the drying time can be 8h, 10h, 12h, 14h, 16h, 18h, 20h, 22h, 24h or any value between 8-24h; the pre-sintering temperature can be 200℃, 210℃, 220℃ or any value between 200-220℃; the secondary sintering temperature can be 500℃, 600℃, 700℃, 800℃ or any value between 500-800℃; the secondary sintering time can be 1h, 3h, 5h, 7h, 9h, 11h, 13h, 15h or any value between 1-15h.

[0085] In this embodiment, drying is performed within a temperature limit range to remove the solvent and facilitate spinning to be peeled off from the aluminum foil. If the temperature is too high, energy is wasted, and if the temperature is too low, the solvent evaporation time is too long. In the air, the purpose of pre-sintering is to pre-oxidize and solidify the spinning, which can avoid structural collapse and increase oxygen-containing functional groups. After the pre-sintering treatment, it is cooled to room temperature and then subjected to secondary sintering. The secondary sintering is performed in an inert atmosphere. The purpose of the secondary sintering is to synthesize sodium phosphate@polyacrylonitrile carbonized nanofiber composite materials by annealing. Among them, secondary sintering in an inert atmosphere is conducive to improving the purity of NVP and ensuring that the NVP structure is not destroyed.

[0086] In a third aspect, an embodiment of the present application provides a positive electrode plate, comprising the aforementioned carbon nanofiber-encapsulated sodium vanadium phosphate flexible self-supporting electrode material, or comprising the carbon nanofiber-encapsulated sodium vanadium phosphate flexible self-supporting electrode material prepared by the aforementioned preparation method.

[0087] In this embodiment, the positive electrode plate includes the aforementioned carbon nanofiber-encapsulated sodium vanadium phosphate flexible self-supporting electrode material, thereby having the advantages of high electronic conductivity and good flexibility brought by the material.

[0088] In a fourth aspect, an embodiment of the present application provides a sodium ion battery, comprising the aforementioned positive electrode plate.

[0089] In this embodiment, the sodium ion battery includes the aforementioned positive electrode plate, and thus has the advantage of high energy density.

[0090] Some specific embodiments are listed below. It should be noted that the embodiments described below are exemplary and are only used to explain the present application, and should not be construed as limiting the present application. If specific techniques or conditions are not specified in the embodiments, the techniques or conditions described in the literature in this area or the product specifications are used. The reagents or instruments used without specifying the manufacturer are all conventional products that can be obtained commercially.

[0091] 1. Preparation method

[0092] Example 1

[0093] A method for preparing a flexible self-supporting electrode material of carbon nanofiber encapsulated sodium alum phosphate comprises:

[0094] S1. Add 3.15 g of ammonium metavanadate (NH4VO3) into a beaker containing 150 mL of H2O, and stir magnetically at 80°C for 30 min. Then, add 3.32 g of sodium citrate (C6H5Na3O7), 4.65 g of ammonium dihydrogen phosphate (NH4H2PO4), and 1.50 g of citric acid (C6H8O7) in sequence. Both the reducing agent and the carbon source are citric acid. Stir continuously at 80°C until the solution becomes a black gel. Take out the black gel and place it in a long magnetic boat, and place it in a tubular furnace filled with nitrogen (N2) atmosphere. Keep it at 350°C for 5 h, and the heating rate is 5°C min -1 After cooling to room temperature, manually grind to obtain sodium alum phosphate particles. Further, take 10mL DMF into a 25mL beaker, then add 1.0g PAN under continuous stirring, wait for 6 hours for it to fully dissolve, then add 1.0g sodium alum phosphate particles, stir magnetically for 10 hours, and evenly disperse the sodium alum phosphate particles in the PAN / DMF solution to obtain a precursor solution;

[0095] S2. The precursor solution was sucked into the syringe, and a No. 18 stainless steel needle was put on. The syringe was installed in the electrospinning machine, and a layer of aluminum paper was pasted on the surface of the cylindrical receiver. The distance between the receiver and the needle was adjusted to 20 cm. The working temperature was maintained at 25 ° C, the humidity was 25%, the positive and negative voltages were connected to 13 kV and -3 kV, and the injection speed was set to 0.16 cm / min. After 5 hours, a sheet of about 15×20 cm 2 Precursor film;

