Copper iron borate-aluminum oxide-rGO composite particle, preparation method thereof and aqueous zinc ion battery

By preparing copper-iron borate-alumina-rGO composite particles with core-shell structure, the problems of high stability and cost of positive electrode materials of water-based zinc ion batteries are solved, and a water-based zinc ion battery with high specific capacity and stable performance are achieved. Large-scale industrial application.

CN119069682APending Publication Date: 2024-12-03SOUTH CHINA UNIV OF TECH +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411368416.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-29
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

Existing water-based zinc-ion battery positive electrode materials such as manganese, vanadium, and cobalt-based transition metal compounds have poor stability, toxicity and high cost in water. Copper-iron-based materials are easily soluble in water electrolytes, resulting in structural collapse and zinc negative electrodes. Inactivation hinders its commercial application in water-based secondary batteries.

Method used

Copper-iron borate-alumina-rGO composite particles with core-shell structure are used as the positive electrode material. The core is copper-iron borate particles, the intermediate shell is aluminum oxide, and the outer shell is reduced graphene oxide. It is chelated and dried, Prepare through heat treatment and sintering steps to form stable composite particles.

Benefits of technology

The copper-iron borate-alumina-rGO composite particles with high zinc storage potential, good structural stability, and compatible with aqueous electrolyte are achieved. The aqueous zinc ion battery as the positive electrode material has high specific capacity, stable charging and discharge platform and low production costs. Suitable for large-scale industrial production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119069682A_ABST
    Figure CN119069682A_ABST
Patent Text Reader

Abstract

The invention discloses copper iron borate-aluminum oxide-rGO composite particles, a preparation method thereof and an aqueous zinc ion battery. The ferric copper borate-aluminum oxide-rGO composite particle has a core-shell structure, the core is a ferric copper borate particle, the middle shell layer comprises aluminum oxide, and the shell comprises rGO. The preparation method of the copper iron borate-aluminum oxide-rGO composite particles comprises the following steps: 1) preparing copper iron borate particles; (2) preparing copper borate iron particles coated with aluminum oxide on the surfaces; and 3) coating the copper borate iron particles of which the surfaces are coated with aluminum oxide with rGO. The copper ferric borate-aluminum oxide-rGO composite particle has the advantages of high zinc storage potential, stable structure and performance, good compatibility with aqueous electrolyte, simple preparation method and low production cost, and the aqueous zinc ion battery prepared by using the copper ferric borate-aluminum oxide-rGO composite particle as a positive electrode material has the advantages of large specific capacity, good cycle performance, stable discharge platform, and wide application prospect. The method is suitable for large-scale industrial production and application.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of electrochemical energy storage, and in particular to copper iron borate-aluminum oxide-rGO composite particles and a preparation method thereof, and an aqueous zinc ion battery. Background Art

[0002] Aqueous zinc-ion batteries have the advantages of high specific capacity, high safety and low cost. They are considered to be an ideal alternative to lithium-ion batteries and have been favored by researchers in recent years. The positive electrode material is one of the key factors that determine the performance of aqueous zinc-ion batteries. Currently, the common positive electrode materials for aqueous zinc-ion batteries mainly include transition metal compounds such as manganese-based, vanadium-based, and cobalt-based. However, these transition metal compounds not only have poor stability in water, but also have certain toxicity and high prices, which to some extent deviate from the original intention of developing environmentally friendly and safe energy storage systems. In addition, studies have shown that copper-iron-based positive electrode materials have the advantages of low manufacturing cost and green environmental protection, and are suitable for aqueous zinc-ion batteries for large-scale energy storage. However, since copper ions are easily soluble in aqueous electrolytes and undergo disproportionation reactions, they will lead to problems such as reduction of active substances, collapse of electrode structure, and inactivation of zinc negative electrodes, which seriously hinder the commercial application of copper-iron-based compounds in aqueous secondary batteries.

