Binder composition for secondary battery, application of binder composition, secondary battery and electronic equipment
By using polymer A as a binder, the antigel slurry composition for secondary batteries is prepared, and the stability of the lithium secondary battery positive electrode slurry is solved, and the operability and performance of the battery are improved, especially in the magnification Excellent performance in low temperature output.
Patent Information
- Application Number
- CN202310596289.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-24
- Publication Date
- 2024-12-03
AI Technical Summary
The interaction between polyvinylidene fluoride and the positive electrode particles in the positive electrode slurry of lithium secondary batteries is unstable, resulting in a decrease in the stability of the slurry, and adverse phenomena such as gel, miscoating, slope climbing, and burrs, affecting the performance of the battery.
The antigel slurry composition for secondary battery is prepared using polymer A containing N-vinylpyrrolidone monomer and an alkenyl chain carboxylic acid ester monomer with 3-15 carbon atoms as the binder. , improve the operability of the functional layer or electrode layer.
The storage stability and operability of the slurry composition for secondary batteries are significantly improved, the adhesion is enhanced, and the excellent functional layer and electrode layer are formed, which improves the battery's magnification and low-temperature output performance.
Smart Images

Figure BDA0004247375010000271 
Figure BDA0004247375010000272 
Figure BDA0004247375010000281
Abstract
Description
Technical Field
[0001] The present application belongs to the field of new energy technology, and specifically relates to a binder composition for a secondary battery, a slurry composition for a secondary battery, a functional layer for a secondary battery, an electrode layer for a secondary battery, a secondary battery and an electronic device. Background Art
[0002] With the implementation of the dual carbon policy, secondary batteries have developed rapidly, especially lithium secondary batteries, which have been widely used in many fields. In the manufacturing process of lithium batteries, the stability of the slurry is one of the important indicators of the slurry properties. The stability of the slurry directly affects the storage time of the slurry. The more stable the slurry is, the more continuity it can provide for production. At the same time, the stability of the slurry will also have a significant impact on the coating effect. The more stable the slurry is, the more stable the coating process is, the more stable the coating surface density is, and the prepared battery performance is stable and consistent.
[0003] However, the positive electrode slurry of lithium secondary batteries currently generally uses polyvinylidene fluoride as a binder. The interaction between the polyvinylidene fluoride molecular chain and the positive electrode particles is unstable, resulting in a decrease in the stability of the slurry, and the occurrence of adverse phenomena such as gelation, coating leakage, climbing, burrs, etc., which affects the performance of the battery. Summary of the invention
[0004] Problem that the invention aims to solve
[0005] In the art, there is no sufficient research on the gelation and dispersion of the slurry composition for secondary batteries, and the operability of the functional layer or electrode layer. Therefore, in the secondary battery, it is required to provide the following technology: a slurry composition for secondary batteries that is resistant to gelation can be prepared, and the operability of the functional layer or electrode layer formed using the slurry composition for secondary batteries can be improved.
[0006] In order to solve all or part of the above technical problems, one of the purposes of the present application is to provide a binder composition for secondary batteries, comprising a polymer A, wherein the polymer A comprises an N-vinyl pyrrolidone monomer unit and a carboxylate-containing monomer unit having an alkenyl chain, and the mass content of the carboxylate-containing monomer unit having an alkenyl chain with carbon atoms of 3-15 in the polymer A is 25%-50%. The binder composition for secondary batteries has excellent adhesion, the battery slurry prepared using the binder has good anti-gel properties, and the battery functional layer and battery electrode layer prepared using the binder have excellent operability.
[0007] The second purpose of the present application is to provide the use of the binder composition for secondary batteries in the preparation of slurry compositions for secondary batteries, functional layers for secondary batteries, electrode layers for secondary batteries, secondary batteries and electronic devices.
[0008] The third object of the present application is to provide a slurry composition for a secondary battery, comprising the binder composition for a secondary battery and non-conductive particles, wherein the slurry composition for a secondary battery has excellent storage stability.
[0009] A fourth object of the present application is to provide a slurry composition for a secondary battery, comprising the binder composition for a secondary battery and an electrode active material, wherein the slurry composition for a secondary battery has excellent storage stability.
[0010] A fifth object of the present application is to provide a functional layer for a secondary battery having excellent heat resistance and strength to improve the rate and low-temperature output performance of the secondary battery.
[0011] The sixth object of the present application is to provide an electrode layer for a secondary battery having excellent flexibility so as to improve the rate and low-temperature output performance of the secondary battery.
[0012] The seventh object of the present application is to provide a secondary battery, comprising a positive electrode, a negative electrode, a separator and an electrolyte, wherein at least one of the positive electrode, the negative electrode and the separator has the functional layer for the secondary battery and / or the electrode layer for the secondary battery. The secondary battery has excellent rate characteristics and output characteristics.
[0013] An eighth object of the present application is to provide an electronic device, wherein the power supply source of the electronic device includes the secondary battery.
[0014] Solutions for solving problems
[0015] The present applicant has conducted in-depth research for the purpose of providing the following technology: a slurry composition for a secondary battery that is resistant to gelling can be prepared, and the operability of a functional layer or electrode layer formed using the prepared slurry composition for a secondary battery can be improved. Based on this, the present inventor has found that by using a binder composition containing a specific polymer A, a slurry composition for a secondary battery that is resistant to gelling can be prepared, and the operability of a functional layer or electrode layer formed using the slurry composition for a secondary battery can be improved, so as to complete the present application.
[0016] That is, the purpose of the present application is to advantageously solve the above-mentioned problem. The binder composition for secondary batteries of the present application is characterized in that it is a binder composition for secondary batteries comprising polymer A, wherein the polymer A comprises N-vinyl pyrrolidone monomer units and carboxylate-containing monomer units having an alkenyl chain with carbon atoms of 3-15, and the mass content of carboxylate-containing monomer units having an alkenyl chain in the polymer A is 25%-50%. By using the binder composition for secondary batteries comprising polymer A, wherein the polymer A comprises N-vinyl pyrrolidone monomer units and a specified amount of carboxylate-containing monomer units having an alkenyl chain with carbon atoms of 3-15, a gel-resistant slurry composition for secondary batteries can be prepared, and the operability of the functional layer or electrode layer formed using the slurry composition for secondary batteries can be improved.
[0017] It should be noted that, in the present application, "comprising a monomer unit" means "a polymer obtained by using a monomer comprises a repeating unit derived from the monomer". In addition, in the present application specification, "improving the operability of the functional layer" includes, for example, improving the "adhesiveness" evaluated in the examples of the present application, and "improving the operability of the electrode layer" includes, for example, improving the "flexibility of the electrode layer during electrode rolling" evaluated in the examples of the present application.
[0018] In the present application, the “N-vinylpyrrolidone monomer unit” and the “content ratio of the carboxylate-containing monomer unit having an alkenyl chain having 3 to 15 carbon atoms” can be measured using a nuclear magnetic resonance (NMR) method such as 1H-NMR.
[0019] Here, in the binder composition for secondary batteries of the present application, it is preferred that the mass content of the carboxylate-containing monomer unit having an alkenyl chain with carbon numbers of 3 to 15 in the polymer A is 25% or more and 50% or less. If the mass content of the carboxylate-containing monomer unit having an alkenyl chain with carbon numbers of 3 to 15 in the polymer A is 25% or more and 50% or less, the operability of the functional layer or electrode layer formed using the prepared slurry composition for secondary batteries can be further improved, and the rate of the secondary battery having the electrode or separator formed using the binder composition can be improved.
[0020] In addition, in the secondary battery binder composition of the present application, the weight average molecular weight of the polymer A is preferably 5 kDa or more and 800 kDa or less. If the weight average molecular weight of the polymer A is 8 kDa or more and 800 kDa or less, the thickening of the slurry composition for secondary batteries can be suppressed, and the operability of the functional layer or electrode layer formed using the prepared slurry composition for secondary batteries can be further improved, and in the case where the slurry composition for secondary batteries contains an electrode active material, the surface of the electrode active material can be well covered by the adhesive layer formed by the binder composition for secondary batteries, and the bonding strength of the functional layer or electrode layer formed using the binder composition can be further improved.
[0021] It should be noted that, in the present application, the "weight average molecular weight of polymer A" can be measured by the method described in the examples of the present application.
[0022] In addition, the binder composition for secondary batteries of the present application preferably further contains component B, wherein component B includes at least one of citrate, tartrate, laurate, myristate, oleate, and stearate.
[0023] If the above-mentioned component B includes at least one of citrate, tartrate, laurate, myristic acid ester, oleate, and stearate, the gelation of the slurry composition for secondary batteries can be suppressed, and the operability of the functional layer or electrode layer formed using the prepared slurry composition for secondary batteries can be further improved, and the bonding strength of the functional layer or electrode layer formed using the binder composition can be further improved.
[0024] In addition, the purpose of the present application is to advantageously solve the above-mentioned problems. The secondary battery slurry composition of the present application is characterized in that it contains any of the above-mentioned secondary battery binder compositions and non-conductive microparticles. The secondary battery slurry composition containing any of the above-mentioned secondary battery binder compositions and non-conductive microparticles can suppress gelation, and can form a functional layer with improved operability, and can form a porous membrane layer with excellent heat resistance and strength.
[0025] In addition, the purpose of the present application is to advantageously solve the above-mentioned problems. The secondary battery slurry composition of the present application is characterized in that it contains any of the above-mentioned secondary battery binder compositions and electrode active materials. The secondary battery slurry composition containing any of the above-mentioned secondary battery binder compositions and electrode active materials can inhibit gelation, and can form an electrode layer with improved operability, and can form an electrode layer with excellent flexibility and can enable a secondary battery using the electrode to exert improved rate characteristics.
[0026] In addition, the purpose of the present application is to advantageously solve the above-mentioned problems, and the functional layer for secondary batteries of the present application is characterized in that it is formed using any of the above-mentioned slurry compositions for secondary batteries. The functional layer for secondary batteries formed using any of the above-mentioned slurry compositions for secondary batteries has excellent operability.