[0096] S3. Place the precursor film in a forced air oven at 80°C for 12 hours for standby use. Cut the dried precursor film into long strips and place them in a magnetic boat. Then, place them in a muffle furnace and set the heating rate to 0.5°C min -1 , and kept at 200℃ for 2h. After the temperature dropped to room temperature, it was moved to a tubular furnace filled with argon and heated to 800℃ and kept for 2h at a heating rate of 2℃min -1 , and obtain a flexible self-supporting electrode material of carbon nanofiber-encapsulated sodium alum phosphate.

[0097] The carbon nanofiber-encapsulated sodium vanadium phosphate flexible self-supporting electrode material obtained according to the above method includes a plurality of staggered overlapping polyacrylonitrile carbonized nanofibers, and the polyacrylonitrile carbonized nanofibers are coated with sodium vanadium phosphate particles; the polyacrylonitrile carbon nanofibers include a coated area coated with sodium vanadium phosphate particles and an uncoated area not coated with the sodium vanadium phosphate particles, wherein the cross-sectional diameter of the uncoated area is 500nm, and the cross-sectional diameter of the coated area is 580nm.

[0098] Example 2

[0099] A method for preparing a flexible self-supporting electrode material of carbon nanofiber encapsulated sodium alum phosphate comprises:

[0100] S1. Add 3.15g of ammonium metavanadate (NH4VO3) into a beaker containing 150mL of H2O, and stir magnetically at 80°C for 30min. Then, add 3.32g of sodium source sodium citrate (C6H5Na3O7), 4.65g of ammonium dihydrogen phosphate (NH4H2PO4), and 1.50g of citric acid (C6H8O7) in sequence. Both the reducing agent and the carbon source are citric acid. Stir continuously at 80°C until the solution becomes a black gel. Take out the black gel and place it in a long magnetic boat, and place it in a tubular furnace filled with nitrogen (N2) atmosphere. Keep it at 350°C for 5h, and the heating rate is 5°C min -1After cooling to room temperature, manually grind to obtain sodium alum phosphate particles. Further, take 10mL DMF into a 25mL beaker, then slowly add 0.5g PAN under continuous stirring, wait for 6h to fully dissolve, then add 1.0g sodium alum phosphate particles, stir magnetically for 10h, and evenly disperse the sodium alum phosphate particles in the PAN / DMF solution to obtain a precursor solution.

[0101] S2. The precursor solution was sucked into the syringe, and a No. 18 stainless steel needle was put on. The syringe was installed in the electrospinning machine, and a layer of aluminum paper was pasted on the surface of the cylindrical receiver. The distance between the receiver and the needle was adjusted to 20 cm. The working temperature was maintained at 25 ° C, the humidity was 25%, the positive and negative voltages were connected to 13 kV and -3 kV, and the injection speed was set to 0.16 cm / min. After 5 hours, a sheet of about 15×20 cm 2 Precursor film;

[0102] S3. Place the precursor film in a forced air oven at 80°C for 12 hours. Cut the dried precursor film into strips and place them in a magnetic boat. Then, place them in a muffle furnace and set the heating rate to 0.5°C min. -1 , and kept at 200℃ for 2h. After the temperature dropped to room temperature, it was moved to a tubular furnace filled with argon and heated to 800℃ and kept for 2h at a heating rate of 2℃min -1 , and obtain a flexible self-supporting electrode material of carbon nanofiber-encapsulated sodium alum phosphate.

[0103] The carbon nanofiber-encapsulated sodium vanadium phosphate flexible self-supporting electrode material obtained according to the above method includes a plurality of staggered overlapping polyacrylonitrile carbonized nanofibers, and the polyacrylonitrile carbonized nanofibers are coated with sodium vanadium phosphate particles; the polyacrylonitrile carbon nanofibers include a coated area coated with sodium vanadium phosphate particles and an uncoated area not coated with the sodium vanadium phosphate particles, wherein the cross-sectional diameter of the uncoated area is 500nm, and the cross-sectional diameter of the coated area is 550nm.