[0003] Therefore, it is of great significance to develop an aqueous zinc-ion battery positive electrode material with excellent performance, good stability, low cost, and green environmental protection. Summary of the invention

[0004] The object of the present invention is to provide copper iron borate-aluminum oxide-rGO composite particles and a preparation method thereof and an aqueous zinc ion battery.

[0005] The technical solution adopted by the present invention is:

[0006] A copper iron borate-aluminum oxide-rGO composite particle has a core-shell structure, wherein the core is a copper iron borate (Cu2Fe(BO3)O2) particle, the composition of the middle shell layer includes aluminum oxide, and the composition of the outer shell includes reduced graphene oxide (rGO).

[0007] Preferably, the particle size of the copper-iron borate particles is 0.08 μm to 1.6 μm.

[0008] Preferably, the particle size of the copper iron borate-aluminum oxide-rGO composite particles is 0.1 μm to 2 μm.

[0009] A method for preparing the copper iron borate-aluminum oxide-rGO composite particles as described above comprises the following steps:

[0010] 1) dispersing a copper source, an iron source, a boric acid source and an organic chelating agent in water for chelation reaction, and then drying, heat treating, sintering and grinding the chelate to obtain copper iron borate particles;

[0011] 2) dispersing copper iron borate particles and potassium aluminum sulfate dodecahydrate in water to prepare a suspension, separating the copper iron borate particles loaded with potassium aluminum sulfate, drying, sintering and grinding, and obtaining copper iron borate particles coated with aluminum oxide;

[0012] 3) The reduced graphene oxide is dispersed in ethanol to prepare a reduced graphene oxide dispersion, and copper iron borate particles with aluminum oxide coated on the surface are added and dispersed evenly, and then dried and ground to obtain copper iron borate-aluminum oxide-rGO composite particles.

[0013] Preferably, a method for preparing the copper iron borate-aluminum oxide-rGO composite particles as described above comprises the following steps:

[0014] 1) dispersing a copper source, an iron source, a boric acid source and an organic chelating agent in water, heating and stirring to carry out a chelating reaction, and then taking the chelate and drying, grinding, heat treating, cooling, grinding, sintering, cooling and grinding to obtain copper iron borate particles;

[0015] 2) dissolving potassium aluminum sulfate dodecahydrate in water, adding copper iron borate particles and performing ultrasonic dispersion to prepare a suspension, filtering and separating the copper iron borate particles loaded with potassium aluminum sulfate, drying, sintering, cooling and grinding to obtain copper iron borate particles coated with aluminum oxide;

[0016] 3) Ultrasonic dispersion of reduced graphene oxide in ethanol is prepared, and copper iron borate particles coated with aluminum oxide are added and ultrasonically dispersed uniformly, followed by drying, cooling and grinding to obtain copper iron borate-aluminum oxide-rGO composite particles.

[0017] Preferably, the copper source in step 1) is at least one of copper acetate (Cu(CH3COO)2), copper oxalate (CuC2O4), copper citrate (Cu2C6H4O7), copper carbonate (CuCO3), copper sulfate (CuSO4), copper nitrate (Cu(NO3)2), and copper oxide (CuO).

[0018] Preferably, the iron source in step 1) is at least one of ferric citrate (FeC6H5O7), ferrous oxalate (FeC2O4), ferric nitrate (Fe(NO3)3), ferrous carbonate (FeCO3), iron powder (Fe), and iron oxide (Fe2O3).

[0019] Preferably, the boric acid source in step 1) is at least one of ammonium pentaborate (NH4B5O8), boric acid (H3BO3), ammonium borate (NH4HB4O7), boron oxide (B2O3), and boron powder (B).

[0020] Preferably, the organic chelating agent in step 1) is citric acid (C6H8O7), oxalic acid (H2C2O4), ethylenediaminetetraacetic acid (C 10 H 16 N2O8), diethylenetriaminepentaacetic acid (C 14 H 23 N3O 10 ) at least one of.