[0027] In addition, the purpose of the present application is to advantageously solve the above-mentioned problems, and the electrode layer for secondary batteries of the present application is preferably formed using the above-mentioned slurry composition for secondary batteries. The electrode layer for secondary batteries formed using the above-mentioned slurry composition for secondary batteries has excellent handleability.
[0028] In addition, the purpose of the present application is to advantageously solve the above-mentioned problems. The secondary battery of the present application is characterized in that it has a positive electrode, a negative electrode, a separator and an electrolyte, and at least one of the positive electrode, the negative electrode and the separator has the above-mentioned secondary battery functional layer and / or the above-mentioned secondary battery electrode layer. By having at least one of the positive electrode, the negative electrode and the separator have the above-mentioned secondary battery functional layer and / or the above-mentioned secondary battery electrode layer, a secondary battery having a secondary battery functional layer or a secondary battery electrode layer with excellent operability can be provided.
[0029] In addition, the purpose of the present application is to advantageously solve the above-mentioned problems. The secondary battery of the present application is characterized in that it has a positive electrode, a negative electrode, a separator and an electrolyte, at least one of the above-mentioned positive electrode, the above-mentioned negative electrode and the above-mentioned separator has the above-mentioned functional layer for secondary batteries or the above-mentioned electrode layer for secondary batteries, and the above-mentioned electrolyte includes at least one of 1,3-propane sultone, vinyl sulfate or methylene disulfonate. Based on the weight of the electrolyte, the content of 1,3-propane sultone, vinyl sulfate or methylene disulfonate is 0.1% to 3%. When at least one of 1,3-propane sultone, vinyl sulfate or methylene disulfonate is used in the electrolyte, the decomposition reaction of polymer A during the charge and discharge process can be suppressed, thereby not only improving the rate of the secondary battery, but also improving the low-temperature output performance.
[0030] In addition, the purpose of the present application is to advantageously solve the above-mentioned problems. An electronic device of the present application is characterized in that it has a secondary battery as a power supply source, the above-mentioned secondary battery has a positive electrode, a negative electrode, a separator and an electrolyte, and at least one of the above-mentioned positive electrode, the above-mentioned negative electrode and the above-mentioned separator has the above-mentioned functional layer for the secondary battery or the above-mentioned electrode layer for the secondary battery.
[0031] Technical Effects
[0032] The present application provides a binder composition for a secondary battery, which can prepare a gel-resistant slurry composition for a secondary battery, and can form a functional layer or an electrode layer with excellent workability using the slurry composition for a secondary battery.
[0033] Furthermore, the present application provides a slurry composition for a secondary battery, which can reduce gel and form a functional layer or an electrode layer with excellent workability.
[0034] Furthermore, the present application provides a functional layer for a secondary battery having excellent handleability.
[0035] Furthermore, the present application provides an electrode layer for a secondary battery having excellent handleability.
[0036] Furthermore, the present application provides a secondary battery having excellent rate and output performance, the secondary battery having a secondary battery functional layer or a secondary battery electrode layer having excellent operability.
[0037] In addition, the present application provides a secondary battery with excellent rate and low-temperature output performance, which has a functional layer for a secondary battery or an electrode layer for a secondary battery with excellent operability; and in an electrolyte system comprising at least one of 1,3-propane sultone, vinyl sulfate and methanedisulfonic acid methylene ester, not only the rate of the secondary battery is improved, but also the low-temperature output performance can be further improved.
[0038] Furthermore, the present application provides an electronic device having a secondary battery having excellent rate and low-temperature output performance. DETAILED DESCRIPTION
[0039] Hereinafter, embodiments of the present application are described in detail. However, these embodiments are exemplary and the present application is not limited thereto.
[0040] Here, the binder composition for secondary batteries of the present application is used to form an electrode layer formed on the current collector of the electrode, or to form a functional layer formed on the electrode layer (i.e., on the electrode active material layer) and on the diaphragm substrate. In addition, the slurry composition for secondary batteries of the present application contains the binder composition for secondary batteries of the present application, which is used as a material for preparing the functional layer for secondary batteries of the present application and the electrode layer for secondary batteries of the present application. In addition, the functional layer for secondary batteries of the present application is prepared using the slurry composition for secondary batteries of the present application, constituting a part of, for example, a diaphragm or an electrode. The electrode layer for secondary batteries of the present application is prepared using the slurry composition for secondary batteries of the present application, constituting a part of an electrode. Moreover, the secondary battery of the present application has a functional layer for secondary batteries or an electrode layer for secondary batteries of the present application.
[0041] Binder composition for secondary battery
[0042] The binder composition for secondary batteries of the present application is characterized in that it comprises a polymer A and an arbitrary component B, wherein the polymer A comprises an N-vinyl pyrrolidone monomer unit and a carboxylate-containing monomer unit having an alkenyl chain with 3 to 15 carbon atoms, and the mass content of the carboxylate-containing monomer unit having an alkenyl chain in the polymer A is 25 wt% to 50 wt%.
[0043] By using the secondary battery binder composition of the present application, a gel-resistant secondary battery slurry composition can be prepared, and the operability of the functional layer or electrode layer formed using the secondary battery slurry composition can be improved. In addition, the polymer A in the secondary battery binder composition of the present application has excellent adhesion, so the secondary battery binder composition of the present application can also be used as any one of the electrode binder composition and the functional layer binder composition. Hereinafter, for the secondary battery binder composition of the present application, the case where the secondary battery binder composition is used to form an electrode layer and a functional layer is cited as an example for explanation.
[0044] Polymer A
[0045] The polymer A comprises an N-vinyl pyrrolidone monomer unit and a carboxylate-containing monomer unit having an alkenyl chain with a carbon number of 3-15, and may optionally further comprise monomer units other than the N-vinyl pyrrolidone monomer unit and the carboxylate-containing monomer unit having an alkenyl chain with a carbon number of 3-15. By having such a monomer composition, the polymer A can prepare a gel-resistant secondary battery slurry composition. In addition, the functional layer or electrode layer comprising the polymer A having such a monomer composition has excellent operability.
[0046] In addition, the polymer A is preferably a water-soluble polymer. When the polymer A is a water-soluble polymer, the viscosity of the slurry composition can be controlled, and a functional layer or electrode layer having a uniform film thickness can be obtained. For example, the polymer A is preferably copolyvidone.
[0047] It should be noted that, in the present application, the polymer A being "water-soluble" means that when 0.5 g of the polymer is dissolved in 100 g of water at 25°C, the insoluble component is less than 0.5%.
[0048] N-vinyl pyrrolidone monomer unit
[0049] The mass content of the N-vinyl pyrrolidone monomer unit in polymer A is 50% or more, more preferably 55% or more, particularly preferably 60% or more, and preferably 75% or less, more preferably 70% or less. By making the content of the N-vinyl pyrrolidone monomer unit in polymer A above the lower limit, the rate of the secondary battery having an electrode or separator formed using the binder composition can be increased. On the other hand, by making the content of the N-vinyl pyrrolidone monomer unit in polymer A below the upper limit, the operability of the functional layer or electrode layer formed using the prepared secondary battery slurry composition can be further improved.
[0050] The content of the N-vinyl pyrrolidone monomer unit in the polymer A (the ratio of the N-vinyl pyrrolidone monomer unit to all monomer units contained in the polymer A) can be measured using a nuclear magnetic resonance (NMR) method such as 1H-NMR.
[0051] Carboxylate-containing monomer units having an alkenyl chain having 3 to 15 carbon atoms
[0052] As carboxylate-containing monomers having an alkenyl chain having 3 to 15 carbon atoms that can form carboxylate-containing monomer units having an alkenyl chain having 3 to 15 carbon atoms, there are, but are not limited to, vinyl acetate, vinyl propionate, vinyl butyrate, vinyl valerate, propylene acetate, butylene acetate, pentyl acetate, propylene propionate, butylene propionate, butylene butyrate, etc. These can be used alone or in combination of two or more in any ratio. Moreover, among these, vinyl acetate is preferred from the viewpoint of affinity for active substances.
[0053] Moreover, the number of carbon atoms of the alkenyl chain in the carboxylate-containing monomer unit needs to be 3 or more, preferably 4 or more, and needs to be 15 or less, preferably 12 or less, more preferably 10 or less, and particularly preferably 9 or less. By making the number of carbon atoms of the alkenyl chain in the carboxylate-containing monomer unit above the above lower limit, the operability of the functional layer or electrode layer formed by the prepared slurry composition for secondary batteries can be further improved. On the other hand, by making the number of carbon atoms of the alkenyl chain in the carboxylate-containing monomer unit below the above upper limit, a gel-resistant slurry composition for secondary batteries can be prepared, and the operability of the functional layer or electrode layer formed by the prepared slurry composition for secondary batteries can be further improved.
[0054] Moreover, the mass content of the carboxylate-containing monomeric unit of the alkenyl chain in polymer A (the proportion of the carboxylate-containing monomeric unit of the alkenyl chain in all the monomeric units contained in polymer A) needs to be more than 20%, preferably more than 25%, more preferably more than 30%, and needs to be less than 50%, preferably less than 45%, more preferably less than 40%. By making the content of the carboxylate-containing monomeric unit of the alkenyl chain in polymer A above the above lower limit, the operability of the functional layer or electrode layer formed using the prepared slurry composition for secondary batteries can be further improved, and in the case where the slurry composition for secondary batteries contains an electrode active material, the surface of the electrode active material can be well covered by the adhesive layer formed by the binder composition for secondary batteries. On the other hand, by making the content of the carboxylate-containing monomeric unit of the alkenyl chain in polymer A below the above upper limit, a gel-resistant slurry composition for secondary batteries can be prepared, and the operability of the functional layer or electrode layer formed using the prepared slurry composition for secondary batteries can be further improved.