[0104] Example 3

[0105] A method for preparing a flexible self-supporting electrode material of carbon nanofiber encapsulated sodium alum phosphate comprises:

[0106] S1. Add 3.15g of ammonium metavanadate (NH4VO3) into a beaker containing 150mL of H2O, and stir magnetically at 80°C for 30min. Then, add 4.17g of sodium citrate (C6H5Na3O7), 4.65g of ammonium dihydrogen phosphate (NH4H2PO4), and 2.30g of citric acid (C6H8O7) in sequence. Both the reducing agent and the carbon source are citric acid. Stir continuously at 80°C until the solution becomes a black gel. Take out the black gel and place it in a long magnetic boat, and place it in a tubular furnace filled with nitrogen (N2) atmosphere. Keep it at 300°C for 5h, and the heating rate is 5°C min -1 After cooling to room temperature, manually grind to obtain sodium alum phosphate particles. Further, take 10mL DMF into a 25mL beaker, then slowly add 1.5g PAN under continuous stirring, wait for 6 hours for it to fully dissolve, then add 1.0g sodium alum phosphate particles, stir magnetically for 10 hours, and evenly disperse the sodium alum phosphate particles in the PAN / DMF solution to obtain a precursor solution;

[0107] S2. The precursor solution was sucked into the syringe, and a No. 18 stainless steel needle was put on. The syringe was installed in the electrospinning machine, and a layer of aluminum paper was pasted on the surface of the cylindrical receiver. The distance between the receiver and the needle was adjusted to 20 cm, the working temperature was maintained at 25 ° C, the humidity was 25%, the positive and negative voltages were connected to 13 kV and -3 kV, and the injection speed was set to 0.16 cm / min. After 5 hours, a sheet of about 15×20 cm 2 Precursor film;

[0108] S3. Place the precursor film in a forced air oven at 80°C for 12 hours. Cut the dried precursor film into strips and place them in a magnetic boat. Then, place them in a muffle furnace and set the heating rate to 0.5°C min. -1 , and kept at 220℃ for 2h. After the temperature dropped to room temperature, it was moved to a tubular furnace filled with argon and heated to 700℃ and kept for 2h at a heating rate of 2℃min -1 , and obtain a flexible self-supporting electrode material of carbon nanofiber-encapsulated sodium alum phosphate.

[0109] The carbon nanofiber-encapsulated sodium vanadium phosphate flexible self-supporting electrode material obtained according to the above method includes a plurality of staggered overlapping polyacrylonitrile carbonized nanofibers, and the polyacrylonitrile carbonized nanofibers are coated with sodium vanadium phosphate particles; the polyacrylonitrile carbon nanofibers include a coated area coated with sodium vanadium phosphate particles and an uncoated area not coated with the sodium vanadium phosphate particles, wherein the cross-sectional diameter of the uncoated area is 460nm, and the cross-sectional diameter of the coated area is 600nm.

[0110] Example 4

[0111] A method for preparing a carbon nanofiber-encapsulated sodium vanadium phosphate flexible self-supporting electrode material, the other contents are the same as those in Example 1, except that the vanadium source is vanadium dioxide, the sodium source is sodium oxalate, and the phosphorus source is phosphoric acid.

[0112] The carbon nanofiber-encapsulated sodium alum phosphate flexible self-supporting electrode material obtained according to the above method comprises a plurality of staggered overlapping polyacrylonitrile carbonized nanofibers, and the polyacrylonitrile carbonized nanofibers are coated with sodium alum phosphate particles.

[0113] Example 5

[0114] A method for preparing a carbon nanofiber encapsulated sodium alum phosphate flexible self-supporting electrode material, the other contents are the same as those of Example 1, except that the drying temperature is 100°C and the secondary sintering temperature is 500°C.

[0115] The carbon nanofiber-encapsulated sodium alum phosphate flexible self-supporting electrode material obtained according to the above method comprises a plurality of staggered overlapping polyacrylonitrile carbonized nanofibers, and the polyacrylonitrile carbonized nanofibers are coated with sodium alum phosphate particles.

