Secondary battery and electronic device

By setting up a high porosity separator and ceramic coating in the electrode assembly of the lithium-ion battery, the problem of lithium dissipation on the outer electrode plate of the electrode assembly is solved, and the circulation and safety performance are improved.

CN119069773AActive Publication Date: 2024-12-03NINGDE AMPEREX TECHNOLOGY LTD

Patent Information

Application Number
CN202411389394.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-30
Publication Date
2024-12-03
Estimated Expiration
2044-09-30

AI Technical Summary

Technical Problem

The outer electrode plates of the electrode assembly in lithium-ion batteries are prone to black spots and lithium extraction problems, resulting in reduced performance and safety risks.

Method used

By providing membranes with different porosities in the electrode assembly, the porosity of the first membrane is greater than that of the second membrane, and the specific surface area and thickness of the ceramic coating are regulated to improve the liquid storage capacity and circulation performance outside the electrode assembly. .

Benefits of technology

It effectively reduces the risk of black spots and lithium excretion on the outer electrode plate of the electrode assembly, improves the circulation and safety performance of the secondary battery, and extends the service life.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119069773A_ABST
    Figure CN119069773A_ABST
Patent Text Reader

Abstract

The invention provides a secondary battery and an electronic device, the secondary battery comprises a shell and an electrode assembly of a lamination structure, the electrode assembly comprises a first pole piece, a second pole piece and a diaphragm which are laminated, the first pole piece comprises two outer side first pole pieces, two secondary outer side first pole pieces and an inner side first pole piece, the second pole pieces comprise two outer side second pole pieces and an inner side second pole piece, the two outer side first pole pieces are located on the two outermost sides of the electrode assembly respectively, and at least one outer side first pole piece is a single-face first pole piece. The diaphragms comprise a first diaphragm and a second diaphragm, the first diaphragm is arranged between the single-sided first pole piece and the outer side second pole piece, and the second diaphragm is arranged between the inner side first pole piece and the inner side second pole piece adjacent to the inner side first pole piece. The porosity of the first diaphragm is P1, the porosity of the second diaphragm is P2, and P1 is larger than P2. Through the arrangement, the risks of black spots and lithium precipitation of the pole piece on the outer side of the electrode assembly are reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of electrochemical technology, and in particular to a secondary battery and an electronic device. Background Art

[0002] Secondary batteries, such as lithium-ion batteries, have the characteristics of large specific energy, high operating voltage, low self-discharge rate, small size and light weight, and are widely used in the field of consumer electronics.

[0003] At present, the electrode assembly in lithium-ion batteries often adopts a multi-electrode and laminated structure to reduce the battery impedance. Among them, in order to ensure the ultra-thinness and high energy density of lithium-ion batteries, the outermost electrode of the electrode assembly usually adopts a single-sided coated electrode. However, due to the manufacturing process and structural particularity of the single-sided coated electrode, black spots or lithium precipitation are prone to occur during the cycle, resulting in reduced performance of lithium-ion batteries. Summary of the invention

[0004] The purpose of the present application is to provide a secondary battery and an electronic device to reduce the risk of black spots and lithium deposition on the outer pole pieces of the electrode assembly and improve the cycle performance of the secondary battery.

[0005] It should be noted that in the invention content of the present application, a lithium-ion battery is used as an example of a secondary battery to explain the present application, but the secondary battery of the present application is not limited to a lithium-ion battery.

[0006] The production of the electrode assembly of the laminated structure in the secondary battery is to cut the positive electrode sheet, the negative electrode sheet and the separator by a cutter and then stack them by hot pressing. The conventional soft-pack laminated secondary battery structure is stacked and packaged by N layers of the inner second electrode sheet, N-1 layers of the inner first electrode sheet and 2 layers of the outer first electrode sheet. Due to the existence of the curling effect, the thickness of the collector of the outer first electrode sheet is usually 2 to 3 times the thickness of the collector of the inner first electrode sheet, which leads to a small resistance and a large current density of the outer first electrode sheet, and the ability to consume and transmit electrolyte is greater than that of the inner electrode sheet. In the long-term cycle process, it is more likely to cause the problem of lithium precipitation at the interface of the outer electrode sheet due to insufficient electrolyte on the outer side of the electrode assembly. As the cycle continues, lithium dendrites continue to form and intensify, and eventually pierce the separator to cause direct contact between the positive and negative electrode sheets and short circuit, affecting the safety performance of the secondary battery. Based on this, the present application provides a secondary battery that can reduce the risk of lithium precipitation on the outer electrode sheet caused by insufficient electrolyte on the outer side of the electrode assembly, while taking into account the energy density of the secondary battery, and improving the cycle performance of the secondary battery. The specific technical solutions are as follows:

[0007] The first aspect of the present application provides a secondary battery, comprising a housing and an electrode assembly of a laminated structure, wherein along the thickness direction of the electrode assembly, the electrode assembly comprises a first electrode sheet, a second electrode sheet and a diaphragm arranged between the first electrode sheet and the second electrode sheet, the first electrode sheet comprises two outer first electrode sheets, two second outer first electrode sheets and an inner first electrode sheet located between the two second outer first electrode sheets, the second electrode sheet comprises two outer second electrode sheets and an inner second electrode sheet located between the two outer second electrode sheets, the two outer first electrode sheets are respectively located on the outermost two sides of the electrode assembly, at least one outer first electrode sheet is a single-sided first electrode sheet, the two outer second electrode sheets are respectively located on the side of the two outer first electrode sheets away from the housing and are respectively adjacent to the two outer first electrode sheets, the two second outer first electrode sheets are respectively located on the side of the two outer second electrode sheets away from the housing and are respectively adjacent to the two outer second electrode sheets. The diaphragm comprises a first diaphragm and a second diaphragm, the first diaphragm is arranged between the single-sided first electrode sheet and the outer second electrode sheet, and the second diaphragm is arranged between the inner first electrode sheet and the inner second electrode sheet adjacent thereto. The porosity of the first diaphragm is P1, the porosity of the second diaphragm is P2, and P1>P2. By arranging diaphragms of different porosities in the electrode assembly of the laminated structure, and making the porosity of the first diaphragm greater than the porosity of the second diaphragm, the liquid storage capacity outside the electrode assembly can be improved, and the risk of black spots and lithium precipitation on the outer pole piece caused by insufficient electrolyte outside the electrode assembly during the cycle can be reduced, and the secondary battery has good cycle performance.

[0008] In some embodiments of the present application, 1.30≤P1 / P2≤2.17, 30%≤P2≤50%. By adjusting the values ​​of P1 / P2 and P2 within the above range, the secondary battery has good cycle performance while taking into account safety performance.

[0009] In some embodiments of the present application, the first pole piece is a positive pole piece. When the positive pole piece is selected as the first pole piece, the risk of black spots and lithium deposition on the outer pole piece caused by insufficient electrolyte on the outer side of the electrode assembly during the cycle is more significantly reduced, thereby further improving the cycle performance of the secondary battery.

[0010] In some embodiments of the present application, the first diaphragm includes a first base film and a first ceramic coating located on at least one surface of the first base film, the first ceramic coating includes first ceramic particles, the second diaphragm includes a second base film and a second ceramic coating located on at least one surface of the second base film, the second ceramic coating includes second ceramic particles, the first ceramic particles and the second ceramic particles are independently selected from at least one of boehmite, Al2O3, ZrO2 or TiO2; the average particle size of the first ceramic particles is D1μm, 0.10≤D1≤1.50; the average particle size of the second ceramic particles is D2μm, 0.50≤D2≤5.00. By selecting the above-mentioned types of first ceramic particles and second ceramic particles, and regulating the average particle size of the first ceramic particles and the second ceramic particles within the above-mentioned range, it is beneficial to adjust the specific surface area of ​​the first ceramic coating and the second ceramic coating, thereby reducing the risk of black spots and lithium precipitation on the outer pole piece caused by insufficient electrolyte on the outer side of the electrode assembly during the cycle, and improving the cycle performance of the secondary battery.

[0011] In some embodiments of the present application, 0.02≤D1 / D2≤1.00. By adjusting the value of D1 / D2 within the above range, the particle size of the first ceramic particles is less than or equal to the particle size of the second ceramic particles, which is conducive to adjusting the specific surface area of ​​the first ceramic coating and the second ceramic coating, thereby reducing the risk of black spots and lithium precipitation on the outer electrode sheet caused by insufficient electrolyte on the outer side of the electrode assembly during the cycle, and improving the cycle performance of the secondary battery.