[0055] The content of alkenyl chain carboxylate-containing monomer units in polymer A (ratio of alkenyl chain carboxylate-containing monomer units in all monomer units contained in polymer A) can be measured using a nuclear magnetic resonance (NMR) method such as 1H-NMR.
[0056] Furthermore, the amount added during polymerization is substantially consistent with the amount of the monomer units in the polymer.
[0057] Preparation method of polymer A
[0058] The polymer A can be produced by polymerizing a monomer composition containing the above-mentioned monomers in water or an organic solvent. In this case, the content ratio of each monomer in the monomer composition can be determined based on the content (content ratio) of each repeating unit (monomer unit) in the polymer A.
[0059] The polymerization method is not particularly limited, and any method can be used, such as solution polymerization, suspension polymerization, bulk polymerization, emulsion polymerization, etc. Also, any reaction such as ionic polymerization, radical polymerization, and living radical polymerization can be used as the polymerization reaction.
[0060] In addition, the emulsifier, dispersant, polymerization initiator, polymerization aid and other additives used in the polymerization can use those commonly used. The amount of these additives used can also be the amount commonly used. The polymerization conditions can be appropriately adjusted according to the polymerization method and the type of polymerization initiator.
[0061] Properties of polymer A
[0062] The weight average molecular weight of polymer A is preferably more than 5kDa, more preferably more than 800kDa, further preferably more than 10kDa, particularly preferably more than 20kDa, most preferably more than 30kDa, and preferably less than 800kDa, more preferably less than 600kDa, further preferably less than 500kDa, particularly preferably less than 300kDa, and most preferably less than 200kDa. By making the weight average molecular weight of polymer A more than the above lower limit, the bonding strength of the functional layer or electrode layer formed using the binder composition can be improved. On the other hand, by making the weight average molecular weight of polymer A less than the above upper limit, a slurry composition for secondary batteries in which thickening is suppressed can be prepared, and the operability of the functional layer or electrode layer formed using the prepared slurry composition for secondary batteries can be further improved, and, in the case where the slurry composition for secondary batteries includes an electrode active material, the surface of the electrode active material can be well covered by the bonding layer formed by the binder composition for secondary batteries.
[0063] In addition, the "weight average molecular weight" of the polymer A is measured by gel permeation chromatography (GPC).
[0064] Component B
[0065] The component B includes at least one of citrate, tartrate, laurate, myristic acid ester, oleate and stearate.
[0066] The citrate ester includes one or more of tributyl citrate, acetyl tributyl citrate, isopropyl citrate, propylene glycol polyoxyethylene polyoxypropylene ether monoester of citrate, alkyl glycoside monoester of citrate or glycerol stearate citrate. The tartaric acid ester includes one or more of diethyl tartaric acid ester, stearyl tartaric acid ester, lauryl polyoxyethylene ether tartaric acid ester, varenicline tartaric acid ester, diacetyl tartaric acid ester of monoglyceride, and diacetyl tartaric acid ester of diglyceride. The lauric acid ester includes one or more of triglycerol monolaurate, diethylene glycol monolaurate, polyethylene glycol laurate, pentaerythritol monolaurate, sorbitan monolaurate, and decaglycerol monolaurate. The myristic acid ester includes one or more of decaglycerol monomyristate, cholesteryl myristic acid ester, and ascorbyl myristic acid ester. The oleic acid ester includes one or more of triglycerol oleate, pentaerythritol oleate, and epoxidized acrylate soybean oil ester. The stearate includes one or more of glyceryl stearate, glyceryl stearate citrate, propylene glycol stearate, and pentaerythritol stearate.
[0067] By adding component B, component B and polymer A can inhibit the thickening of the secondary battery slurry composition through abundant hydrogen bonding, and prolong the gel time. In addition, the functional layer or electrode layer containing component B has excellent operability. Furthermore, the bonding strength of the functional layer or electrode layer formed using the binder composition can be improved.
[0068] Solvents
[0069] The secondary battery binder composition of the present application may further contain a solvent. The solvent is not particularly limited, and examples of the solvent include water and NMP.
[0070] Other ingredients
[0071] The secondary battery electrode binder composition of the present application may also contain reinforcing materials, leveling agents, viscosity modifiers, electrolyte additives and other components in addition to the above-mentioned components. They are not particularly limited if they do not affect the battery reaction. In addition, these components can be used alone or in combination of two or more in any ratio.
[0072] Preparation method of binder composition for secondary battery
[0073] The preparation method of the secondary battery binder composition of the present application is not particularly limited. For example, when polymer A is a water-soluble polymer, the preparation of polymer A is implemented in an aqueous solvent. When polymer A is obtained in the form of an aqueous solution, the aqueous solution of polymer A can be directly used as a secondary battery binder composition, or any other components can be added to the aqueous solution of polymer A as a secondary battery binder composition. Here, as other components, other components described in the item "slurry composition for secondary batteries" described later can be cited. In addition, the secondary battery binder composition may also contain solvents other than water.
[0074] Slurry composition for secondary battery
[0075] The slurry composition for secondary batteries of the present application can use water as a dispersion medium, for example. In some embodiments, the slurry composition for secondary batteries at least comprises the above-mentioned polymer A, solvent and component B, further contains non-conductive materials and / or electrode active materials, and further contains any other ingredients.
[0076] Furthermore, when the slurry composition for secondary batteries of the present application contains non-conductive fine particles, the functional layer obtained using the slurry composition for secondary batteries of the present application can function well as a porous membrane layer having excellent heat resistance and strength.
[0077] Furthermore, when the slurry composition for secondary batteries of the present application contains an electrode active material, an electrode layer obtained using the slurry composition for secondary batteries of the present application can have excellent flexibility, and a secondary battery using the electrode layer can exhibit excellent rate performance and low-temperature output performance.
[0078] Ratio of the mass of polymer A to the total solid content mass of the slurry composition containing the electrode active material (mass of polymer A / total solid content mass of the slurry composition)
[0079] As the ratio of the mass of polymer A to the total solid content mass of the slurry composition containing the electrode active material (the mass of polymer A / the total solid content mass of the slurry composition), it is preferably 0.1% or more, more preferably 0.3% or more, and preferably 3.0% or less, more preferably 2.0% or less. By making the above ratio above the above lower limit, when the slurry composition contains an electrode active material, the dispersibility of the electrode active material can be prevented from deteriorating. On the other hand, by making the above ratio below the above upper limit, it is possible to prevent the battery cell capacity from decreasing and the battery cell resistance from increasing in the obtained secondary battery.
[0080] Ratio of the mass of component B to the total solid content mass of the slurry composition containing the electrode active material (mass of component B / total solid content mass of the slurry composition)
[0081] The mass of component B is preferably 0.2% or more, more preferably 0.5% or more, and preferably 3.0% or less, more preferably 2.5% or less. By making the above ratio above the above lower limit, the bonding strength of the obtained electrode layer can be improved. On the other hand, by making the above ratio below the above upper limit, the battery cell capacity can be prevented from being reduced and the battery cell resistance from being increased in the obtained secondary battery.
[0082] Ratio of the mass of polymer A to the total solid mass of the slurry composition containing non-conductive fine particles (mass of polymer A / total solid mass of the slurry composition)
[0083] The ratio of the mass of polymer A to the total solid content mass of the slurry composition containing the non-conductive material (the mass of polymer A / the total solid content mass of the slurry composition) is preferably 1.0% or more, more preferably 2.0% or more, particularly preferably 3.0% or more, and preferably 7.0% or less, more preferably 6.0% or less, particularly preferably 5.0% or less. By making the above ratio above the above lower limit, a porous film layer with excellent strength can be formed. On the other hand, by making the above ratio below the above upper limit, a porous film layer with excellent heat resistance can be formed.
[0084] Ratio of the mass of component B to the total solid content mass of the slurry composition containing the non-conductive material (mass of component B / total solid content mass of the slurry composition)
[0085] As the mass of component B relative to the ratio of the total solid content mass of the slurry composition comprising non-conductive material (the total solid content mass of the mass of component B / slurry composition), preferably more than 0.2 mass %, more preferably more than 0.5 mass %, particularly preferably more than 2.0 mass %, and, preferably less than 7.0 mass %, more preferably less than 5.0 mass %, particularly preferably less than 4.0 mass %. By making the above ratio more than the above lower limit, a porous film layer with excellent strength can be formed. On the other hand, by making the above ratio less than the above upper limit, a porous film layer with excellent heat resistance can be formed.
[0086] Non-conductive materials
[0087] The non-conductive material is a material that is insoluble in water, organic solvents, and electrolytes, and is a particle that can maintain its shape even in these. Furthermore, the non-conductive material is electrochemically stable, and therefore exists stably in the functional layer under the use environment of the secondary battery.
[0088] Furthermore, as the non-conductive material, for example, various inorganic fine particles and organic fine particles may be used.
[0089] Specifically, as a non-conductive material, both inorganic particles and organic particles can be used, but inorganic particles are usually used. Among them, as a material of a non-conductive material, it is preferred that the material exists stably and is electrochemically stable under the use environment of a secondary battery. When the preferred examples of non-conductive materials are listed from this point of view, oxide particles such as aluminum oxide, hydrated aluminum oxide (boehmite), silicon oxide, magnesium oxide (magnesia), calcium oxide, titanium oxide (Titania), BaTiO3, ZrO, aluminum oxide-silicon dioxide composite oxides, etc.; Nitride particles such as aluminum nitride and boron nitride; Covalent bond crystal particles such as silicon and diamond; Barium sulfate, calcium fluoride, barium fluoride and other insoluble ionic crystal particles; Talc, montmorillonite and other clay particles, etc. In addition, element replacement, surface treatment, solid solution, etc. can be implemented on these particles as needed.
[0090] The above-mentioned non-conductive material may be used alone or in combination of two or more. Moreover, as the non-conductive material, aluminum oxide is preferred. In addition, the particle size of the non-conductive material is not particularly limited and can be the same as the non-conductive material currently used.