[0116] Comparative Example 1

[0117] A sodium vanadium phosphate electrode, the preparation method of which is as follows:

[0118] 3.15 g of ammonium nitrate (NH4VO3) was added to a beaker containing 150 mL of H2O and stirred magnetically at 80°C for 30 min. Then, 3.32 g of sodium citrate (C6H5Na3O7), 4.65 g of ammonium dihydrogen phosphate (NH4H2PO4), and 1.50 g of citric acid (C6H8O7) were added in sequence and stirred continuously at 80°C until the solution was in the form of a black gel. The black gel was taken out and placed in a long magnetic boat, which was then placed in a tubular furnace filled with nitrogen (N2) atmosphere and kept at 350°C for 5 h with a heating rate of 5°C min -1 After cooling to room temperature, the precursor particles are manually ground.

[0119] The precursor particles were placed flatly in a magnetic boat, placed in a tubular furnace filled with argon, heated to 800 °C and kept at this temperature for 2 h at a heating rate of 2 °C min -1 , and obtain sodium vanadium phosphate positive electrode material.

[0120] 2. Test Method

[0121] 1. SEM test

[0122] The carbon nanofiber encapsulated sodium vanadium phosphate flexible self-supporting electrode prepared in Example 1 and the sodium vanadium phosphate positive electrode material prepared in Comparative Example 1 were subjected to SEM test. The test results are shown in Figure 2-3 .

[0123] 2. XRD test

[0124] XRD test was performed on the carbon nanofiber encapsulated sodium vanadium phosphate flexible self-supporting electrode prepared in Example 1 and the sodium vanadium phosphate positive electrode material prepared in Comparative Example 1. The test results are shown in Figure 4 .

[0125] 3. TEM test

[0126] The carbon nanofiber encapsulated sodium vanadium phosphate flexible self-supporting electrode prepared in Example 1 was subjected to TEM test. The test results are shown in Figure 5 .

[0127] 4. Properties test of sodium ion batteries

[0128] The carbon nanofibers encapsulated sodium vanadium phosphate flexible self-supporting electrode prepared in Example 1 were assembled into a sodium ion battery, and the sodium ion battery was subjected to charge and discharge experiments at different rates. The results are as follows: Figure 6 shown.

[0129] III. Analysis of test results of various embodiments and comparative examples

[0130] See also Figure 2 ,pass Figure 2 It can be seen that the microscopic morphology of the electrode is continuous irregularly oriented nanofibers, and multiple bean-shaped structures are connected to the fibers, which shows that the NVP is successfully encapsulated in the carbon nanofibers.

[0131] See also Figure 3 ,pass Figure 3 It can be seen that the NVP precursor is at the nano-particle level after ball milling, and the sodium alum phosphate electrode prepared in Comparative Example 1 is a granular material.

[0132] See also Figure 4 ,pass Figure 4 It can be seen that the crystallinity of the material prepared in Example 1 is higher than that of the comparative example 1 and the commercial sodium alum phosphate, which is beneficial to improving its ionic conductivity and accelerating the reaction kinetics.

[0133] See also Figure 5 ,pass Figure 5 It can be seen that the inside of the bean-shaped object on the fiber is clearly visible, which more intuitively shows the morphology of the carbon fiber-coated NVP and further proves that the electrode preparation of Example 1 is successful.

[0134] See also Figure 6 ,pass Figure 6 It can be seen that the battery obtained in Example 1 can still maintain a good platform and a relatively high capacity even at a high current density, and has good cycle performance.

[0135] It should be noted that the present application is not limited to the above-mentioned embodiments. The above-mentioned embodiments are only examples, and the embodiments having the same structure as the technical idea and playing the same role within the technical solution of the present application are all included in the technical scope of the present application. In addition, without departing from the scope of the main purpose of the present application, various modifications that can be thought of by those skilled in the art to the embodiments and other methods of combining some of the constituent elements in the embodiments are also included in the scope of the present application.

Claims

1. A carbon nanofiber encapsulated sodium alum phosphate flexible self-supporting electrode material, characterized in that: The invention comprises a plurality of staggered and overlapped carbonized polyacrylonitrile nanofibers, wherein the carbonized polyacrylonitrile nanofibers are coated with sodium alum phosphate particles.