[0012] In some embodiments of the present application, the thickness of the first ceramic coating is 1.0 μm to 8.0 μm, and the thickness of the second ceramic coating is 1.0 μm to 5.0 μm. By adjusting the thickness T1 of the first ceramic coating and the thickness T2 of the second ceramic coating within the above range, it is beneficial to further increase the space for the diaphragm, especially the outermost diaphragm of the electrode assembly, to accommodate the electrolyte, and improve the liquid storage capacity of the outside of the electrode assembly, thereby reducing the risk of black spots and lithium precipitation on the outer electrode sheet caused by insufficient electrolyte on the outside of the electrode assembly during the cycle, while taking into account the energy density of the secondary battery, and improving the cycle performance of the secondary battery.

[0013] In some embodiments of the present application, the material of the first base film and the material of the second base film are independently selected from at least one of polyethylene or polypropylene; the porosity of the first base film is p1, 50%≤p1≤65%, and the porosity of the second base film is p2, 30%≤p2≤50%. By selecting the above-mentioned types of first base film and second base film, and regulating the porosity of the first base film and the second base film within the above-mentioned range, the risk of black spots and lithium precipitation on the outer pole piece caused by insufficient electrolyte on the outer side of the electrode assembly during the cycle is reduced, and the cycle performance of the secondary battery is improved. At the same time, the mechanical strength of the first diaphragm and the second diaphragm is relatively high, which is conducive to further taking into account the safety performance of the secondary battery.

[0014] In some embodiments of the present application, 1.30≤p1 / p2≤2.17. By regulating the value of p1 / p2 within the above range, the first base film has a higher porosity than the second base film, reducing the risk of black spots and lithium precipitation on the outer electrode sheet caused by insufficient electrolyte on the outer side of the electrode assembly during the cycle, while taking into account the mechanical strength of the first diaphragm and the second diaphragm, the cycle performance of the secondary battery is improved.

[0015] In some embodiments of the present application, the thickness of the first base film is 4.0 μm to 12.0 μm, and the thickness of the second base film is 4.0 μm to 9.0 μm. By adjusting the thickness T'1 of the first base film and the thickness T'2 of the second base film within the above range, the cycle performance of the secondary battery is improved while taking into account the energy density of the secondary battery.

[0016] In some embodiments of the present application, the first ceramic coating further includes a first binder, and the second ceramic coating further includes a second binder, and the first binder and the second binder are independently selected from at least one of polyvinylidene fluoride, polyacrylic acid, carboxymethyl cellulose or sodium alginate; based on the mass of the first ceramic coating, the mass percentage of the first binder is 1.0% to 10.0%; based on the mass of the second ceramic coating, the mass percentage of the second binder is 1.0% to 10.0%. By selecting the above-mentioned first binder and the second binder, and regulating the mass percentage W1 of the first binder and the mass percentage W2 of the second binder within the above-mentioned range, the safety performance of the secondary battery is improved while taking into account the cycle performance.

[0017] In some embodiments of the present application, the shell is an aluminum-plastic film.

[0018] In some embodiments of the present application, the thickness of the first diaphragm is H1μm, the thickness of the second diaphragm is H2μm, 1.0≤H1 / H2≤5.8, 5.0≤H2≤19.0. By regulating the values ​​of H1 and H2 within the above range, the risk of black spots and lithium precipitation on the outer pole piece caused by insufficient electrolyte on the outer side of the electrode assembly during the cycle is reduced, while taking into account the energy density of the secondary battery, the cycle performance and safety performance of the secondary battery are improved.

[0019] In some embodiments of the present application, the diaphragm also includes a third diaphragm, which is disposed between the outer second pole piece and the second outer first pole piece, and the porosity of the third diaphragm is P3, P3>P2. In some embodiments of the present application, the diaphragm also includes a fourth diaphragm, which is disposed between the second outer first pole piece and the inner second pole piece adjacent thereto, and the porosity of the fourth diaphragm is P4, P4>P2. Through the above-mentioned regulation, the porosity of the second outer diaphragm and / or the second outer diaphragm of the electrode assembly, and the outermost diaphragm and the electrolyte accommodation space are larger, which further reduces the risk of black spots and lithium precipitation on the outer pole piece caused by insufficient electrolyte on the outer side of the electrode assembly during the cycle, thereby further improving the cycle performance of the secondary battery.

[0020] The second aspect of the present application provides an electronic device, which includes the secondary battery in any one of the above embodiments. The secondary battery of the present application has good cycle performance, so the electronic device of the present application has a long service life.

[0021] Beneficial effects of the embodiments of the present application:

[0022] The present application provides a secondary battery and an electronic device. By setting the porosity of the first diaphragm to be greater than the porosity of the second diaphragm, the porosity of the outermost diaphragm of the electrode assembly and the electrolyte storage space are larger, thereby improving the liquid storage capacity on the outside of the electrode assembly, reducing the risk of black spots and lithium deposition on the outer pole pieces of the electrode assembly during the cycle, and improving the cycle performance of the secondary battery.

[0023] Of course, implementing any product or method of the present application does not necessarily require achieving all of the advantages described above at the same time. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] In order to more clearly illustrate the embodiments of the present application or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present application, and for ordinary technicians in this field, other embodiments can also be obtained based on these drawings.

[0025] Figure 1 A schematic diagram of a cross-sectional structure of a secondary battery according to an embodiment of the present application observed along its length direction;

[0026] Figure 2 A schematic diagram of a cross-sectional structure of a secondary battery according to another embodiment of the present application observed along its length direction;

[0027] Figure 3 A schematic diagram of a cross-sectional structure of a secondary battery according to another embodiment of the present application observed along its length direction;

[0028] Figure 4 This is a schematic diagram of the cross-sectional structure of a secondary battery according to another embodiment of the present application observed along its length direction.

[0029] Figure numerals: secondary battery 001; electrode assembly 01; shell 02; first pole piece 10; outer first pole piece 101; second outer first pole piece 102; inner first pole piece 103; second pole piece 20; outer second pole piece 201; inner second pole piece 202; diaphragm 30; first diaphragm 301; first base film 3011; first ceramic coating 3012; second diaphragm 302; second base film 3021; ​​second ceramic coating 3022; third diaphragm 303; fourth diaphragm 304. DETAILED DESCRIPTION

[0030] The following will be combined with the drawings in the embodiments of the present application to clearly and completely describe the technical solutions in the embodiments of the present application. Obviously, the described embodiments are only part of the embodiments of the present application, rather than all the embodiments. All other embodiments obtained by those skilled in the art based on the present application belong to the scope of protection of the present application.

[0031] It should be noted that in the specific implementation of the present application, lithium-ion batteries are used as an example of secondary batteries to explain the present application, but the secondary batteries of the present application are not limited to lithium-ion batteries. The specific technical solutions are as follows:

[0032] The first aspect of the present application provides a secondary battery, comprising a housing and an electrode assembly of a laminated structure, wherein along the thickness direction of the electrode assembly, the electrode assembly comprises a first electrode sheet, a second electrode sheet and a diaphragm arranged between the first electrode sheet and the second electrode sheet, the first electrode sheet comprises two outer first electrode sheets, two second outer first electrode sheets and an inner first electrode sheet located between the two second outer first electrode sheets, the second electrode sheet comprises two outer second electrode sheets and an inner second electrode sheet located between the two outer second electrode sheets, the two outer first electrode sheets are respectively located on the outermost two sides of the electrode assembly, at least one outer first electrode sheet is a single-sided first electrode sheet, the two outer second electrode sheets are respectively located on the side of the two outer first electrode sheets away from the housing and are respectively adjacent to the two outer first electrode sheets, the two second outer first electrode sheets are respectively located on the side of the two outer second electrode sheets away from the housing and are respectively adjacent to the two outer second electrode sheets. The diaphragm comprises a first diaphragm and a second diaphragm, the first diaphragm is arranged between the single-sided first electrode sheet and the outer second electrode sheet, and the second diaphragm is arranged between the inner first electrode sheet and the inner second electrode sheet adjacent thereto. The porosity of the first diaphragm is P1, the porosity of the second diaphragm is P2, and P1>P2.

[0033] In this application, the electrode assembly of the laminated structure is defined as having a width direction of X, a length direction of Y, and a thickness direction of Z. It is understood that the length direction, width direction, and thickness direction of the diaphragm, the first pole piece, and the second pole piece are the same as those of the electrode assembly. For example, Figure 1 As shown, the secondary battery 001 includes an electrode assembly 01 and a shell 02 of a laminated structure. Along the thickness direction Z direction of the electrode assembly 01, the electrode assembly 01 includes a first pole piece 10, a second pole piece 20 and a diaphragm 30 arranged between the first pole piece 10 and the second pole piece 20. The first pole piece 10 includes two outer first pole pieces 101, two second outer first pole pieces 102 and an inner first pole piece 103 located between the two second outer first pole pieces 102. The second pole piece 20 includes two outer second pole pieces 201 and The inner second pole piece 202 is located between the two outer second pole pieces 201, the two outer first pole pieces 101 are respectively located on the outermost two sides of the electrode assembly 01, the two outer first pole pieces 101 are single-sided first pole pieces, the two outer second pole pieces 201 are respectively located on the side of the two outer first pole pieces 101 away from the shell 02 and are respectively adjacent to the two outer first pole pieces 101, and the two sub-outer first pole pieces 102 are respectively located on the side of the two outer second pole pieces 201 away from the shell 02 and are respectively adjacent to the two outer second pole pieces 201. The diaphragm 30 includes a first diaphragm 301 and a second diaphragm 302, the first diaphragm 301 is arranged between the single-sided first pole piece 101 and the outer second pole piece 201, and the second diaphragm 302 is arranged between the inner first pole piece 103 and the inner second pole piece 202 adjacent thereto.