[0091] Ratio of the mass of the non-conductive material to the mass of the total solid content of the slurry composition (mass of the non-conductive material / mass of the total solid content of the slurry composition)
[0092] As the ratio of the mass of the non-conductive material to the total solid content mass of the slurry composition (the mass of the non-conductive material / the total solid content mass of the slurry composition), it is preferably 85% by mass or more, more preferably 87% by mass or more, particularly preferably 91% by mass or more, and preferably 99% by mass or less, more preferably 97% by mass or less. By making the above ratio more than the above lower limit, good heat resistance can be obtained. On the other hand, by making the above ratio less than the above upper limit, good adhesion strength can be given to the functional layer.
[0093] Electrode active material
[0094] The electrode active material is a material that transfers electrons between the electrodes (positive electrode and negative electrode) of a lithium ion battery. In addition, as the electrode active material (positive electrode active material and negative electrode active material) of a lithium ion battery, a material that can absorb and release lithium is generally used.
[0095] Positive active material
[0096] The positive electrode active material may include a compound capable of inserting and extracting lithium, specifically, may include one or more composite oxides of lithium and a metal selected from cobalt, manganese, nickel, and a combination thereof. As a specific example, a compound represented by one of the chemical formulas may be used. Li a A 1-b Xb D2(0.90≤a≤1.8,0≤b≤0.5);Li a A 1-b X b O 2-c D c (0.90≤a≤1.8,0≤b≤0.5,0≤c≤0.05);Li a HAVE BEEN 1-b X b O 2-c D c (0.90≤a≤1.8,0≤b≤0.5,0≤c≤0.05);Li a HAVE BEEN 2-b X b O 4-c D c (0.90≤a≤1.8,0≤b≤0.5,0≤c≤0.05);Li a Ni 1-b-c Co b X c D α (0.90≤a≤1.8,0≤b≤0.5,0≤c≤0.5,0<α≤2);Li a Ni 1-b-c Co b X c O 2-α T α (0.90≤a≤1.8,0≤b≤0.5,0≤c≤0.05,0<α<2);Li a Ni 1-b-c Co b X c O 2-α T2(0.90≤a≤1.8,0≤b≤0.5,0≤c≤0.05,0<α<2);Li a Ni 1-b-c Mr b X c D α (0.90≤a≤1.8,0≤b≤0.5,0≤c≤0.05,0<α≤2);Li a Ni 1-b- c Mr b X c O 2-α T α (0.90≤a≤1.8,0≤b≤0.5,0≤c≤0.05,0<a<2);Li a Ni 1-b-c Mr b X c O 2-αT2 (0.90≤a≤1.8, 0≤b≤0.5, 0≤c≤0.05, 0<α<2); Li a Ni b E c G d O2(0.90≤a≤1.8, 0≤b≤0.9, 0≤c≤0.5, 0.001≤d≤0.1); Li a Ni b Co c Mn d GeO2(0.90≤a≤1.8, 0≤b≤0.9, 0≤c≤0.5, 0≤d≤0.5, 0.001≤e≤0.1); Li a NeG b O2(0.90≤a≤1.8, 0.001≤b≤0.1); Li a CoG b O2(0.90≤a≤1.8, 0.001≤b≤0.1); Li a Mn 1-b G b O2(0.90≤a≤1.8, 0.001≤b≤0.1); Li a Mn b O4(0.90≤a≤1.8, 0.001≤b≤0.1); Li a Mn 1-g G g PO4(0.90≤a≤1.8, 0≤g≤0.5); QO2; QS2; LiQS2; V2O5; LiV2O5; LiZO2; LiNiVO4; Li (3-f) J2(PO4)3(0≤f≤2);Li (3-f) Fe2(PO4)3(0≤f≤2);Li a FePO4(0.90≤a≤1.8).
[0097] In the chemical formula, A is selected from Ni, Co, Mn and combinations thereof; X is selected from Al, Ni, Co, Mn, Cr, Fe, Nb, Mg, Sr, V, rare earth elements and combinations thereof; D is selected from O, F, S, P and combinations thereof; E is selected from Co, Mn and combinations thereof; T is selected from F, S, P and combinations thereof; G is selected from Al, Cr, Mn, Fe, Nb, Mg, La, Ce, Sr, V and combinations thereof; Q is selected from Ti, Mo, Mn and combinations thereof; Z is selected from Cr, V, Fe, Sc, Y and combinations thereof; J is selected from V, Cr, Mn, Co, Ni, Cu and combinations thereof.
[0098] The compound may have a coating layer on the surface, or may be mixed with another compound having a coating layer. The coating layer may include at least one coating element compound selected from an oxide of a coating element, a hydroxide of a coating element, an oxyhydroxide of a coating element, an oxycarbonate of a coating element, and a hydroxycarbonate of a coating element. The compound for the coating layer may be amorphous or crystalline. The coating element included in the coating layer may include Mg, Al, Co, K, Na, Ca, Si, Ti, V, Sn, Ge, Ga, B, As, Nb, Zr, or a mixture thereof. The coating layer may be provided by using these elements in the compound and by a method that has no negative impact on the properties of the positive active material, for example, the method may include any coating method (e.g., spraying, dipping, etc.), but since it is well known to those skilled in the relevant art, it is not described in more detail.
[0099] Negative active material
[0100] As the negative electrode active material, a material that can reversibly intercalate and deintercalate lithium ions, lithium metal, a lithium metal alloy, a material that can be doped and dedoped with lithium, or a transition metal oxide can be used.
[0101] The material that reversibly intercalates / deintercalates lithium ions may include carbon materials, i.e., carbon-based negative electrode active materials conventionally used in rechargeable lithium batteries. Examples of carbon-based negative electrode active materials may include crystalline carbon, amorphous carbon, or mixtures thereof. Crystalline carbon may be amorphous (no specific shape), plate-like, flaky, spherical, or fibrous natural graphite or artificial graphite. Amorphous carbon may be soft carbon, hard carbon, mesophase pitch carbonization product, sintered coke, etc.
[0102] Lithium metal alloys include alloys of lithium with a metal selected from Na, K, Rb, Cs, Fr, Be, Mg, Ca, Sr, Si, Sb, Pb, In, Zn, Ba, Ra, Ge, Al and Sn.
[0103] The materials that can be doped / dedoped with lithium can be Si, SiO x(0<x<2), Si-Q alloy (wherein Q is an element selected from alkali metals, alkaline earth metals, group 13 elements, group 14 elements, group 15 elements, group 16 elements, transition metals, rare earth elements and combinations thereof, but not Si), Si-carbon composites, Sn, SnO2, Sn-R alloy (wherein R is an element selected from alkali metals, alkaline earth metals, group 13 elements, group 14 elements, group 15 elements, group 16 elements, transition metals, rare earth elements and combinations thereof, but not Sn), Sn-carbon composites, etc., and at least one of these materials may be mixed with SiO2. Elements Q and R can be selected from Mg, Ca, Sr, Ba, Ra, Sc, Y, Ti, Zr, Hf, Rf, V, Nb, Ta, Db, Cr, Mo, W, Sg, Tc, Re, Bh, Fe, Pb, Ru, Os, Hs, Rh, Ir, Pd, Pt, Cu, Ag, Au, Zn, Cd, B, Al, Ga, Sn, In, Ge, P, As, Sb, Bi, S, Se, Te, Po and combinations thereof.
[0104] Transition metal oxides include lithium titanium oxide.
[0105] Ratio of the mass of the electrode active material to the mass of the total solid content of the slurry composition (mass of the electrode active material / mass of the total solid content of the slurry composition)
[0106] As the ratio of the mass of the electrode active material to the total solid content mass of the slurry composition (the mass of the electrode active material / the total solid content mass of the slurry composition), it is preferably 90% by mass or more, more preferably 92% by mass or more, particularly preferably 97% by mass or more, and preferably 99% by mass or less, more preferably 98% by mass or less. By making the above ratio above the above lower limit, it is possible to prevent the battery cell capacity in the obtained secondary battery from being reduced. On the other hand, by making the above ratio below the above upper limit, it is possible to increase the rate of the obtained secondary battery.
[0107] Other ingredients
[0108] The secondary battery slurry composition may include other arbitrary components in addition to the above-mentioned components. The above-mentioned arbitrary components are not particularly limited as long as they do not have an excessively adverse effect on the battery reaction in the secondary battery containing the functional layer and the electrode layer. In addition, the type of the above-mentioned arbitrary components may be one or more.
[0109] Examples of the optional components include a particulate binder, a wetting agent, a leveling agent, and an electrolyte decomposition inhibitor.
[0110] Preparation of slurry composition for secondary battery
[0111] The above-mentioned slurry composition for secondary batteries can be prepared by dispersing the above-mentioned components in a dispersion medium, and the dispersion medium is preferably an aqueous medium. Specifically, the slurry composition for secondary batteries can be prepared by mixing the above-mentioned components and the dispersion medium using a ball mill, a sand mill, a bead mill, a pigment disperser, a grinder, an ultrasonic disperser, a homogenizer, a planetary mixer, a mixer such as Filmix. Here, from the viewpoint of being able to apply high dispersion shear, a high dispersion device such as a bead mill, a roller mill, and Filmix can be used. In addition, the mixing of the above-mentioned components and the dispersion medium (e.g., an aqueous medium) can usually be carried out in the range of room temperature to 80°C for 10 minutes to several hours.
[0112] Here, water is generally used as the aqueous medium, but an aqueous solution of any compound, a mixed solution of a small amount of an organic solvent and water, etc. may also be used. In addition, the water used as the aqueous medium may also include water contained in the binder composition.