2. The carbon nanofiber encapsulated sodium aluminate phosphate flexible self-supporting electrode material according to claim 1, characterized in that: The polyacrylonitrile carbon nanofiber comprises a coated region coated with sodium vanadium phosphate particles and an uncoated region not coated with the sodium vanadium phosphate particles, wherein the cross-sectional diameter of the uncoated region is 300-500nm, and the cross-sectional diameter of the coated region is 400-600nm.

3. A method for preparing a flexible self-supporting electrode material of carbon nanofiber encapsulated sodium alum phosphate as claimed in claim 1, characterized in that: The following steps are involved: preparing a precursor solution containing sodium vanadium phosphate particles and polyacrylonitrile; Electrospinning the precursor solution to obtain a precursor film; The precursor film is sequentially dried, pre-sintered and secondary-sintered to obtain the carbon nanofiber-encapsulated sodium alum phosphate flexible self-supporting electrode material.

4. The method for preparing the flexible self-supporting electrode material of carbon nanofiber encapsulated sodium alum phosphate according to claim 3, characterized in that: The step of preparing a precursor solution containing sodium vanadium phosphate particles and polyacrylonitrile comprises: dissolving polyacrylonitrile in a first solvent to obtain a polyacrylonitrile solution; A vanadium source, a sodium source, a phosphorus source, a reducing agent, a carbon source and a second solvent are mixed and stirred to obtain a black gel; The black gel is calcined and ground to obtain sodium vanadium phosphate precursor particles; Dispersing the sodium vanadium phosphate precursor particles in a polyacrylonitrile solution to obtain a precursor solution containing sodium vanadium phosphate particles and polyacrylonitrile; The first solvent includes at least one of dimethylformamide and N-methylpyrrolidone, and the second solvent includes at least one of deionized water, anhydrous ethanol, acetic acid, and tetrahydrofuran.

5. The method for preparing a flexible self-supporting electrode material of carbon nanofiber encapsulated sodium alum phosphate according to claim 3, wherein in the precursor mixed solution, the mass ratio of the sodium alum phosphate particles to the polyacrylonitrile is 1:(0.5-1.5).

6. The method for preparing the flexible self-supporting electrode material of carbon nanofiber encapsulated sodium alum phosphate according to claim 3, characterized in that: The drying temperature is 60-100°C, and the drying time is 8-24h; and / or The pre-sintering temperature is 200-220°C, and the pre-sintering heating rate is 0.5-0.6°C min -1 ; and / or The temperature of the secondary sintering is 500-800° C., and the time of the secondary sintering is 1-15 hours.

7. The method for preparing a flexible self-supporting electrode material of carbon nanofiber encapsulated sodium aluminate phosphate according to claim 4, characterized in that: The molar ratio of the vanadium source to the reducing agent is 1:(1-4); and / or The molar ratio of the vanadium source to the carbon source is (0.05-5):1; and / or The molar ratio of the vanadium source to the sodium source is 2:(3-5); and / or The molar ratio of the vanadium source to the phosphorus source is 2:(3-5).

8. The method for preparing a flexible self-supporting electrode material of carbon nanofiber encapsulated sodium aluminate phosphate according to claim 4, characterized in that: The vanadium source includes one or more of vanadium pentoxide, ammonium metavanadate, vanadium dioxide, and sodium metavanadate; and / or The sodium source includes one or more of sodium oxalate, disodium hydrogen phosphate, sodium carbonate, sodium bicarbonate, sodium hydroxide, and sodium citrate; and / or The phosphorus source includes one or more of diammonium hydrogen phosphate, ammonium dihydrogen phosphate, diammonium phosphate, and phosphoric acid; and / or The reducing agent comprises one or more of citric acid, oxalic acid, oxalic acid, malonic acid, and ascorbic acid; and / or The carbon source includes at least one of citric acid, sucrose and glucose.

9. A positive electrode sheet, characterized in that: It includes the carbon nanofiber encapsulated sodium vanadium phosphate flexible self-supporting electrode material as described in claims 1-2, or includes the carbon nanofiber encapsulated sodium vanadium phosphate flexible self-supporting electrode material prepared by the preparation method as described in claims 3-8.

10. A sodium ion battery, characterized in that: Comprising the positive electrode sheet as described in claim 9.