[0021] Preferably, in step 1), the molar ratio of copper in the copper source, iron in the iron source, and boron in the boric acid source is 1:0.4-0.6:0.50-0.75.

[0022] Preferably, the molar ratio of the copper source to the organic chelating agent in step 1) is 1:1-5.

[0023] Preferably, the chelating reaction in step 1) is carried out at a temperature of 60° C. to 90° C., and the reaction time is 2 h to 4 h.

[0024] Preferably, the drying in step 1) is carried out at a temperature of 80°C to 150°C.

[0025] Preferably, the grinding time in step 1) is 0.5h to 1h.

[0026] Preferably, the heat treatment in step 1) is carried out in an air atmosphere at a temperature of 300° C. to 400° C., and the treatment time is 3 h to 6 h.

[0027] Preferably, the sintering in step 1) is carried out in an air atmosphere at a temperature of 700° C. to 900° C., and the sintering time is 10 h to 20 h.

[0028] Preferably, in step 2), the mass ratio of the copper iron borate particles to potassium aluminum sulfate dodecahydrate is 1:0.005-0.050.

[0029] Preferably, the drying in step 2) is carried out at a temperature of 80°C to 150°C.

[0030] Preferably, the sintering in step 2) is carried out in an air atmosphere at a temperature of 300° C. to 500° C., and the sintering time is 3 h to 5 h.

[0031] Preferably, the grinding time in step 2) is 0.5h to 1h.

[0032] Preferably, in step 3), the mass ratio of the copper iron borate particles coated with aluminum oxide to the reduced graphene oxide is 1:0.005-0.050.

[0033] Preferably, the drying in step 3) is carried out at a temperature of 80°C to 150°C.

[0034] Preferably, the grinding time in step 3) is 0.5h to 1h.

[0035] A positive electrode material comprises the copper iron borate-aluminum oxide-rGO composite particles.

[0036] An aqueous zinc ion battery comprises the positive electrode material.

[0037] The beneficial effects of the present invention are as follows: the copper iron borate-aluminum oxide-rGO composite particles of the present invention have a high zinc storage potential, stable structure and performance, good compatibility with aqueous electrolytes, and a simple preparation method and low production cost. The aqueous zinc ion battery made using the composite particles as positive electrode materials has a large specific capacity, good cycle performance, and a stable discharge platform, and is suitable for large-scale industrial production and application.

[0038] Specifically:

[0039] 1) The copper iron borate-alumina-rGO composite particles of the present invention contain copper iron borate, borate and other polyanions (for example: (PO4) 3- 、(SO4) 2- 、(AsO4) 3- Compared with other borate cathode materials, copper iron borate has a smaller molecular weight and a larger proportion of active metal ions, thus having a higher theoretical specific capacity.

[0040] 2) The B and O atoms in the copper iron borate-aluminum oxide-rGO composite particles of the present invention have multiple coordination modes, so that they have more abundant ion diffusion channels, which is beneficial to improving the rate performance of aqueous zinc ion batteries;

[0041] 3) The copper iron borate-alumina-rGO composite particles of the present invention contain copper iron borate. Compared with copper iron oxide, copper iron borate improves the zinc storage potential and structural stability of the positive electrode material by virtue of the "inductive effect" of the borate group;

[0042] 4) The copper iron borate-aluminum oxide-rGO composite particles of the present invention contain aluminum oxide and reduced graphene oxide. Aluminum oxide is coated on the surface of the copper iron borate particles, which can reduce the acidity of the electrolyte and reduce the corrosion of the positive electrode material. Reduced graphene oxide can inhibit the dissolution of copper ions and improve the conductivity of the positive electrode material.