[0113] Functional layer for secondary batteries
[0114] The functional layer for secondary battery of the present application is formed by the above-mentioned slurry composition for secondary battery containing non-conductive microparticles, and can be formed by, for example, the following method: after the above-mentioned slurry composition for secondary battery is applied on the surface of a suitable substrate to form a coating film, the formed coating film is dried. That is, the functional layer for secondary battery of the present application is formed by the dried product of the above-mentioned slurry composition for secondary battery, and usually contains the above-mentioned polymer A, the above-mentioned non-conductive microparticles, and can further include the above-mentioned other components added arbitrarily.
[0115] In addition, the abundance ratio of each component (excluding dispersion medium such as water) contained in the functional layer for secondary batteries of the present application is generally the same as the abundance ratio of each component contained in the above-mentioned slurry composition for secondary batteries, and the preferred abundance ratio of each component in the functional layer for secondary batteries is also the same as the preferred abundance ratio of each component in the above-mentioned slurry composition for secondary batteries.
[0116] Moreover, the functional layer for secondary battery of the present application is formed by the slurry composition for secondary battery of the present application, so it also functions well as a porous membrane layer with excellent heat resistance and strength. In addition, the functional layer for secondary battery of the present application can improve the battery characteristics such as rate and low temperature output of the secondary battery.
[0117] Substrate
[0118] There is no particular limitation on the substrate for forming the functional layer for secondary batteries. For example, when the functional layer for secondary batteries is used as a component constituting a part of the diaphragm, the diaphragm substrate can be used as the substrate. In addition, when the functional layer is used as a component constituting a part of the electrode, the electrode substrate formed by forming the electrode layer on the current collector can be used as the substrate. In addition, there is no particular limitation on the usage of the functional layer formed on the substrate. For example, the functional layer can be formed on the diaphragm substrate and used directly as a battery component such as a diaphragm, the functional layer can be formed on the electrode substrate and used as an electrode, and the functional layer formed on the demoulding substrate can be peeled off from the substrate at one time and pasted on other substrates as a battery component.
[0119] However, from the viewpoint of omitting the step of peeling the functional layer from the release substrate and improving the production efficiency of the battery module, it is preferred to use a separator substrate or an electrode substrate as the substrate.
[0120] Diaphragm substrate
[0121] As the diaphragm substrate, there is no particular limitation, for example, it can be a known diaphragm substrate such as an organic diaphragm substrate. The organic diaphragm substrate is a porous member formed of an organic material, and the organic diaphragm substrate includes but is not limited to microporous membranes containing polyolefin resins such as polyethylene and polypropylene, aromatic polyamide resins, etc., and is preferably a microporous membrane made of polyethylene because of its excellent strength. In addition, the thickness of the organic diaphragm can be any thickness, usually 0.5 μm or more, preferably 5 μm or more, usually 40 μm or less, preferably 30 μm or less, and more preferably 20 μm or less.
[0122] Electrode substrate
[0123] The electrode substrate (positive electrode substrate and negative electrode substrate) is not particularly limited, and examples thereof include an electrode substrate in which an electrode layer is formed on a current collector.
[0124] Here, the electrode active material (positive electrode active material, negative electrode active material) in the current collector and the electrode layer and the electrode layer binding material (positive electrode composite material layer binding material, negative electrode composite material layer binding material) and the electrode layer to the current collector The formation method can use known substances and methods. In addition, as an electrode layer binding material, the polymer A included in the secondary battery binder composition of the present application can also be used.
[0125] Release substrate
[0126] The release substrate for forming the functional layer is not particularly limited, and a known release substrate can be used.
[0127] Method for forming functional layer for secondary battery
[0128] As a method for forming a functional layer on the above-mentioned substrate such as a separator substrate and an electrode substrate, the following methods can be cited:
[0129] 1) applying the slurry composition for secondary battery on the surface of the separator substrate or the electrode substrate, and then drying;
[0130] 2) After the separator substrate or the electrode substrate is immersed in the slurry composition for secondary batteries, it is dried;
[0131] 3) The slurry composition for secondary batteries is applied on a release substrate and dried to produce a functional layer, and the obtained functional layer for secondary batteries is transferred to a separator substrate or an electrode substrate.
[0132] Among these, the method 1) is particularly preferred because it is easy to control the film thickness of the functional layer for secondary batteries. The method 1) includes the following steps in detail: a step of applying the slurry composition for secondary batteries on a diaphragm substrate or an electrode substrate (coating step), and a step of drying the slurry composition for secondary batteries applied on the diaphragm substrate or the electrode substrate to form a functional layer (functional layer forming step).
[0133] Coating process
[0134] In the coating step, the method for coating the slurry composition for secondary batteries on the substrate is not particularly limited, and examples thereof include doctor blade method, reverse roll method, direct roll method, gravure printing method, extrusion method, brush coating method and the like.
[0135] Functional layer forming process
[0136] In addition, in the functional layer forming step, the method for drying the secondary battery slurry composition on the substrate is not particularly limited, and a known method can be used, such as drying using warm air, hot air, or low-humidity air; vacuum drying; and drying using irradiation of infrared rays, electron beams, etc. There are no particular limitations on the drying conditions, but the drying temperature is preferably 50 to 100° C., and the drying time is preferably 5 to 30 minutes.
[0137] In addition, the thickness of the secondary battery functional layer formed on the substrate can be adjusted appropriately.
[0138] Electrode layer for secondary battery
[0139] The electrode layer for secondary battery of the present application is a layer formed by the above-mentioned slurry composition for secondary battery containing electrode active material, which can be formed by, for example, the following method: after the above-mentioned slurry composition for secondary battery is applied on the surface of an appropriate current collector to form a coating film, the formed coating film is dried. That is, the electrode layer for secondary battery of the present application is formed by the dried product of the above-mentioned slurry composition for secondary battery, usually containing the above-mentioned polymer A, the above-mentioned electrode active material, and further containing the above-mentioned other components added arbitrarily.
[0140] In addition, the abundance ratio of each component (except dispersion medium such as water) contained in the electrode layer for secondary batteries of the present application is generally the same as the abundance ratio of each component contained in the above-mentioned slurry composition for secondary batteries, and the preferred abundance ratio of each component in the electrode layer for secondary batteries is also the same as the preferred abundance ratio of each component in the above-mentioned slurry composition for secondary batteries.
[0141] Furthermore, the electrode layer for a secondary battery of the present application is formed of the slurry composition for a secondary battery of the present application, and therefore has high flexibility and can enable the secondary battery to exhibit excellent rate and low-temperature output.
[0142] Method for forming electrode layer for secondary battery
[0143] The method for forming an electrode layer for a secondary battery of the present application includes, for example, the following steps: coating the above-mentioned slurry composition for a secondary battery on a current collector (coating step); and drying the slurry composition for a secondary battery coated on the current collector to form an electrode layer on the current collector (drying step).
[0144] Coating process
[0145] As a method for coating the above-mentioned secondary battery slurry composition on the current collector, there is no particular limitation, and a known method can be used. Specifically, as a coating method, a doctor blade method, an immersion method, a reverse roller method, a direct roller method, a gravure printing method, an extrusion method, a brush coating method, etc. can be used. At this time, the slurry composition can be coated only on one side of the current collector, or it can be coated on both sides. The thickness of the slurry film on the current collector before drying after coating can be appropriately set according to the thickness of the electrode layer obtained by drying.
[0146] Here, as a current collector for coating the slurry composition for secondary batteries, a material having conductivity and electrochemical durability can be used. Specifically, as a current collector, a current collector formed of, for example, iron, copper, aluminum, nickel, stainless steel, titanium, tantalum, gold, platinum, etc. can be used. Among them, as a current collector for the negative electrode, copper foil is particularly preferred. In addition, as a current collector for the positive electrode, aluminum foil is particularly preferred. In addition, the above-mentioned materials can be used alone or in combination of two or more in any ratio.
[0147] Drying process
[0148] The method for drying the slurry composition for secondary batteries on the current collector is not particularly limited, and a known method can be used, such as drying using warm air, hot air, or low-humidity air; vacuum drying; and drying using irradiation with infrared rays, electron beams, etc. By drying the slurry composition for secondary batteries on the current collector in this way, an electrode layer can be formed on the current collector, and a secondary battery electrode having a current collector and an electrode layer can be obtained.
[0149] In addition, after the drying step, the electrode layer can be subjected to a pressurization process (pressing process) by using a mold press or a roll press. By the press process, the adhesion between the electrode layer and the current collector can be improved. In addition, the electrode layer can be made high-densified, and the secondary battery can be miniaturized.
[0150] Secondary battery
[0151] The secondary battery of the present application has the above-mentioned secondary battery functional layer of the present application and / or the secondary battery electrode layer of the present application. More specifically, the secondary battery of the present application has a positive electrode, a negative electrode, a separator and an electrolyte, and the above-mentioned secondary battery functional layer and / or the secondary battery electrode layer are included in at least one of the positive electrode, the negative electrode and the separator as a battery component.
[0152] Since the secondary battery of the present application includes the secondary battery functional layer or the secondary battery electrode layer of the present application, it is possible to provide a secondary battery having the secondary battery functional layer or the secondary battery electrode layer having excellent handleability.
[0153] Positive electrode, negative electrode and separator
[0154] At least one of the positive electrode, negative electrode and separator used in the secondary battery of the present application has a functional layer for a secondary battery or an electrode layer for a secondary battery. Specifically, as a positive electrode and a negative electrode having a functional layer for a secondary battery, an electrode formed by arranging a functional layer on an electrode substrate can be used, and the electrode substrate is an electrode substrate formed by forming an electrode layer as an electrode layer for a secondary battery on a current collector. In addition, as a separator having a functional layer for a secondary battery, a separator formed by arranging a functional layer for a secondary battery on a separator substrate can be used. In addition, as an electrode substrate and a separator substrate, the same substrates as those listed in the item "substrate" can be used. As a positive electrode and a negative electrode having an electrode layer for a secondary battery, an electrode formed by forming an electrode layer as an electrode layer for a secondary battery on a current collector can be used.