[0034] The inventors have discovered that by using a laminated layered diaphragm in an electrode assembly with a laminated structure, the porosity of the first diaphragm is greater than that of the second diaphragm, that is, the porosity of the outermost diaphragm is greater than that of the inner diaphragm, P1>P2. At this time, the porosity of the outermost diaphragm of the electrode assembly and the electrolyte storage space are larger, which improves the liquid storage capacity of the outside of the electrode assembly, reduces the risk of black spots and lithium deposition on the outer electrode sheets due to insufficient electrolyte on the outside of the electrode assembly during the cycle, and improves the cycle performance of the secondary battery. When the porosity of the first diaphragm is less than or equal to the porosity of the second diaphragm, that is, the porosity of the outermost diaphragm is less than or equal to the porosity of the inner diaphragm, P1≤P2, the porosity of the outermost diaphragm of the electrode assembly and the electrolyte storage space are small. In the long-term cycle process, it is easy to cause black spots and lithium precipitation on the outer electrode sheet due to insufficient electrolyte on the outer side of the electrode assembly. As the cycle continues, lithium dendrites continue to be generated, piercing the diaphragm to cause direct contact between the positive and negative electrode sheets and a high risk of short circuit, which reduces the cycle performance and safety performance of the secondary battery. When the first diaphragm, that is, a high-porosity diaphragm, is used in the electrode assembly, there is more free electrolyte in the secondary battery shell at this time, and the overall shaking of the electrode assembly is more violent when it falls, and the falling performance is poor; at the same time, when it falls, the free electrolyte impacts the outer diaphragm of the electrode assembly, resulting in an increased risk of short circuit in the secondary battery. Therefore, by arranging diaphragms with different porosities in the electrode assembly of the stacked structure and making the porosity of the first diaphragm greater than the porosity of the second diaphragm, the liquid storage capacity on the outside of the electrode assembly can be improved, and the risk of black spots and lithium deposition on the outer electrode sheets due to insufficient electrolyte on the outside of the electrode assembly during the cycle can be reduced. While taking into account the drop performance and safety performance, the cycle performance of the secondary battery is improved.

[0035] In the present application, it is understood that in an electrode assembly of a laminated structure, when the total number of layers of the remaining first and second pole sheets is less than 7 except for the two outer first pole sheets, the diaphragm only includes the first diaphragm and the second diaphragm; or, the diaphragm only includes the first diaphragm, the second diaphragm and the third diaphragm. Figure 2 As shown, in the electrode assembly 01 of the stacked structure, the first pole piece 10 includes two outer first pole pieces 101 and an inner first pole piece 103 located between the two outer first pole pieces 101, and the two outer first pole pieces 101 are both single-sided first pole pieces, and the second pole piece 20 only includes two outer second pole pieces 201. At this time, except for the two outer first pole pieces 101, the total number of layers of the remaining first pole pieces 10 and the second pole pieces 20 is 3 layers, and the second pole piece 20 does not include the inner second pole piece. Then, the first diaphragm 301 is arranged between the single-sided first pole piece 101 and the outer second pole piece 201, and the second diaphragm 302 is arranged between the inner first pole piece 103 and the second pole piece 20 adjacent thereto, that is, the outer second pole piece 201. At this time, the diaphragm 30 only includes the first diaphragm 301 and the second diaphragm 302.

[0036] In some embodiments of the present application, 1.30≤P1 / P2≤2.17, 30%≤P2≤50%. For example, the value of P1 / P2 can be 1.30, 1.35, 1.40, 1.45, 1.50, 1.55, 1.60, 1.65, 1.70, 1.75, 1.80, 1.85, 1.90, 1.95, 2.0, 2.05, 2.1, 2.13, 2.15, 2.17 or a range consisting of any two of them; the value of P2 can be 30%, 32%, 35%, 38%, 40%, 42%, 45%, 48%, 50% or a range consisting of any two of them. By regulating the values ​​of P1 / P2 and P2 within the above range, while taking into account the mechanical strength of the first diaphragm and the second diaphragm, the outermost diaphragm of the electrode assembly has a larger space for accommodating the electrolyte, thereby improving the liquid storage capacity on the outside of the electrode assembly and the ion transmission efficiency during the cycle, and reducing the risk of black spots and lithium deposition on the outer electrode sheets due to insufficient electrolyte on the outside of the electrode assembly during the cycle. While taking into account the safety performance, the secondary battery has good cycle performance.

[0037] In some embodiments of the present application, the first pole piece is a positive pole piece. When the positive pole piece is selected as the first pole piece, the first pole piece on the outside of the electrode assembly is the positive pole piece, and the volume change of the positive pole piece during the charge and discharge process is relatively small, which is conducive to maintaining the stability of the internal structure of the secondary battery, slowing down the consumption rate of the electrolyte on the outside of the electrode assembly during the cycle, and reducing the risk of black spots and lithium precipitation on the outside pole piece caused by insufficient electrolyte on the outside of the electrode assembly during the cycle. The effect is more obvious, thereby further improving the cycle performance of the secondary battery.

[0038] In some embodiments of the present application, the first diaphragm includes a first base film and a first ceramic coating located on at least one surface of the first base film, the first ceramic coating includes first ceramic particles, and the second diaphragm includes a second base film and a second ceramic coating located on at least one surface of the second base film, the second ceramic coating includes second ceramic particles; illustratively, as Figure 1As shown, the first diaphragm 301 includes a first base film 3011 and a first ceramic coating 3012 located on both surfaces of the first base film 3011, the second diaphragm 302 includes a second base film 3021 and a second ceramic coating 3022 located on both surfaces of the second base film 3021, the first ceramic particles and the second ceramic particles are independently selected from at least one of boehmite, Al2O3, ZrO2 or TiO2; the average particle size of the first ceramic particles is D1μm, 0.10≤D1≤1.50, for example, the value of D1 can be 0.10, 0.20, 0.30, 0.40, 0.50, 0.60, 0.70, 0.80, 0.90, 100, 100, 100, 100, 100, 100, 100, 100, 100, 100, 100, 100, 100, 100 .70, 0.80, 0.90, 1.00, 1.10, 1.20, 1.30, 1.40, 1.50 or a range consisting of any two of the values; the average particle size of the second ceramic particles is D2 μm, 0.50≤D2≤5.00, for example, the value of D2 can be 0.50, 0.80, 1.00, 1.30, 1.50, 1.80, 2.00, 2.30, 2.50, 2.80, 3.00, 3.30, 3.50, 3.80, 4.00, 4.30, 4.50, 4.80, 5.00 or a range consisting of any two of the values. By selecting the above-mentioned types of first ceramic particles and second ceramic particles, and regulating the average particle size of the first ceramic particles and the second ceramic particles within the above-mentioned range, it is beneficial to adjust the specific surface area of ​​the first ceramic coating and the second ceramic coating, and then regulate the porosity of the first diaphragm and the porosity of the second diaphragm, so that the porosity of the first diaphragm is smaller than the porosity of the second diaphragm, the porosity of the outermost diaphragm of the electrode assembly and the electrolyte storage space are larger, thereby improving the liquid storage capacity of the outside of the electrode assembly, thereby reducing the risk of black spots and lithium precipitation on the outer electrode sheet due to insufficient electrolyte on the outside of the electrode assembly during the cycle, and improving the cycle performance of the secondary battery.

[0039] In some embodiments of the present application, 0.02≤D1 / D2≤1.00. For example, the value of D1 / D2 can be 0.02, 0.05, 0.08, 0.10, 0.20, 0.30, 0.40, 0.50, 0.60, 0.70, 0.80, 0.90, 1.00 or a range consisting of any two of the values. By regulating the value of D1 / D2 within the above range, the average particle size of the first ceramic particles is less than or equal to the average particle size of the second ceramic particles, which is conducive to regulating the specific surface area of ​​the first ceramic coating and the second ceramic coating. The specific surface area of ​​the first ceramic coating is larger, thereby making the porosity of the first diaphragm greater than the porosity of the second diaphragm, and the porosity of the outermost diaphragm of the electrode assembly and the electrolyte storage space are larger, thereby improving the liquid storage capacity of the outside of the electrode assembly, thereby reducing the risk of black spots and lithium precipitation on the outer pole piece caused by insufficient electrolyte on the outside of the electrode assembly during the cycle, and improving the cycle performance of the secondary battery.