[0043] 5) The aqueous zinc ion battery made of the copper iron borate-aluminum oxide-rGO composite particles of the present invention as the positive electrode material has a high specific capacity and a stable charge and discharge platform (when the operating voltage window is 0.2V to 1.5V, the maximum discharge specific capacity can reach 416.3mAh / g);

[0044] 6) Compared with the currently common vanadium-based and cobalt-based positive electrode materials, the copper iron borate-aluminum oxide-rGO composite particles of the present invention have the advantages of low raw material cost and green environmental protection;

[0045] 7) The preparation method of the copper iron borate-aluminum oxide-rGO composite particles of the present invention is simple and has low production cost, and is suitable for large-scale industrial production and application. BRIEF DESCRIPTION OF THE DRAWINGS

[0046] Figure 1 : This is the XRD diagram of the copper iron borate-alumina-rGO composite particles in Examples 1 to 3.

[0047] Figure 2 This is the SEM image of the copper iron borate-alumina-rGO composite particles in Example 1.

[0048] Figure 3 This is the charge and discharge curve of the aqueous zinc ion battery assembled from the copper iron borate-alumina-rGO composite particles in Example 1.

[0049] Figure 4 This is the charge and discharge curve of the aqueous zinc ion battery assembled from the copper iron borate-alumina-rGO composite particles in Example 2.

[0050] Figure 5 This is the charge and discharge curve of the aqueous zinc ion battery assembled from the copper iron borate-alumina-rGO composite particles in Example 3. DETAILED DESCRIPTION

[0051] The present invention will be further explained and illustrated below in conjunction with specific embodiments.

[0052] Embodiment 1:

[0053] A copper iron borate-aluminum oxide-rGO composite particle, the preparation method of which is as follows:

[0054] 1) Cu(CH3COO)2, FeC6H5O7 and NH4B5O8 are dissolved in an appropriate amount of deionized water according to a molar ratio of Cu, Fe and B of 1:0.5:0.65, and then C6H8O7 in an equal molar amount to Cu(CH3COO)2 is added, and the mixture is stirred at a constant temperature of 80°C for 3 hours to form a sol, and then placed in an oven at 70°C for 12 hours to form a gel, and then the gel is ground with a quartz mortar for 0.5 hours to form a powder, and then placed in a muffle furnace at 400°C in an air atmosphere for 3 hours, and then naturally cooled to room temperature and ground for 0.5 hours, and then placed in a muffle furnace at 900°C in an air atmosphere for sintering for 10 hours, and then naturally cooled to room temperature and ground to obtain copper iron borate particles;

[0055] 2) stirring and dissolving an appropriate amount of potassium aluminum sulfate dodecahydrate in deionized water, and then adding copper iron borate particles according to a mass ratio of copper iron borate particles to potassium aluminum sulfate dodecahydrate of 1:0.05, ultrasonicating for 1 hour to make a suspension, filtering, taking the filtered solid and placing it in an oven at 80° C. for 4 hours, and then placing it in a muffle furnace at 300° C. in an air atmosphere for 5 hours. After naturally cooling to room temperature, grinding is performed to obtain copper iron borate particles coated with aluminum oxide;

[0056] 3) Add an appropriate amount of reduced graphene oxide to anhydrous ethanol, and then alternately stir and ultrasonicate for 3 times, the single stirring time is 0.5h, and the single ultrasonic time is 0.5h to form a reduced graphene oxide dispersion, and then add copper iron borate particles coated with aluminum oxide according to a mass ratio of 1:0.05 between copper iron borate particles coated with aluminum oxide and reduced graphene oxide, and then alternately stir and ultrasonicate for 2 times, the single stirring time is 1h, and the single ultrasonic time is 1h, and then place in an oven at 80°C for 3h, naturally cool to room temperature and grind to obtain copper iron borate-alumina-rGO composite particles.

[0057] Performance Test:

[0058] 1) The X-ray diffraction (XRD) pattern of the copper iron borate-aluminum oxide-rGO composite particles in this example is as follows Figure 1 shown.