[0155] Positive electrode, negative electrode
[0156] As described above, if at least one of the positive electrode, negative electrode and separator used in the secondary battery has the functional layer for the secondary battery or the electrode layer for the secondary battery of the present application, the negative electrode can be a known negative electrode, the positive electrode can be a known positive electrode, and the positive electrode and negative electrode of the secondary battery can be respectively known electrodes.
[0157] Diaphragm
[0158] As the separator, a microporous membrane composed of a polyolefin resin (polyethylene, polypropylene, polybutylene, polyvinyl chloride) is preferred because the overall thickness of the separator can be reduced, thereby increasing the ratio of the electrode active material in the lithium ion secondary battery and increasing the capacity per unit volume.
[0159] Electrolyte
[0160] As the electrolyte, an organic electrolyte in which a supporting electrolyte is dissolved in an organic solvent can generally be used. As the supporting electrolyte, for example, a lithium salt can be used in a lithium ion secondary battery. As the lithium salt, for example, LiPF6, LiAsF6, LiBF4, LiSbF6, LiAlCl4, LiClO4, CF3SO3Li, C4F9SO3Li, CF3COOLi, (CF3CO)2NLi, (CF3SO2)2NLi, (C2F5SO2)NLi, etc. can be cited. Among them, LiPF6, LiClO4, and CF3SO3Li are preferred because they are easily dissolved in a solvent and show a high degree of dissociation. In addition, the electrolyte can be used alone or in combination of two or more. Because there is generally a tendency that the higher the degree of dissociation of the supporting electrolyte, the higher the lithium ion conductivity, the lithium ion conductivity can be adjusted according to the type of supporting electrolyte.
[0161] As an organic solvent used in the electrolyte, as long as it can dissolve the supporting electrolyte, there is no particular limitation. For example, in lithium-ion secondary batteries, carbonates such as dimethyl carbonate (DMC), ethylene carbonate (EC), diethyl carbonate (DEC), propylene carbonate (PC), butylene carbonate (BC), and ethyl methyl carbonate (EMC) can be preferably used; esters such as γ-butyrolactone, methyl formate, ethyl acetate, propyl propionate, and ethyl propionate; ethers such as 1,2-dimethoxyethane and tetrahydrofuran; sulfur-containing compounds such as cyclopentane and dimethyl sulfoxide, etc. In addition, a mixed solution of these solvents can also be used. Among them, carbonates are preferred because of their high dielectric constant and wide stable potential region. Because there is usually a tendency that the lower the viscosity of the solvent used, the higher the lithium ion conductivity, the lithium ion conductivity can be adjusted according to the type of solvent.
[0162] In addition, the concentration of the electrolyte in the electrolytic solution can be adjusted appropriately.
[0163] In addition, at least one of 1,3-propane sultone, vinyl sulfate or methylene disulfonate can be preferably added to the electrolyte. Based on the weight of the electrolyte, the content of 1,3-propane sultone, vinyl sulfate or methylene disulfonate is 0.1% to 3%. When at least one of 1,3-propane sultone (PS), vinyl sulfate (DTD) and methylene disulfonate (MMDS) is added to the electrolyte, the decomposition reaction of polymer A during the charge and discharge process can be suppressed, thereby not only improving the rate of the secondary battery, but also improving the low temperature output performance.
[0164] Method for manufacturing secondary battery
[0165] The secondary battery can be manufactured, for example, by overlapping the positive electrode and the negative electrode through a separator, winding and folding them as needed and placing them in a battery container, injecting an electrolyte into the battery container, and sealing it. In addition, at least one of the positive electrode, the negative electrode, and the separator is a component having a functional layer for a secondary battery or an electrode layer for a secondary battery of the present application. Here, in the battery container, metal mesh, fuses, PTC elements, and other overcurrent protection elements, guide plates, etc. can also be placed as needed to prevent the pressure inside the battery from rising and overcharging and discharging. The shape of the battery can be, for example, any one of a coin type, a button type, a sheet type, a cylindrical type, a square type, a flat type, etc.
[0166] Electronic devices
[0167] The present application also provides an electronic device, which includes the secondary battery.
[0168] The electronic device may be, for example, a laptop computer, a tablet computer, an electric toy, a smart phone, etc. Among them, the electric toy may include a fixed or mobile electric toy, such as a game console, an electric car toy, an electric ship toy, an electric airplane toy, etc. It is understandable that the electronic device is not limited thereto, and may also be an electric device with a power battery, for example, an electric vehicle, such as an electric bicycle, an electric motorcycle, an electric car, etc.
[0169] Example
[0170] Hereinafter, the present application will be specifically described based on Examples, but the present application is not limited to these Examples. It should be noted that in the following description, "%" and "part" indicating an amount are based on mass unless otherwise specified.
[0171] In addition, unless otherwise specified, in a polymer produced by copolymerizing multiple monomers, the proportion of repeating units (monomer units) formed by polymerizing a certain monomer in the above-mentioned polymer is generally consistent with the ratio (such as input ratio) of the certain monomer in all monomers used to polymerize the polymer.
[0172] In the examples and comparative examples, (1) storage stability of the slurry composition, (2) positive electrode bonding strength, (3) positive electrode flexibility, (4) blocking resistance of the separator, and (5) rate characteristics of the secondary battery were measured and evaluated by the following methods.
[0173] (1) Storage stability of slurry composition
[0174] The viscosity of 100g of the prepared slurry composition at 25°C was measured as the initial viscosity. The viscosity of the above-mentioned slurry composition after being stored at 25°C for 3 days was measured as the later viscosity. Using a B-type viscometer ("BL" manufactured by Toki Industry), the slurry composition was fully stirred with a spatula at a temperature of 25°C, and then immediately measured at a B-type viscometer rotor rotation speed of 6rpm, and then measured at 60rpm, and the viscosity measured at 60rpm was used as the initial viscosity.
[0175] The storage stability judgment standard is to compare the later viscosity with the initial viscosity. The A, B, C, and D in the storage stability column in Table 1 represent:
[0176] A: Same as the initial stage
[0177] B: Slight change in viscosity
[0178] C: Viscosity increased but no gelation occurred
[0179] D: Gelation occurred
[0180] (2) Positive electrode bonding strength
[0181] The bonding strength is measured in the form of peel strength. Cut the positive electrode into rectangles of 1 cm in width and 10 cm in length, and fix the obtained test piece with the positive electrode composite material layer facing upward. After sticking a transparent tape on the surface of the positive electrode composite material layer of the fixed test piece, peel off the transparent tape from one end of the test piece in a direction of 180° at a speed of 50 mm / min, and measure the stress during peeling. Carry out the same measurement 5 times, and take the average value as the peel strength, and judge the bonding strength using the following criteria. The greater the peel strength, the higher the bonding strength. A, B, C, and D in the positive electrode bonding strength column in Table 1 represent:
[0182] A: Peel strength is 60N / m or more
[0183] B: Peel strength is 50 N / m or more and less than 60 N / m
[0184] C: Peel strength is 40 N / m or more and less than 50 N / m
[0185] D: Peel strength less than 40N / m
[0186] (3) Positive electrode flexibility
[0187] The flexibility index is an indicator of the softness of the electrode. The larger the flexibility index, the softer the electrode. When the flexibility index is large, the positive electrode or negative electrode contained in the wound electrode body is prone to buckling after the rolled body is pressed. On the other hand, when the flexibility index is small, the positive electrode contained in the wound electrode body is too hard, and cracks are easily generated. The flexibility index of the positive electrode is determined by the following steps:
[0188] (1) A positive electrode having a width of 50 mm and a length of 100 mm was wound around a core rod having a diameter of 5 mm and kept there for 60 seconds.
[0189] (2) When the positive electrode is released with the core rod facing up and down, the positive electrode plate 30 rebounds and moves away from the core rod.
[0190] (3) The value after removing the unit (mm) from the inner diameter of the positive electrode after rebounding is used as the flexibility index of the positive electrode. Here, the inner diameter of the positive electrode refers to the length of the diameter of the positive electrode farthest from the center of the mandrel and the center of the mandrel when the positive electrode is wound around the mandrel from the inner end of the roll. A, B, C, and D in the column of positive electrode flexibility in Table 1 represent:
[0191] A: Flexibility index is above 30
[0192] B: Flexibility index is 20 or more and less than 30
[0193] C: Flexibility index is 10 or more and less than 20 N / m
[0194] D: Flexibility index is less than 10
[0195] (4) Diaphragm adhesion resistance
[0196] The separator with the functional layer and the separator without the functional layer were cut into square pieces of 5 cm in width and 5 cm in length. Two pieces of the separator with the functional layer and the separator without the functional layer were stacked with the functional layer sandwiched between them and placed at 40°C and 10 g / cm 2 The test sample was prepared under pressure. The obtained test sample was further placed for 24 hours. In the test sample after being placed for 24 hours, one of the overlapping diaphragms was fixed, and the other was stretched with a force of 2N / m to confirm whether it could be peeled off. The bonding state (adhesion state) was evaluated using the following criteria. The less adhesion was observed, the better the adhesion resistance. A, B, and C in the column of diaphragm adhesion resistance in Table 1 represent:
[0197] A: Overlapping diaphragms are not bonded to each other
[0198] B: Overlapping diaphragms peel off from each other
[0199] C: Overlapping separators adhere to each other without peeling off
[0200] (5) Rate characteristics
[0201] After injecting the electrolyte into the prepared lithium-ion secondary battery, let it stand at a temperature of 25°C for 5 hours. Then, charge it by a constant current method at a temperature of 25°C and 0.2C until the battery cell voltage is 3.65V, and then age it at a temperature of 60°C for 12 hours. Then, discharge it by a constant current method at a temperature of 25°C and 0.2C until the battery cell voltage is 3.00V. Then, perform CC-CV charging by a constant current of 0.2C (the upper limit battery cell voltage is 4.60V), and perform CC discharge by a constant current of 0.2C until the battery cell voltage is 3.00V. Repeat the 0.2C charge and discharge three times.