[0040] The present application does not particularly limit the method for regulating the average particle size of the ceramic particles, as long as the purpose of the present application can be achieved. For example, the average particle size of the ceramic particles can be regulated by grading and grinding the particles of the ceramic particles. Exemplarily, when other conditions remain unchanged, the average particle size of the ceramic particles decreases when the grinding time is extended; and the average particle size of the ceramic particles increases when the grinding time is shortened.

[0041] In some embodiments of the present application, the thickness T1 of the first ceramic coating is 1.0 μm to 8.0 μm, and the thickness T2 of the second ceramic coating is 1.0 μm to 5.0 μm. For example, the thickness T1 of the first ceramic coating may be 1.0 μm, 2.0 μm, 3.0 μm, 4.0 μm, 5.0 μm, 6.0 μm, 7.0 μm, 8.0 μm, or a range consisting of any two values ​​therein; the thickness T2 of the second ceramic coating may be 1.0 μm, 1.5 μm, 2.0 μm, 2.5 μm, 3.0 μm, 3.5 μm, 4.0 μm, 4.5 μm, 5.0 μm, or a range consisting of any two values ​​therein. By regulating the thickness T1 of the first ceramic coating and the thickness T2 of the second ceramic coating within the above range, it is beneficial to further increase the space for the diaphragm, especially the outermost diaphragm of the electrode assembly, to accommodate the electrolyte, thereby improving the liquid storage capacity on the outside of the electrode assembly, thereby reducing the risk of black spots and lithium deposition on the outer electrode sheets due to insufficient electrolyte on the outside of the electrode assembly during the cycle, thereby improving the cycle performance of the secondary battery while taking into account the energy density of the secondary battery.

[0042] In the present application, the thickness of the first ceramic coating and the thickness of the second ceramic coating can be controlled by means known to those skilled in the art. For example, when the first ceramic coating slurry is coated on the surface of the first base film, on the basis of a certain solid content of the first ceramic coating slurry, the coating amount of the first ceramic coating slurry is increased to increase the thickness of the first ceramic coating; when the second ceramic coating slurry is coated on the surface of the second base film, on the basis of a certain solid content of the second ceramic coating slurry, the coating amount of the second ceramic coating slurry is increased to increase the thickness of the second ceramic coating. The present application does not impose any special restrictions as long as the purpose of the present application can be achieved.

[0043] In some embodiments of the present application, the material of the first base film and the material of the second base film are each independently selected from at least one of polyethylene (PE) or polypropylene (PP); the porosity of the first base film is p1, 50%≤p1≤65%, for example, the value of p1 can be 50%, 51%, 52%, 53%, 54%, 55%, 56%, 57%, 58%, 59%, 60%, 61%, 62%, 63%, 64%, 65%, 66%, 67%, 68%, 69%, 70%, 71%, 72%, 73%, 74%, 75%, 76%, 77%, 78%, 79%, 80%, 81%, 82%, 83%, 84%, 85%, 86%, 87%, 88%, 89%, 90%, 91%, 92%, 93%, 94%, 95%, 96%, 97%, 98%, 99%, 100%, 101%, 102%, 103%, 104%, 105%, 106%, 107%, 108%, 109%, 110%, 111%, 112%, 113%, 114%, 115%, 116%, 117%, 118%, 119%, 120%, 121%, 122%, 123%, 124%, 125%, 126%, 127%, 128%, 129%, 130%, 131%, 132%, 133%, 134%, 135 65% or a range consisting of any two of the values ​​therein; the porosity of the second basement membrane is p2, 30%≤p2≤50%, for example, the value of p2 can be 30%, 31%, 32%, 33%, 34%, 35%, 36%, 37%, 38%, 39%, 40%, 41%, 42%, 43%, 44%, 45%, 46%, 47%, 48%, 49%, 50 .... By selecting the above-mentioned types of first base film and second base film, and regulating the porosity of the first base film and the second base film within the above-mentioned range, it is beneficial to regulate the porosity of the first diaphragm and the porosity of the second diaphragm, so that the porosity of the first diaphragm is smaller than the porosity of the second diaphragm, and the porosity of the outermost diaphragm of the electrode assembly and the electrolyte storage space are larger, which improves the liquid storage capacity outside the electrode assembly, thereby reducing the risk of black spots and lithium precipitation on the outer pole piece caused by insufficient electrolyte outside the electrode assembly during the cycle, and improving the cycle performance of the secondary battery. At the same time, by regulating the porosity p1 of the first base film and the porosity p2 of the second base film within the above-mentioned range, the mechanical strength of the first diaphragm and the second diaphragm is relatively high, which is beneficial to further take into account the safety performance of the secondary battery.

[0044] In some embodiments of the present application, 1.30≤p1 / p2≤2.17, for example, the value of p1 / p2 can be 1.30, 1.35, 1.40, 1.45, 1.50, 1.55, 1.60, 1.65, 1.70, 1.75, 1.80, 1.85, 1.90, 1.95, 2.0, 2.05, 2.1, 2.13, 2.15, 2.17 or a range consisting of any two of the values. By regulating the value of p1 / p2 within the above range, the first base membrane has a higher porosity than the second base membrane, which is beneficial to regulating the porosity of the first ceramic coating and the second ceramic coating, so that the porosity of the first diaphragm is greater than that of the second diaphragm, thereby increasing the electrolyte storage space of the outermost diaphragm of the electrode assembly and improving the liquid storage capacity on the outside of the electrode assembly, thereby reducing the risk of black spots and lithium deposition on the outer electrode sheet due to insufficient electrolyte on the outside of the electrode assembly during the cycle, while taking into account the mechanical strength of the first diaphragm and the second diaphragm, the cycle performance of the secondary battery is improved.

[0045] In the present application, the first base film with different porosities can be purchased, and the first base film with the required porosity can be selected in combination with the test method of "Porosity test of the first base film and the second base film" of the present application. In the present application, the second base film with different porosities can be purchased, and the second base film with the required porosity can be selected in combination with the test method of "Porosity test of the first base film and the second base film" of the present application.

[0046] In some embodiments of the present application, the thickness T'1 of the first base film is 4.0 μm to 12.0 μm, and the thickness T'2 of the second base film is 4.0 μm to 9.0 μm. For example, the thickness T'1 of the first base film can be 4.0 μm, 5.0 μm, 6.0 μm, 7.0 μm, 8.0 μm, 9.0 μm, 10.0 μm, 11.0 μm, 12.0 μm, or a range consisting of any two of the values; the thickness T'2 of the second base film can be 4.0 μm, 4.5 μm, 5.0 μm, 5.5 μm, 6.0 μm, 6.5 μm, 7.0 μm, 7.5 μm, 8.0 μm, 8.5 μm, 9.0 μm, or a range consisting of any two of the values. By regulating the thickness T'1 of the first base film and the thickness T'2 of the second base film within the above range, it is beneficial to further increase the space for the diaphragm, especially the outermost diaphragm of the electrode assembly, to accommodate the electrolyte, thereby improving the liquid storage capacity on the outside of the electrode assembly, thereby reducing the risk of black spots and lithium deposition on the outer electrode sheets due to insufficient electrolyte on the outside of the electrode assembly during the cycle, thereby improving the cycle performance of the secondary battery while taking into account the energy density of the secondary battery.

[0047] In the present application, the first base film of different thicknesses can be purchased, and in combination with the test method of "thickness test of first ceramic coating, second ceramic coating, first base film, second base film, first diaphragm and second diaphragm" of the present application, the first base film of the desired thickness can be selected. In the present application, the second base film of different thicknesses can be purchased, and in combination with the test method of "thickness test of first ceramic coating, second ceramic coating, first base film, second base film, first diaphragm and second diaphragm" of the present application, the second base film of the desired thickness can be selected.