[0059] Depend on Figure 1 It can be seen that the main peak intensity of the XRD diffraction peak of copper iron borate-alumina-rGO composite particles is high and sharp, and basically corresponds to the standard diffraction spectrum, indicating that the obtained product has good crystallinity and high purity.

[0060] 2) The scanning electron microscope (SEM) image of the copper iron borate-aluminum oxide-rGO composite particles in this example is as follows Figure 2 shown.

[0061] Depend on Figure 2 It can be seen that the flaky reduced graphene oxide is evenly coated on the surface of the copper iron borate particles.

[0062] 3) The copper iron borate-alumina-rGO composite particles in this example were used as the positive electrode material to assemble a button-type aqueous zinc ion battery (the negative electrode was zinc foil, and the electrolyte was a 2 mol / L aqueous solution of zinc trifluoromethanesulfonate), and then the electrochemical performance was tested by constant current charge and discharge method (current density was 100 mA / g, voltage window was 0.2 V to 1.5 V), and the charge and discharge curves obtained were as follows: Figure 3 shown.

[0063] Depend on Figure 3 It can be seen that the first-cycle discharge specific capacity of the aqueous zinc-ion battery reached 334.1 mAh / g.

[0064] Embodiment 2:

[0065] A copper iron borate-aluminum oxide-rGO composite particle, the preparation method of which is as follows:

[0066] 1) dissolving CuCO3, FeC2O4 and H3BO3 in an appropriate amount of deionized water according to a molar ratio of Cu, Fe and B of 1:0.5:0.6, then adding C6H8O7 in an equal molar amount to CuCO3, stirring at a constant temperature of 80°C for 3 hours to form a sol, then placing it in an oven at 70°C for 12 hours to form a gel, then grinding the gel with a quartz mortar for 0.5 hours to form a powder, then placing it in a muffle furnace at 350°C in an air atmosphere for 5 hours, naturally cooling to room temperature and then grinding for 0.5 hours, then placing it in a muffle furnace at 800°C in an air atmosphere for 15 hours, and then naturally cooling to room temperature and grinding to obtain copper iron borate particles;

[0067] 2) stirring and dissolving an appropriate amount of potassium aluminum sulfate dodecahydrate in deionized water, and then adding copper iron borate particles according to a mass ratio of copper iron borate particles to potassium aluminum sulfate dodecahydrate of 1:0.025, ultrasonicating for 1 hour to prepare a suspension, filtering, taking the filtered solid and placing it in an oven at 80° C. for 3 hours, and then placing it in a muffle furnace for sintering at 400° C. in an air atmosphere for 4 hours, naturally cooling to room temperature and grinding to obtain copper iron borate particles coated with aluminum oxide;

[0068] 3) Add an appropriate amount of reduced graphene oxide to anhydrous ethanol, and then alternately stir and ultrasonicate twice, the single stirring time is 1 hour, and the single ultrasonic time is 1 hour to form a reduced graphene oxide dispersion, and then add copper iron borate particles coated with aluminum oxide according to a mass ratio of 1:0.025 between copper iron borate particles coated with aluminum oxide and reduced graphene oxide, and then alternately stir and ultrasonicate three times, the single stirring time is 0.5 hour, and the single ultrasonic time is 0.5 hour, and then place it in an oven at 80°C for 4 hours, cool it naturally to room temperature, and then grind it to obtain copper iron borate-alumina-rGO composite particles.

[0069] Performance Test:

[0070] 1) The XRD pattern of the copper iron borate-aluminum oxide-rGO composite particles in this embodiment is as follows Figure 1 shown.

[0071] Depend on Figure 1 It can be seen that the main peak intensity of the XRD diffraction peak of copper iron borate-alumina-rGO composite particles is high and sharp, and basically corresponds to the standard diffraction spectrum, indicating that the obtained product has good crystallinity and high purity.