[0202] Next, the battery cell voltage is between 4.60-3.00V and the constant current charge and discharge is performed at 0.2C in an environment with a temperature of 25°C, and the discharge capacity at this time is defined as C0. Then, CC-CV charging is also performed at a constant current of 0.2C, and discharge is performed to 2.5V at a constant current of 0.5C in an environment with a temperature of -10°C. The discharge capacity at this time is defined as C1. Then, the capacity retention rate represented by ΔC = (C1 / C0) × 100 (%) is calculated as the rate characteristic, and evaluated according to the following criteria. The larger the value of the capacity retention rate ΔC, the higher the high current discharge capacity in a low temperature environment and the lower the internal resistance. A, B, C, and D in the rate characteristics column in Table 1 represent:
[0203] A: Capacity retention rate ΔC is more than 95%
[0204] B: Capacity retention rate ΔC is 90% or more and less than 95%
[0205] C: Capacity retention rate ΔC is 80% or more and less than 90%
[0206] D: Capacity retention rate ΔC is less than 80%
[0207] (6) Output characteristics
[0208] After the manufactured lithium-ion secondary battery is left to stand at 25°C for 24 hours, it is charged at 0.1C for 5 hours at 25°C, and the voltage V0 at this time is measured. After that, it is discharged at a discharge rate of 1C at -20°C, and the voltage V1 is measured 15 seconds after the start of discharge. Then, the voltage change ΔV (= V0-V1) is calculated and evaluated according to the following criteria. The smaller the voltage change ΔV, the better the low-temperature output characteristics of the secondary battery. A, B, C, and D in the output characteristics column in Table 1 represent:
[0209] A: Voltage change ΔV is less than 250mV
[0210] B: Voltage change ΔV is greater than 250mV and less than 400mV
[0211] C: Voltage change ΔV is greater than 400mV and less than 500mV
[0212] D: Voltage change ΔV is more than 500mV
[0213] Example 1
[0214] Preparation of battery positive electrode:
[0215] (1) Preparation of a slurry composition for a positive electrode composite material layer: Add 97 parts of lithium cobalt oxide (positive electrode active material), 1 part of acetylene black (conductive material), 1 part of polyvinylidene fluoride (binder), and 1 part (equivalent solid content) of polymer A to a double planetary mixer with a disperser, and then add N-methyl-2-pyrrolidone (dispersion medium) to make the total solid content concentration become 67%, and mix to obtain a slurry composition for a positive electrode composite material layer; wherein the polymer A used in this embodiment is a copolymer of N-vinyl pyrrolidone and vinyl acetate, wherein the number of carbon atoms of the alkenyl chain on the carboxylate group repeating unit is 4, and the mass content of the carboxylate group repeating unit is 30%, and the polymer A is recorded as P01;
[0216] (2) Use a coating machine to apply the slurry composition for the positive electrode composite material layer at a coating amount of 20±0.5 mg / cm 2 The aluminum foil is coated on the current collector in a manner of 9 μm thick.
[0217] (3) The coated aluminum foil was transported in an oven at a temperature of 90° C. for 2 minutes at a speed of 200 mm / min, and then transported in an oven at a temperature of 120° C. for 2 minutes to dry the slurry on the aluminum foil, thereby obtaining a positive electrode raw material having a positive electrode composite material layer formed on the current collector;
[0218] (4) The positive electrode composite material layer of the prepared positive electrode raw material was roll-pressed at a temperature of 25±3°C and a linear pressure of 70 t (tons) to obtain a positive electrode composite material layer with a density of 4.20 g / cm 3 The positive electrode was then placed in an environment with a temperature of 25±3°C and a relative humidity of 50±5% for 1 week.
[0219] The obtained slurry composition for positive electrode composite material layer and positive electrode were evaluated by the above-mentioned method.
[0220] Preparation of battery negative electrode:
[0221] (1) Preparation of a slurry composition for a negative electrode composite material layer: 97 parts of artificial graphite (negative electrode active material), 1 part of carboxymethyl cellulose (thickener) and 2 parts of styrene-butadiene rubber (binder) were added to a planetary mixer, and the solid content concentration was diluted to 60% with ion exchange water, and then stirred at a speed of 45 rpm for 60 minutes, and then stirred at a speed of 40 rpm for 40 minutes to obtain a slurry composition for a negative electrode composite material layer; in this embodiment, the slurry composition for the negative electrode composite material layer does not use polymer A;
[0222] (2) The above-mentioned slurry composition for negative electrode composite material layer was applied in an amount of 11±0.5 mg / cm 2 The surface of a 5 μm thick copper foil as a current collector was coated in a manner.
[0223] (3) The copper foil coated with the slurry composition for the negative electrode composite material layer is then conveyed in an oven at 80°C for 2 minutes at a speed of 400 mm / min, and then conveyed in an oven at 110°C for 2 minutes to dry the slurry composition on the copper foil, thereby obtaining a negative electrode raw material for forming a negative electrode composite material layer on the current collector.
[0224] (4) The negative electrode composite material layer side of the prepared negative electrode raw material was roll-pressed at a temperature of 25±3°C and a linear pressure of 50 t (tons) to obtain a negative electrode composite material layer with a density of 1.70 g / cm 3 of the negative electrode.
[0225] Separator: A single-layer polyethylene separator (width 65 mm, length 500 mm, thickness 7 μm; manufactured by dry process; porosity 45%) was used as the separator of the secondary battery of this example. The separator was cut into 5 cm×5 cm squares for later use.
[0226] Preparation of secondary batteries:
[0227] The aluminum-plastic film is used as the outer packaging of the battery, the positive electrode is cut into a 4cm×4cm square, and the surface of the current collector side is arranged in contact with the aluminum-plastic film outer packaging; the separator is arranged on the surface of the positive electrode composite material layer of the positive electrode. The negative electrode is cut into a 4.2cm×4.2cm square, and the surface of the negative electrode composite material layer is arranged on the separator in a manner that the surface is opposite to the separator; a 12.5% LiPF6 solution is filled as an electrolyte, and the electrolyte solvent is a mixed solvent of ethylene carbonate (EC) / diethyl carbonate (DEC) / propyl propionate = 1 / 2 / 2 (mass ratio), which contains 2% by mass (solvent ratio) of fluoroethylene carbonate; the opening of the aluminum-plastic film is heat-sealed at 150°C to obtain a laminated battery unit type lithium ion secondary battery.
[0228] Example 2-13
[0229] The difference between Example 2-13 and Example 1 is that the addition of polymer A, component B and other electrolyte additives used in Example 2-13 is changed as shown in Table 1. In addition, the same method as Example 1 is used to prepare a slurry composition for a secondary battery, prepare a diaphragm, and manufacture a negative electrode, a positive electrode and a secondary battery. Then, various evaluations are performed in the same manner as Example 1. When polymer A and component B are used at the same time, the mass ratio of the two is 2:1. The mass content of other electrolyte additives and fluoroethylene carbonate are calculated based on the total weight of the electrolyte.
[0230] Embodiment 14
[0231] 94 parts of aluminum oxide (non-conductive fine particles) having a volume average particle size of 0.5 μm, 3 parts of sodium carboxymethyl cellulose (dispersant) and water are mixed, wherein the amount of water added is adjusted so that the solid content concentration in the mixed system is controlled at 50%; the mixture is treated using a medium-free dispersion device to disperse the aluminum oxide to obtain a slurry; 3.0 parts (equivalent to the solid content) of polymer A (P01) are added to the obtained slurry to obtain a slurry composition for a secondary battery;
[0232] The prepared slurry composition for secondary battery was sealed in a polyethylene container and allowed to stand for 30 days, and then a stirring paddle was inserted into the polyethylene container and stirred at a speed of 250 rpm. After no adherent material at the bottom of the container was visually confirmed, stirring was continued for 30 minutes to redisperse the non-conductive particles therein;
[0233] The slurry composition for secondary battery is coated on the separator: a single-layer polyethylene substrate (width 250mm, length 1000m, thickness 7μm) manufactured by a wet method is prepared, and then the slurry composition for secondary battery is coated on the separator substrate with a gravure coating machine (coating speed: 20m / min) in a manner that the thickness after drying is 2.5μm; the coated separator substrate is dried in a drying oven at 50°C and wound to obtain a separator having a functional layer formed on the separator substrate. The separator is cut into 5cm×5cm squares for preparing lithium-ion secondary batteries.
[0234] Embodiment 15
[0235] The only difference between Example 15 and Example 14 is that 3.0 parts (solid content equivalent) of polymer A (P01) is replaced with 2.0 parts (solid content equivalent) of polymer A (P01) and 1.0 part of component B (B01). Other than this, the same procedures as in Example 14 were followed, and various evaluations were performed in the same manner as in Example 14.
[0236] Comparative Examples 1-5
[0237] The difference between Comparative Examples 1-5 and Example 1 is that the addition of polymer A, component B and other electrolyte additives used in Comparative Examples 1-5 is changed as shown in Table 1. Otherwise, the same method as Example 1 is used to prepare a slurry composition for a secondary battery, prepare a diaphragm, and manufacture a negative electrode, a positive electrode and a secondary battery. Then, various evaluations are performed in the same manner as Example 1. When polymer A and component B are used at the same time, the mass ratio of the two is 2:1. The mass content of other electrolyte additives and fluoroethylene carbonate are calculated based on the total weight of the electrolyte.
[0238] The slurry compositions for secondary batteries and the secondary batteries prepared in Examples 1-13 and Comparative Examples 1-5 were tested for relevant performance, and the diaphragms coated with the functional layers prepared in Examples 14-15 were tested for relevant performance. The test results are shown in Table 1.
[0239] Table 1 Addition of relevant components and performance test results in Examples 1-15 and Comparative Examples 1-5
[0240]
[0241] The meanings of the abbreviations of polymer A and component B in Table 1 are shown in Table 2. The polymer A and component B used in the examples and comparative examples can be purchased commercially.