[0048] In some embodiments of the present application, the first ceramic coating further includes a first binder, and the second ceramic coating further includes a second binder, and the first binder and the second binder are each independently selected from at least one of polyvinylidene fluoride, polyacrylic acid, carboxymethyl cellulose or sodium alginate; based on the mass of the first ceramic coating, the mass percentage content W1 of the first binder is 1.0% to 10.0%, for example, the mass percentage content W1 of the first binder can be 1.0%, 2.0%, 3.0%, 4.0%, 5.0%, 6.0%, 7.0%, 8.0%, 9.0%, 10.0%, 11.0%, 12.0%, 13.0%, 14.0%, 15.0%, 16.0%, 17.0%, 18.0%, 19.0%, 20.0%, 21.0%, 22.0%, 23.0%, 24.0%, 25.0%, 26.0%, 27.0%, 28.0%, 29.0%, 30.0%, 31.0%, 32.0%, 33.0%, 34.0%, 35.0%, 36.0%, 37.0%, 38.0%, 39.0%, 40.0%, 41.0%, 42.0%, 43.0%, 44.0%, 45.0%, 46.0%, 47.0%, 48.0%, 49.0%, 50.0%, 51.0%, 52.0%, 53.0%, 54.0%, 55. 5.0%, 6.0%, 7.0%, 8.0%, 9.0%, 10.0% or a range consisting of any two of these values; based on the mass of the second ceramic coating, the mass percentage content W2 of the second binder is 1.0% to 10.0%, for example, the mass percentage content W2 of the second binder can be 1.0%, 2.0%, 3.0%, 4.0%, 5.0%, 6.0%, 7.0%, 8.0%, 9.0%, 10.0% or a range consisting of any two of these values. By selecting the first binder and the second binder of the above type, and regulating the mass percentage content W1 of the first binder and the mass percentage content W2 of the second binder within the above range, the first ceramic particles in the first ceramic coating are fixed on the first base film, and the second ceramic particles in the second ceramic coating are fixed on the second base film, and the first diaphragm and the second diaphragm are applied to the secondary battery, while taking into account the cycle performance, the safety performance of the secondary battery is improved.

[0049] In one embodiment of the present application, based on the mass of the first ceramic coating, the mass percentage W'1 of the first ceramic particles is 90.0% to 99.0%, for example, the mass percentage W'1 of the first ceramic particles can be 90.0%, 91.0%, 92.0%, 93.0%, 94.0%, 95.0%, 96.0%, 97.0%, 98.0%, 99.0% or a range consisting of any two of the values ​​therein; based on the mass of the second ceramic coating, the mass percentage W'2 of the second ceramic particles is 90.0% to 99.0%, for example, the mass percentage W'2 of the second ceramic particles can be 90.0%, 91.0%, 92.0%, 93.0%, 94.0%, 95.0%, 96.0%, 97.0%, 98.0%, 99.0% or a range consisting of any two of the values ​​therein. By regulating the mass percentage content W'1 of the first ceramic particles and the mass percentage content W'2 of the second ceramic particles within the above range, the first ceramic particles and the second ceramic particles can fully play their corresponding roles, and the first diaphragm and the second diaphragm have strong liquid retention capabilities. The first diaphragm and the second diaphragm are used in secondary batteries to improve the cycle performance of the secondary batteries.

[0050] In some embodiments of the present application, the shell is an aluminum-plastic film. When the aluminum-plastic film is used as the shell and the first pole piece on the outer side of the electrode assembly is used as the positive pole piece, it is beneficial to reduce the risk of short circuit of the secondary battery and improve the cycle performance and safety performance of the secondary battery.

[0051] In one embodiment of the present application, the first electrode piece is a negative electrode piece, and the shell is a steel shell. When the steel shell is used as the shell, and the first electrode piece on the outer side of the electrode assembly is used as the negative electrode piece, it is beneficial to reduce the risk of short circuit of the secondary battery and improve the cycle performance and safety performance of the secondary battery.

[0052] In some embodiments of the present application, the thickness of the first diaphragm is H1 μm, the thickness of the second diaphragm is H2 μm, 1.0≤H1 / H2≤5.8, 5.0≤H2≤19.0. For example, the value of H1 / H2 can be 1.0, 1.2, 1.5, 1.8, 2.0, 2.2, 2.5, 2.8, 3.0, 3.2, 3.5, 3.8, 4.0, 4.2, 4.5, 4.8, 5.0, 5.2, 5.5, 5.8 or a range consisting of any two of the values, and the value of H2 can be 5.0, 6.0, 7.0, 8.0, 9.0, 10.0, 11.0, 12.0, 13.0, 14.0, 15.0, 16.0, 17.0, 18.0, 19.0 or a range consisting of any two of the values. By adjusting the values ​​of H1 and H2 within the above range, it is beneficial to further increase the space for the diaphragm, especially the outermost diaphragm of the electrode assembly, to accommodate the electrolyte, thereby improving the liquid storage capacity on the outside of the electrode assembly, thereby reducing the risk of black spots and lithium deposition on the outer electrode sheets due to insufficient electrolyte on the outside of the electrode assembly during the cycle, thereby improving the cycle performance and safety performance of the secondary battery while taking into account the energy density of the secondary battery.

[0053] In some embodiments of the present application, the diaphragm further includes a third diaphragm, and the third diaphragm is disposed between the outer second pole piece and the second outer first pole piece. Figure 1 , Figure 3 and Figure 4 As shown, the diaphragm 30 further includes a third diaphragm 303, which is disposed between the outer second pole piece 201 and the second outer first pole piece 102. The porosity of the third diaphragm is P3, where P3>P2. Figure 3 As shown, the third diaphragm is the same as the first diaphragm. By adjusting the porosity of the third diaphragm to be greater than the porosity of the second diaphragm, the porosity of the outermost diaphragm and the second outer diaphragm of the electrode assembly and the electrolyte storage space are larger, which further improves the liquid storage capacity outside the electrode assembly, reduces the risk of black spots and lithium precipitation on the outer electrode sheet caused by insufficient electrolyte outside the electrode assembly during the cycle, and further improves the cycle performance of the secondary battery.

[0054] In some embodiments of the present application, the diaphragm further includes a fourth diaphragm, and the fourth diaphragm is disposed between the second outer first pole piece and the inner second pole piece adjacent thereto. Figure 1 , Figure 3 and Figure 4 As shown, the diaphragm 30 also includes a fourth diaphragm 304, which is disposed between the second outer first pole piece 102 and the inner second pole piece 202 adjacent thereto. The porosity of the fourth diaphragm is P4, and P4>P2. By adjusting the porosity of the fourth diaphragm to be greater than the porosity of the second diaphragm, the porosity of the outermost diaphragm and the second outer diaphragm of the electrode assembly and the electrolyte accommodation space are larger, which further improves the liquid storage capacity of the outer side of the electrode assembly, reduces the risk of black spots and lithium precipitation on the outer pole piece caused by insufficient electrolyte on the outer side of the electrode assembly during the cycle, and further improves the cycle performance of the secondary battery.

[0055] In one embodiment of the present application, the porosity of the third diaphragm is P3, the porosity of the fourth diaphragm is P4, P3>P2, P4>P2. Figure 4 As shown, the third diaphragm, the fourth diaphragm and the first diaphragm use the same diaphragm. By adjusting the porosity of the third diaphragm to be greater than the porosity of the second diaphragm and the porosity of the fourth diaphragm to be greater than the porosity of the second diaphragm, the porosity of the outermost diaphragm, the second outer diaphragm and the second outer diaphragm of the electrode assembly and the electrolyte storage space are larger, further improving the liquid storage capacity outside the electrode assembly, reducing the risk of black spots and lithium precipitation on the outer pole piece caused by insufficient electrolyte outside the electrode assembly during the cycle, and further improving the cycle performance of the secondary battery.

[0056] The present application does not impose any particular restrictions on the method for preparing the first diaphragm, as long as the purpose of the present application can be achieved. For example, the method for preparing the first diaphragm includes but is not limited to the following steps: (1) adding the first ceramic particles and the first binder to a solvent and mixing them evenly to obtain a first ceramic coating slurry; (2) applying the first ceramic coating slurry on one surface of the first base film, and after drying, forming a first ceramic coating on one surface of the first base film to obtain a first diaphragm with a single-sided first ceramic coating; (3) applying the first ceramic coating slurry on the other surface of the first base film, and after drying, obtaining a first diaphragm with a double-sided first ceramic coating. The present application does not impose any restrictions on the above-mentioned solvent, as long as the purpose of the present application can be achieved.

[0057] The present application does not impose any particular restrictions on the preparation method of the second diaphragm, as long as the purpose of the present application can be achieved. For example, the preparation method of the first diaphragm includes but is not limited to the following steps: (1) adding the second ceramic particles and the second binder to the solvent and mixing them evenly to obtain a second ceramic coating slurry; (2) coating the second ceramic coating slurry on one surface of the second base film, and after drying, forming a second ceramic coating on one surface of the second base film to obtain a second diaphragm with a single-sided second ceramic coating; (3) coating the second ceramic coating slurry on the other surface of the second base film, and after drying, obtaining a second diaphragm with a double-sided second ceramic coating. The present application does not impose any restrictions on the above-mentioned solvent, as long as the purpose of the present application can be achieved.

[0058] In the present application, when the first pole piece is a positive pole piece, the second pole piece is a negative pole piece. When the first pole piece is a negative pole piece, the second pole piece is a positive pole piece.