[0072] 2) The copper iron borate-alumina-rGO composite particles in this example were used as the positive electrode material to assemble a button-type aqueous zinc ion battery (the negative electrode was zinc foil, and the electrolyte was a 2 mol / L aqueous solution of zinc trifluoromethanesulfonate), and then the electrochemical performance was tested by constant current charge and discharge method (current density was 100 mA / g, voltage window was 0.2 V to 1.5 V), and the charge and discharge curves obtained were as follows: Figure 4 shown.

[0073] Depend on Figure 4 It can be seen that the first-cycle discharge specific capacity of the aqueous zinc-ion battery reached 357.7mAh / g.

[0074] Embodiment 3:

[0075] A copper iron borate-aluminum oxide-rGO composite particle, the preparation method of which is as follows:

[0076] 1) dissolving Cu(NO3)2, FeCO3 and B2O3 in an appropriate amount of deionized water according to a molar ratio of Cu, Fe and B of 1:0.5:0.6, then adding C6H8O7 in an equal molar amount to Cu(NO3)2, stirring at a constant temperature of 80°C for 3 hours to form a sol, then placing it in an oven at 70°C for 12 hours to form a gel, then grinding the gel with a quartz mortar for 0.5 hours to form a powder, then placing it in a muffle furnace at 300°C in an air atmosphere for 6 hours, naturally cooling to room temperature and then grinding for 0.5 hours, then placing it in a muffle furnace at 700°C in an air atmosphere for sintering for 20 hours, and naturally cooling to room temperature and then grinding to obtain copper iron borate particles;

[0077] 2) stirring and dissolving an appropriate amount of potassium aluminum sulfate dodecahydrate in deionized water, and then adding copper iron borate particles according to a mass ratio of copper iron borate particles to potassium aluminum sulfate dodecahydrate of 1:0.005, ultrasonicating for 1 hour to make a suspension, filtering, taking the filtered solid and placing it in an oven at 80° C. for 5 hours, and then placing it in a muffle furnace at 500° C. in an air atmosphere for 3 hours. After naturally cooling to room temperature, grinding is performed to obtain copper iron borate particles coated with aluminum oxide;

[0078] 3) Add an appropriate amount of reduced graphene oxide to anhydrous ethanol, and then alternately stir and ultrasonicate for 3 times, the single stirring time is 0.5h, and the single ultrasonic time is 0.5h to form a reduced graphene oxide dispersion, and then add copper iron borate particles coated with aluminum oxide according to a mass ratio of 1:0.005 between copper iron borate particles coated with aluminum oxide and reduced graphene oxide, and then alternately stir and ultrasonicate for 2 times, the single stirring time is 1h, and the single ultrasonic time is 1h, and then place in an oven at 80°C for 5h, naturally cool to room temperature and grind to obtain copper iron borate-alumina-rGO composite particles.

[0079] Performance Test:

[0080] 1) The XRD pattern of the copper iron borate-aluminum oxide-rGO composite particles in this embodiment is as follows Figure 1 shown.

[0081] Depend on Figure 1 It can be seen that the main peak intensity of the XRD diffraction peak of copper iron borate-alumina-rGO composite particles is high and sharp, and basically corresponds to the standard diffraction spectrum, indicating that the obtained product has good crystallinity and high purity.

[0082] 2) The copper iron borate-alumina-rGO composite particles in this example were used as the positive electrode material to assemble a button-type aqueous zinc ion battery (the negative electrode was zinc foil, and the electrolyte was a 2 mol / L aqueous solution of zinc trifluoromethanesulfonate), and then the electrochemical performance was tested by constant current charge and discharge method (current density was 100 mA / g, voltage window was 0.2 V to 1.5 V), and the charge and discharge curves obtained were as follows: Figure 5 shown.

[0083] Depend on Figure 5 It can be seen that the first-cycle discharge specific capacity of the aqueous zinc-ion battery reached 416.3mAh / g.