[0242] Table 2 Meaning of the abbreviations of polymer A and component B in Table 1
[0243]
[0244]
[0245] The technical solution of this application is analyzed in combination with Table 1 and Table 2:
[0246] (1) By comparing Example 1 and Comparative Example 1, it can be seen that without adding polymer A, the stability of the prepared slurry composition is poor, and the bonding strength and flexibility of the battery positive electrode prepared with the slurry composition are poor. The rate capability and output characteristics of the secondary battery assembled based on this positive electrode are poor.
[0247] (2) By comparing Example 1 and Example 2, it can be seen that after adding component B, the storage stability of the obtained slurry composition is improved, and the flexibility of the positive electrode prepared with the battery slurry is improved. This is because the rich hydrogen bonding between component B and polymer A can inhibit the thickening of the slurry composition for secondary batteries, prolong the gel time, and thus improve the performance of the positive electrode and secondary batteries.
[0248] (3) By comparing Example 2 with Examples 3-5, it can be seen that after further adding 1,3-propane sultone (PS), vinyl sulfate (DTD) or methylene disulfonate (MMDS) to the electrolyte, the rate performance and output performance of the prepared secondary battery are significantly improved. This is because when the electrolyte contains the above substances, the decomposition reaction of polymer A during the charge and discharge process can be inhibited, thereby increasing the rate of the secondary battery and improving the low-temperature output performance.
[0249] (4) By comparing Example 2 with Comparative Example 2, and Example 1 with Comparative Example 3, it can be seen that when the number of carbon atoms of the alkenyl chain on the carboxylate-containing repeating unit in polymer A is 16 or 18, the battery slurry prepared thereby has poor storage stability, and the positive electrode prepared using the slurry composition has poor bonding strength and flexibility, and the secondary battery prepared thereby has poor rate characteristics and output characteristics.
[0250] (5) By comparing Example 1 with Example 4 and Example 1 with Example 5, it can be seen that when the mass content of the carboxylate-containing repeating unit in polymer A is lower than 25% or higher than 50%, the slurry composition prepared by using the slurry composition has poor storage stability, and the positive electrode prepared by using the slurry composition has poor bonding strength and flexibility, and thus the secondary battery prepared has poor rate characteristics and output characteristics.
[0251] (6) By comparing Example 14 and Example 15, it can be seen that when preparing the slurry composition for separator, adding component B can significantly improve the blocking resistance of the separator, thereby improving the rate characteristics and output characteristics of the assembled secondary battery.
[0252] In summary, the use of a secondary battery binder composition comprising the following specific polymer A can prepare a gel-resistant secondary battery slurry composition, and can improve the operability of a functional layer or an electrode layer formed using the prepared secondary battery slurry composition, wherein the polymer A comprises an amide group-containing monomer unit and a specified amount of a carboxylate-containing monomer unit having an alkyl chain having 3 or more and 15 carbon atoms.
[0253] When polymer A and component B are used simultaneously, component B and polymer A can inhibit the thickening of the slurry composition for secondary batteries through abundant hydrogen bonding, prolong the gel time, and further improve the performance of the secondary battery.
[0254] When the electrolyte contains at least one of 1,3-propane sultone, vinyl sulfate or methylene methane disulfonate, the decomposition reaction of polymer A during the charge and discharge process can be suppressed, thereby not only increasing the rate of the secondary battery, but also further improving the low-temperature output performance.
[0255] The present application has industrial applicability: according to the present application, a secondary battery binder composition can be provided, which can prepare a gel-resistant secondary battery slurry composition, and the prepared secondary battery slurry composition can form a functional layer or electrode layer with excellent operability.
[0256] Furthermore, according to the present application, it is possible to provide a slurry composition for a secondary battery that can reduce gel and form a functional layer or an electrode layer with excellent workability.
[0257] Furthermore, according to the present application, a functional layer for a secondary battery having excellent handleability can be provided.
[0258] Furthermore, according to the present application, it is possible to provide an electrode layer for a secondary battery that is excellent in handleability.
[0259] Furthermore, according to the present application, a secondary battery having a secondary battery functional layer or a secondary battery electrode layer having excellent handleability can be provided.
[0260] Furthermore, according to the present application, it is possible to provide an electronic device having a secondary battery having excellent rate and low-temperature output performance.
[0261] The above embodiments are merely illustrative of the principles and effects of the present application and are not intended to limit the present application. Anyone familiar with the technology may modify or change the above embodiments without violating the spirit and scope of the present application. Therefore, all equivalent modifications or changes made by a person of ordinary skill in the art without departing from the spirit and technical ideas disclosed in the present application shall still be covered by the claims of the present application.
Claims
1. A binder composition for a secondary battery, characterized in that: The invention comprises a polymer A, wherein the polymer A comprises an N-vinyl pyrrolidone monomer unit and a carboxylate-containing monomer unit having an alkenyl chain, and the polymer A comprises 25 wt % to 50 wt % of the carboxylate-containing monomer unit having an alkenyl chain with 3 to 15 carbon atoms.
2. The binder composition for secondary batteries according to claim 1, characterized in that: The content of carboxylate-containing monomer units having an alkenyl chain with carbon atoms of 3 to 15 in the polymer A is 30 wt% to 45 wt%, more preferably 30 wt% to 40 wt%; and / or, when 0.5 g of the polymer A is dissolved in 100 g of water at 25° C., the mass of the insoluble components is less than 0.5% of the mass of the polymer A; and / or, the weight average molecular weight of the polymer A is 5 kDa-800 kDa; and / or, the substance used to form the carboxylate-containing monomer unit includes one or more of vinyl acetate, vinyl propionate, vinyl butyrate, vinyl valerate, propylene acetate, butylene acetate, pentyl acetate, propylene propionate, butylene propionate, and butylene butyrate; And / or, the binder composition for a secondary battery further includes a solvent, and the solvent includes water or a non-aqueous solvent.
3. The binder composition for secondary batteries according to claim 1, characterized in that: The binder composition further comprises component B, and the component B comprises one or more of citrate, tartrate, laurate, myristic acid ester, oleate, and stearate.
4. The binder composition for secondary batteries according to claim 3, characterized in that: The citric acid ester includes one or more of tributyl citrate, acetyl tributyl citrate, isopropyl citrate, propylene glycol polyoxyethylene polyoxypropylene ether monoester of citrate, alkyl glycoside monoester of citrate or glyceryl stearate citrate; And / or, the tartaric acid ester includes one or more of diethyl tartaric acid ester, stearyl tartaric acid ester, lauryl alcohol polyoxyethylene ether tartaric acid ester, varenicline tartaric acid ester, diacetyl tartaric acid ester of monoglyceride, and diacetyl tartaric acid ester of diglyceride; And / or, the lauric acid ester includes one or more of triglycerol monolaurate, diethylene glycol monolaurate, polyethylene glycol laurate, pentaerythritol monolaurate, sorbitan monolaurate, and decaglycerol monolaurate; And / or, the myristic acid ester includes one or more of decaglycerol monomyristic acid ester, cholesteryl myristic acid ester, and ascorbyl myristic acid ester; And / or, the oleic acid ester includes one or more of triglycerol oleic acid ester, pentaerythritol oleic acid ester, and epoxidized soybean oil acrylate; And / or, the stearate includes one or more of glyceryl stearate, glyceryl stearate citrate, propylene glycol stearate, and pentaerythritol stearate. 5 . Use of the binder composition for secondary batteries according to claim 1 in preparing a slurry composition for secondary batteries, a functional layer for secondary batteries, an electrode layer for secondary batteries, a secondary battery or an electronic device.
6. A slurry composition for secondary batteries, characterized in that: The slurry composition for secondary batteries comprises the binder composition for secondary batteries according to any one of claims 1 to 4 and non-conductive particles; Preferably, the mass ratio of polymer A in the slurry composition to the total solid content in the slurry composition for secondary battery is 1.0% to 7.0%; and / or, the mass ratio of component B in the slurry composition to the total solid content in the slurry composition for secondary battery is 0.2% to 7.0%; and / or, the mass ratio of the non-conductive particles to the total solid content in the slurry composition for secondary battery is 85% to 99%.
7. A slurry composition for secondary batteries, characterized in that: The slurry composition for secondary batteries comprises the binder composition for secondary batteries according to any one of claims 1 to 4 and an electrode active material; Preferably, the mass ratio of polymer A in the slurry composition to the total solid components in the slurry composition is 0.1% to 3.0%; and / or, the mass ratio of component B in the slurry composition to the total solid components in the slurry composition is 0.2% to 3.0%; and / or, the mass ratio of the electrode active substance to the total solid components in the slurry composition is 90% to 99%.
8. A functional layer for a secondary battery, characterized in that: The secondary battery is formed from the slurry composition for secondary batteries according to claim 6.
9. An electrode layer for a secondary battery, characterized in that: The secondary battery is formed from the slurry composition for secondary batteries according to claim 7.
10. A secondary battery comprising a positive electrode, a negative electrode, a separator and an electrolyte, characterized in that: At least one of the positive electrode, the negative electrode, and the separator includes the secondary battery functional layer according to claim 8 or the secondary battery electrode layer according to claim 9 .
11. The secondary battery according to claim 10, characterized in that: The electrolyte includes one or more of 1,3-propane sultone, vinyl sulfate or methylene methane disulfonate; based on the weight of the electrolyte, the content of 1,3-propane sultone, vinyl sulfate or methylene methane disulfonate is 0.1% to 3%.
12. An electronic device, characterized in that: The power supply source of the electronic device includes the secondary battery according to claim 11.
Citation Information
Patent Citations
Binder for battery negative electrode, composition, slurry and preparation method of pole piece
CN116014136A
Process for the production of solid pharmaceutical sustained release forms
DE3810343A1
Method for producing n-vinyl pyrrolidone / vinyl acetate copolymers
US20110263786A1