[0059] The present application has no special restrictions on the positive electrode sheet, as long as the purpose of the present application can be achieved. For example, the positive electrode sheet includes a positive current collector and a positive electrode material layer, and the positive electrode collector includes a first surface and a second surface arranged relatively along the thickness direction of the electrode assembly, and the first surface is closer to the shell than the second surface. When the first electrode sheet is a positive electrode sheet, the positive electrode sheet includes two outer positive electrode sheets, two sub-outer positive electrode sheets, and an inner positive electrode sheet located between the two sub-outer positive electrode sheets, and at least one outer positive electrode sheet is a single-sided positive electrode sheet, and no positive electrode material layer is provided on the first surface of the single-sided positive electrode sheet, and a positive electrode material layer is provided on the second surface of the single-sided positive electrode sheet. It should be noted that the "surface" here can be the entire area of ​​the surface of the positive current collector, or it can be a partial area of ​​the surface of the positive current collector. The present application has no special restrictions, as long as the purpose of the present application can be achieved.

[0060] The present application has no particular restrictions on the positive electrode current collector, as long as the purpose of the present application can be achieved. For example, the positive electrode current collector may include aluminum foil, aluminum alloy foil or a composite current collector (such as an aluminum-carbon composite current collector). The positive electrode material layer of the present application includes a positive electrode active material. The present application has no particular restrictions on the type of positive electrode active material, as long as the purpose of the present application can be achieved. For example, the positive electrode active material may include lithium nickel cobalt manganese oxide (LiNi 0.90 Co 0.05 Mn 0.05O2 (NCM955), NCM811, NCM622, NCM523, NCM111), lithium nickel cobalt aluminum oxide, lithium iron phosphate, lithium-rich manganese-based materials, lithium cobalt oxide (LiCoO2), lithium manganate, lithium iron manganese phosphate or lithium titanate, etc. In the present application, the positive active material may also contain non-metallic elements, for example, the non-metallic elements include at least one of fluorine, phosphorus, boron, chlorine, silicon or sulfur. In the present application, there is no particular restriction on the thickness of the positive current collector and the positive electrode material layer, as long as the purpose of the present application can be achieved. In the present application, the positive electrode material layer may also include a positive electrode binder and a conductive agent. The present application does not particularly limit the type of positive electrode binder in the positive electrode material layer, as long as the purpose of the present application can be achieved. For example, the positive electrode binder may include but is not limited to polyvinylidene fluoride, a copolymer of vinylidene fluoride-hexafluoropropylene, polyamide, polyacrylonitrile, polyacrylate, polyacrylic acid, polyacrylate, polyvinyl pyrrolidone, polyvinyl ether, polymethyl methacrylate, polytetrafluoroethylene or polyhexafluoropropylene. The present application has no particular restrictions on the type of conductive agent in the positive electrode material layer, as long as the purpose of the present application can be achieved. For example, the conductive agent may include but is not limited to at least one of conductive carbon black (Super P), carbon nanotubes (CNTs), carbon fibers, flake graphite, Ketjen black, graphene, metal materials or conductive polymers. The above-mentioned carbon nanotubes may include but are not limited to single-walled carbon nanotubes and / or multi-walled carbon nanotubes. The above-mentioned carbon fibers may include but are not limited to vapor-grown carbon fibers (VGCF) and / or nano-carbon fibers. The above-mentioned metal materials may include but are not limited to metal powders and / or metal fibers. Specifically, the metal may include but is not limited to at least one of copper, nickel, aluminum or silver. The above-mentioned conductive polymers may include but are not limited to at least one of polyphenylene derivatives, polyaniline, polythiophene, polyacetylene or polypyrrole. The present application has no particular restrictions on the mass ratio of the positive active material, the conductive agent, and the positive electrode binder in the positive electrode material layer. Those skilled in the art can choose according to actual needs, as long as the purpose of the present application can be achieved.

[0061] This application places no particular restrictions on the negative electrode sheet, as long as the purpose of this application can be achieved. For example, the negative electrode sheet includes a negative electrode current collector and a negative electrode material layer. The negative electrode current collector includes a third surface and a fourth surface that are oppositely arranged in the thickness direction of the electrode assembly, and the third surface is closer to the housing than the fourth surface. When the first electrode sheet is a negative electrode sheet, the negative electrode sheet includes two outer negative electrode sheets, two sub-outer negative electrode sheets, and an inner negative electrode sheet located between the two sub-outer negative electrode sheets. At least one outer negative electrode sheet is a single-sided negative electrode sheet, and no negative electrode material layer is provided on the third surface of the single-sided negative electrode sheet, while a negative electrode material layer is provided on the second surface of the single-sided negative electrode sheet. It should be noted that the "surface" here can be the entire area of the negative electrode current collector surface or a partial area of the negative electrode current collector surface. This application places no particular restrictions, as long as the purpose of this application can be achieved.

[0062] This application places no particular restrictions on the negative electrode current collector, as long as the purpose of this application can be achieved. For example, the negative electrode current collector can include copper foil, copper alloy foil, nickel foil, stainless steel foil, titanium foil, nickel foam, copper foam, or a composite current collector (such as a lithium-copper composite current collector, a carbon-copper composite current collector, a nickel-copper composite current collector, a titanium-copper composite current collector, etc.). The negative electrode material layer of this application contains a negative electrode active material. This application places no particular restrictions on the type of the negative electrode active material, as long as the purpose of this application can be achieved. For example, the negative electrode active material can include natural graphite, artificial graphite, mesocarbon microbeads (MCMB), hard carbon, soft carbon, silicon, silicon-carbon composite, SiO x (0 < x ≤ 2), Li-Sn alloy, Li-Sn-O alloy, Sn, SnO, SnO2, lithium titanate Li4Ti5O with a spinel structure 12 , Li-Al alloy, or at least one of metallic lithium. In this application, there are no particular restrictions on the thickness of the negative electrode current collector and the negative electrode material layer, as long as the purpose of this application can be achieved. Optionally, the negative electrode material layer can also include a conductive agent and a negative electrode binder. This application places no particular restrictions on the type of the conductive agent in the negative electrode material layer, as long as the purpose of this application can be achieved. For example, the conductive agent can be of the same type as the conductive agent in the above-mentioned positive electrode material layer. This application places no particular restrictions on the type of the negative electrode binder in the negative electrode material layer, as long as the purpose of this application can be achieved. For example, the negative electrode binder can be of the same type as the positive electrode binder in the above-mentioned positive electrode material layer. Optionally, the negative electrode material layer further includes a thickening agent. This application places no particular restrictions on the type of the thickening agent, as long as the purpose of this application can be achieved. For example, the thickening agent can include at least one of carboxymethyl cellulose or sodium carboxymethyl cellulose. This application places no particular restrictions on the mass ratio of the negative electrode active material, conductive agent, binder, and thickening agent in the negative electrode material layer, and those skilled in the art can select according to actual needs, as long as the purpose of this application can be achieved.

[0063] In the present application, the secondary battery also includes an electrolyte, and the electrolyte includes a lithium salt and a non-aqueous solvent. The present application has no particular restrictions on lithium salts, as long as the purpose of the present application can be achieved. For example, the lithium salt may include but is not limited to at least one of LiPF6, LiBF4, LiAsF6, LiClO4, LiB(C6H5)4, LiCH3SO3, LiCF3SO3, LiN(SO2CF3)2, LiC(SO2CF3)3, Li2SiF6, lithium bis(oxalate borate) (LiBOB) or lithium difluoroborate. The present application has no particular restrictions on the content of lithium salts in the electrolyte, as long as the purpose of the present application can be achieved. The present application has no particular restrictions on non-aqueous solvents, as long as the purpose of the present application can be achieved, for example, non-aqueous solvents may include but are not limited to at least one of carbonate compounds, carboxylate compounds, ether compounds or other organic solvents. The above-mentioned carbonate compounds may include but are not limited to at least one of chain carbonate compounds, cyclic carbonate compounds or fluorocarbonate compounds. The above-mentioned linear carbonate compound may include but is not limited to at least one of dimethyl carbonate (DMC), diethyl carbonate (DEC), dipropyl carbonate (DPC), methyl propyl carbonate (MPC), ethyl propyl carbonate (EPC) or methyl ethyl carbonate (MEC). The above-mentioned cyclic carbonate may include but is not limited to at least one of ethylene carbonate (EC), propylene carbonate (PC), butylene carbonate (BC) or vinyl ethylene carbonate (VEC). Fluorinated carbonate compounds may include but are not limited to at least one of fluoroethylene carbonate (FEC), 1,2-difluoroethylene carbonate, 1,1-difluoroethylene carbonate, 1,1,2-trifluoroethylene carbonate, 1,1,2-tetrafluoroethylene carbonate, 1-fluoro-2-methylethylene carbonate, 1-fluoro-1-methylethylene carbonate, 1,2-difluoro-1-methylethylene carbonate, 1,1,2-trifluoro-2-methylethylene carbonate or trifluoromethylethylene carbonate. The above-mentioned carboxylate compounds may include but are not limited to at least one of methyl formate, methyl acetate, ethyl acetate, n-propyl acetate, tert-butyl acetate, methyl propionate, ethyl propionate, propyl propionate, γ-butyrolactone, decanolactone, valerolactone or caprolactone. The above-mentioned ether compounds may include but are not limited to at least one of dibutyl ether, tetraethylene glycol dimethyl ether, diethylene glycol dimethyl ether, 1,2-dimethoxyethane, 1,2-diethoxyethane, 1-ethoxy-1-methoxyethane, 2-methyltetrahydrofuran or tetrahydrofuran. The above-mentioned other organic solvents may include but are not limited to at least one of dimethyl sulfoxide, 1,2-dioxolane, cyclopentane, methylcyclopentane, 1,3-dimethyl-2-imidazolidinone, N-methyl-2-pyrrolidone, dimethylformamide, acetonitrile, trimethyl phosphate, triethyl phosphate or trioctyl phosphate. The present application does not particularly limit the content of the non-aqueous solvent in the electrolyte, as long as the purpose of the present application can be achieved.