[0084] The above embodiments are preferred implementation modes of the present invention, but the implementation modes of the present invention are not limited to the above embodiments. Any other changes, modifications, substitutions, combinations, and simplifications that do not deviate from the spirit and principles of the present invention should be equivalent replacement methods and are included in the protection scope of the present invention.

Claims

1. A copper iron borate-aluminum oxide-rGO composite particle, characterized in that: The invention has a core-shell structure, wherein the core is copper iron borate particles, the composition of the middle shell layer includes aluminum oxide, and the composition of the outer shell includes reduced graphene oxide.

2. The copper iron borate-aluminum oxide-rGO composite particles according to claim 1, characterized in that: The particle size of the copper-iron borate particles is 0.08 μm to 1.6 μm.

3. The copper iron borate-aluminum oxide-rGO composite particles according to claim 1 or 2, characterized in that: The particle size of the copper iron borate-aluminum oxide-rGO composite particles is 0.1 μm to 2 μm.

4. A method for preparing copper iron borate-aluminum oxide-rGO composite particles as claimed in any one of claims 1 to 3, characterized in that: The following steps are involved: 1) dispersing a copper source, an iron source, a boric acid source and an organic chelating agent in water for chelation reaction, and then drying, heat treating, sintering and grinding the chelate to obtain copper iron borate particles; 2) dispersing copper iron borate particles and potassium aluminum sulfate dodecahydrate in water to prepare a suspension, separating the copper iron borate particles loaded with potassium aluminum sulfate, drying, sintering and grinding, and obtaining copper iron borate particles coated with aluminum oxide; 3) The reduced graphene oxide is dispersed in ethanol to prepare a reduced graphene oxide dispersion, and copper iron borate particles with aluminum oxide coated on the surface are added and dispersed evenly, and then dried and ground to obtain copper iron borate-aluminum oxide-rGO composite particles.

5. The preparation method according to claim 4, characterized in that: The copper source in step 1) is at least one of copper acetate, copper oxalate, copper citrate, copper carbonate, copper sulfate, copper nitrate, and copper oxide; the iron source in step 1) is at least one of ferric citrate, ferrous oxalate, ferric nitrate, ferrous carbonate, iron powder, and ferric oxide; the boric acid source in step 1) is at least one of ammonium pentaborate, boric acid, ammonium borate, boric oxide, and boron powder; the organic chelating agent in step 1) is at least one of citric acid, oxalic acid, ethylenediaminetetraacetic acid, and diethylenetriaminepentaacetic acid.

6. The preparation method according to claim 4 or 5, characterized in that: The molar ratio of copper in the copper source, iron in the iron source, and boron in the boric acid source in step 1) is 1:0.4-0.6:0.50-0.75; the molar ratio of the copper source and the organic chelating agent in step 1) is 1:1-5; the mass ratio of the copper iron borate particles and potassium aluminum sulfate dodecahydrate in step 2) is 1:0.005-0.050; the mass ratio of the copper iron borate particles coated with aluminum oxide and reduced graphene oxide in step 3) is 1:0.005-0.

050.

7. The preparation method according to claim 4 or 5, characterized in that: The chelating reaction in step 1) is carried out at a temperature of 60°C to 90°C, and the reaction time is 2h to 4h; the heat treatment in step 1) is carried out in an air atmosphere at a temperature of 300°C to 400°C, and the treatment time is 3h to 6h; the sintering in step 1) is carried out in an air atmosphere at a temperature of 700°C to 900°C, and the sintering time is 10h to 20h.

8. The preparation method according to claim 4 or 5, characterized in that: Step 2) The sintering is carried out in an air atmosphere at a temperature of 300° C. to 500° C., and the sintering time is 3 h to 5 h.

9. A positive electrode material, characterized in that: The invention comprises the copper iron borate-aluminum oxide-rGO composite particles according to any one of claims 1 to 3.

10. An aqueous zinc ion battery, characterized in that: Contains the positive electrode material according to claim 9.