[0064] The secondary battery of the present application is not particularly limited, and may include any device that undergoes an electrochemical reaction. In one or more embodiments, the secondary battery may include, but is not limited to, a lithium ion secondary battery (lithium ion battery), a lithium polymer secondary battery, or a lithium ion polymer secondary battery.

[0065] The preparation process of the secondary battery of the present application is well known to those skilled in the art, and there is no special limitation in the present application. For example, the preparation process of the secondary battery may include but is not limited to the following steps: the outer first pole piece, the first diaphragm, the outer second pole piece, the third diaphragm, the second outer first pole piece, the fourth diaphragm, the inner second pole piece, the second diaphragm, the inner first pole piece, the second diaphragm, the inner second pole piece, the fourth diaphragm, the second outer first pole piece, the third diaphragm, the outer second pole piece, the first diaphragm, and the outer first pole piece are stacked in sequence, and then the four corners of the entire laminate structure are fixed with tape to obtain the electrode assembly of the laminate structure, the electrode assembly is placed in the shell, the electrolyte is injected into the shell and sealed, and the secondary battery is obtained. In addition, the overcurrent protection element, the guide plate, etc. can also be placed in the shell as needed to prevent the pressure inside the secondary battery from rising and overcharging and discharging.

[0066] The second aspect of the present application provides an electronic device, which includes the secondary battery in any one of the above embodiments. The secondary battery of the present application has good cycle performance, so the electronic device of the present application has a long service life.

[0067] The electronic device of the present application is not particularly limited, and it can be used for any electronic device known in the prior art. For example, the electronic device can include but is not limited to a laptop computer, a pen-input computer, a mobile computer, an electronic book player, a portable phone, a portable fax machine, a portable copier, a portable printer, a head-mounted stereo headset, a video recorder, a liquid crystal television, a portable cleaner, a portable CD player, a mini-disc, a transceiver, an electronic notepad, a calculator, a memory card, a portable recorder, a radio, a backup power supply, a motor, a car, a motorcycle, a power-assisted bicycle, a bicycle, a lighting fixture, a toy, a game console, a clock, an electric tool, a flashlight, a camera, a large household battery, and a lithium-ion capacitor.

[0068] Example

[0069] The following examples and comparative examples are given to more specifically describe the embodiments of the present application. Various tests and evaluations were performed according to the following methods. In addition, unless otherwise specified, "parts" and "%" are based on mass.

[0070] Test methods and equipment:

[0071] Sampling methods for the first, second, third and fourth diaphragms:

[0072] The lithium-ion batteries in the tested embodiments and comparative examples were disassembled, and the first, second, third and fourth diaphragms were taken out and soaked in dimethyl carbonate (DMC) for 20 min to remove residual electrolyte. Then, the first, second, third and fourth diaphragms were placed in an oven and dried at 60° C. for 12 h to obtain the first, second, third and fourth diaphragm samples.

[0073] Sampling method of the first basement membrane and the second basement membrane:

[0074] The first diaphragm and the second diaphragm obtained by the above sampling were placed in containers respectively, N-methylpyrrolidone (NMP) was added, and the containers were placed in an ultrasonic instrument with a heating function for ultrasonication, the temperature was controlled at 45°C, and the ultrasonication was performed for 3 hours. When the first diaphragm and the second diaphragm became completely transparent, they were taken out to obtain the first basement membrane and the second basement membrane. The above method was used to obtain the first basement membrane and the second basement membrane in the following tests unless otherwise specified.

[0075] Porosity test of the first diaphragm, the second diaphragm, the third diaphragm and the fourth diaphragm:

[0076] The gas displacement method is used for testing. The first diaphragm, the second diaphragm, the third diaphragm and the fourth diaphragm are punched out with a mold to prepare samples (technical personnel in this field can select molds of common sizes and shapes in the field according to factors such as the size and shape of the test object and the requirements of the test equipment). The true volume V0 of the sample is measured by a true density tester. The apparent volume V of the sample can be calculated by measuring the area and thickness of the sample. Then, the percentage of the sample pore volume to the total area P = (V-V0) / V×100%, that is, the porosity P1 of the first diaphragm, the porosity P2 of the second diaphragm, the porosity P3 of the third diaphragm or the porosity P4 of the fourth diaphragm are obtained respectively.

[0077] Porosity test of the first base film and the second base film:

[0078] The gas displacement method is used for testing, and the first basement membrane and the second basement membrane are punched out with a mold to prepare samples (technical personnel in this field can select molds of common sizes and shapes in the field according to factors such as the size and shape of the test object and the requirements of the test equipment). The true volume V0 of the sample is measured by a true density tester. The apparent volume V of the sample can be calculated by measuring the area and thickness of the sample. Then, the percentage of the sample pore volume to the total area p = (V-V0) / V×100%, that is, the porosity p1 of the first basement membrane or the porosity p2 of the second basement membrane is obtained, respectively.

[0079] Test of the average particle size of the first ceramic particles and the average particle size of the second ceramic particles:

[0080] The cross-sections of the first diaphragm and the second diaphragm along the thickness direction are prepared by argon ion polishing, and the cross-sections of the first ceramic coating and the second ceramic coating are observed respectively by scanning electron microscopy (SEM). Ten first ceramic particles and ten second ceramic particles are randomly selected, and the equivalent diameters of the ten first ceramic particles and the ten second ceramic particles are measured respectively (i.e., a particle with an irregular cross-section is converted into a circle of equal area, and the diameter of the circle), and the average value is calculated to obtain the average particle size D1 of the first ceramic particles and the average particle size D2 of the second ceramic particles.

[0081] Thickness test of the first ceramic coating, the second ceramic coating, the first base film, the second base film, the first diaphragm and the second diaphragm:

[0082] The first diaphragm is subjected to argon ion polishing to obtain a cross section of the first diaphragm, and the morphology of the cross section of the first diaphragm along the thickness direction is observed by a field emission scanning electron microscope (Philips, XL-30 model) and a scanning electron microscope photograph is taken, and the thickness T1 of the first ceramic coating, the thickness T'1 of the first base film, and the thickness H1 of the first diaphragm are measured by the scanning electron microscope;

[0083] The second diaphragm was subjected to argon ion polishing to obtain a cross section of the second diaphragm. The cross-sectional morphology of the second diaphragm along the thickness direction was observed using a field emission scanning electron microscope (Philips, model XL-30) and scanning electron microscope photographs were taken. The thickness T2 of the second ceramic coating, the thickness T'2 of the second base film and the thickness H2 of the second diaphragm were measured using a scanning electron microscope.

[0084] Lithium deposition performance test:

[0085] The lithium-ion battery in the embodiment and the comparative example is placed in a constant temperature box at 10°C. After 60 minutes, it is charged to 4.5V at 2C constant current, charged to 0.025C at 4.5V constant voltage, and then discharged to 3.0V at 0.5C constant current after standing for 5 minutes. This is one cycle. After 100 cycles of the above charge and discharge process, it is charged to 4.5V at 2C constant current, charged to 0.025C at 4.5V constant voltage, and then disassembled after standing for 5 minutes. The outer negative electrode of the electrode assembly is taken out, and the lithium deposition state on the surface of the outer negative electrode is observed. The non-lithium deposition area on the surface of the outer negative electrode is golden yellow, and the lithium deposition area is grayish white.

[0086] The criteria for judging the degree of lithium deposition in lithium-ion batteries are as follows: a lithium deposition area of ​​0% means no lithium deposition, i.e., the degree of lithium deposition is zero; a lithium deposition area greater than 0 and less than or equal to 2% means mild lithium deposition, i.e., the degree of lithium deposition is mild; a lithium deposition area greater than 2% and less than or equal to 20% means moderate lithium deposition, i.e., the degree of lithium deposition is moderate; a lithium deposition area greater than 20% and less than or equal to 100% means severe lithium deposition, i.e., the degree of lithium deposition is severe, wherein the percentage of the lithium deposition area is calculated based on the total area of ​​the negative electrode material layer of the outer negative electrode sheet.

[0087] Black spot test:

[0088] Place the lithium-ion battery in a 0℃ constant temperature box and let it stand for 60 minutes to allow the lithium-ion battery to reach a constant temperature. Charge the lithium-ion battery that has reached a constant temperature at 0℃ with a constant current of 1C to a full charge voltage of 4.5V, then charge it to 0.025C at a constant voltage of 4.5V, let it stand for 5 minutes, and then discharge it to 3.0V at a constant current of 1C; this is a charge and discharge cycle. After 500 cycles of charge and discharge, charge it to a full charge voltage of 4.5V at a constant current of 1C, and then charge it to 0.025C at a constant voltage of 4.5V to obtain a fully charged battery with 500 cycles. Disassemble the lithium-ion battery in a dry room with a humidity of less than 5%, and take photos to record whether there are black spots on the surface of the outer negative electrode.

[0089] The criteria for judging the degree of black spots in lithium-ion batteries are as follows: a black spot area of ​​0% means no black spots appear, that is, the degree of black spots is none; a black spot area greater than 0 and less than or equal to 2% means mild black spots, that is, the degree of black spots is mild; a black spot area of ​​2% and less than or equal to 20% means moderate black spots, that is, the degree of black spots is moderate; a black spot area greater than 20% and less than or equal to 100% means severe black spots, that is, the degree of black spots is severe, wherein the percentage of the black spot area is calculated based on the total area of ​​the negative electrode material layer of the outer negative electrode plate.

[0090] Cycle performance test:

[0091] Place the lithium-ion battery in a 25℃ constant temperature test box and let it stand for 30 minutes to allow the lithium-ion battery to reach a constant temperature of 25℃. Charge to 4.5V at a constant current of 1C, charge to a current of 0.025C at a constant voltage of 4.5V, let it stand for 5 minutes, and discharge to 3.0V at a constant current of 0.2C. This is the first cycle, and the initial discharge capacity is recorded as C0, and the initial thickness at this time is recorded as T0. Perform charge and discharge cycles on the lithium-ion battery according to the above process. When the cycle reaches 500 cycles (cls), stop the test, record the discharge capacity after 500 cycles (cls) as C1, and the initial thickness at this time is recorded as T1. Calculate the 500cls capacity retention rate and thickness growth rate as indicators for evaluating the cycle performance of lithium-ion batteries.

[0092] 500cls capacity retention rate (%) = C1 / C0×100%.

[0093] 500cls thickness growth rate (%) = (T1-T0) / C0×100%.

[0094] The higher the 500cls capacity retention rate and the smaller the thickness growth rate, the better the cycle performance of the lithium-ion battery.

[0095] Drop performance test:

[0096] (1) The lithium-ion batteries in the examples and comparative examples were placed in an environment at 25±2°C and humidity ≤60% for 30 minutes, and then charged in the following steps: charged to 3.908V at a constant current of 0.5C, then charged to 0.025C at a constant voltage, and allowed to stand for 30 minutes.

[0097] (2) Place the lithium-ion battery in the fixture, take a high-definition photo of the lithium-ion battery before the drop to confirm that the appearance of the lithium-ion battery is normal, and test the voltage and volatile organic compounds (VOC) before the drop. The voltage range is required to be between 3.853V and 3.933V, and the VOC range is required to be between 0 and 500ppm. Ensure that the lithium-ion battery is not damaged before the drop. Arrange the drop performance test when there is no voltage abnormality.

[0098] (3) Use an automatic drop tower drop device to perform 18 rounds of free fall in different directions from a height of 1.5 m above the ground in the following order (front right edge, top front edge, bottom left edge, bottom right edge, bottom front edge, front, front left edge, top left edge, rear right edge, left side, right side, bottom rear edge, rear side, top rear edge, top right edge, rear left edge, top surface, bottom surface). After the fall, leave the battery at room temperature for 24 h and take high-definition photos of its appearance.

[0099] (4) After the drop, perform an appearance inspection to check if the lithium-ion battery is damaged or leaking; measure and record the voltage and VOC of the lithium-ion battery. Criteria for passing the drop test: the lithium-ion battery is not damaged or leaking; the voltage drop is less than 10mV; the VOC organic gas detection is less than 500ppm (30 lithium-ion batteries are prepared for each group of embodiments or comparative examples and the number of lithium-ion batteries that fail the test is X, so the drop test failure rate of the group of lithium-ion batteries is X / 30).

[0100] The higher the drop test failure rate, the worse the drop performance of the lithium-ion battery pack.

[0101] Example 1-1

[0102] <Preparation of First Separator>

[0103] A polyethylene (PE) film with a thickness of T'1 = 10 μm is used as the first base film, and the porosity p1 of the first base film is 60%.

[0104] The first ceramic particles Al2O3 and the first binder polyvinylidene fluoride were mixed in a mass ratio of 95:5, and then deionized water was added as a solvent. After mixing evenly, a first ceramic coating slurry was obtained.

[0105] A first ceramic coating slurry is coated on one surface of the first base film, and after drying at 60°C, a first ceramic coating is formed on one surface of the first base film; a first ceramic coating slurry is coated on the other surface of the first base film, and after drying at 60°C, a first ceramic coating is formed on the other surface of the first base film, thereby obtaining a first diaphragm.

[0106] The average particle size of the first ceramic particles is 0.9 μm, that is, D1 is 0.9 μm. Based on the mass of the first ceramic coating, the mass percentage W1 of the first binder is 5%, the mass percentage W'1 of the first ceramic particles is 95%, the thickness T1 of the first ceramic coating is 5 μm, the thickness H1 of the first diaphragm is 20 μm, and the porosity P1 of the first diaphragm is 63.0%.

[0107] <Preparation of Second Separator>

[0108] A polyethylene (PE) film with a thickness of T'2=6 μm is used as the second base film, and the porosity p2 of the second base film is 40%.

[0109] The second ceramic particles Al2O3 and the second binder polyvinylidene fluoride were mixed in a mass ratio of 95:5, and then deionized water was added as a solvent. After mixing evenly, a second ceramic coating slurry was obtained.

[0110] A second ceramic coating slurry is coated on one surface of the second base film, and after drying at 60°C, a second ceramic coating is formed on one surface of the second base film; a second ceramic coating slurry is coated on the other surface of the second base film, and after drying at 60°C, a second ceramic coating is formed on the other surface of the second base film, thereby obtaining a second diaphragm.

[0111] The average particle size of the second ceramic particles is 3 μm, that is, D2 is 3 μm. Based on the mass of the second ceramic coating, the mass percentage W2 of the second binder is 5%, the mass percentage W'2 of the first ceramic particles is 95%, the thickness T2 of the second ceramic coating is 3 μm, the thickness H2 of the second diaphragm is 12 μm, and the porosity P2 of the second diaphragm is 44.0%.

[0112] <Preparation of the third separator> is the same as the above <Preparation of the second separator>.

[0113] <Preparation of Fourth Separator> is the same as the above <Preparation of Second Separator>.

[0114] <Preparation of positive electrode sheet>

[0115] A positive electrode sheet was selected as the first electrode sheet, and the positive electrode active material lithium cobalt oxide, the conductive agent conductive carbon black and the positive electrode binder polyvinylidene fluoride were mixed in a mass ratio of 97.0:1.5:1.5, and N-methylpyrrolidone (NMP) was added as a solvent. The mixture was fully stirred and evenly mixed to form a positive electrode slurry with a solid content of 75wt%. The positive electrode slurry was evenly coated on one surface of a positive electrode current collector aluminum foil with a thickness of 10μm, and dried at 110°C to obtain a positive electrode sheet with a single-sided coating of a positive electrode material layer with a thickness of 55μm. The positive electrode slurry was coated on the other surface of the positive electrode current collector aluminum foil, and after drying, a positive electrode sheet with a total thickness of 120μm was obtained. The coated positive electrode sheet was cold pressed and then cut into a specification of 70mm×800mm for standby use. Among them, the compaction density of the positive electrode material layer is 4.23g / cm 3 .

[0116] The positive electrode active material lithium cobalt oxide, the conductive agent conductive carbon black and the positive electrode binder polyvinylidene fluoride are mixed in a mass ratio of 97.0:1.5:1.5, and N-methylpyrrolidone (NMP) is added as a solvent. The mixture is stirred and evenly mixed to form a positive electrode slurry with a solid content of 75wt%. The positive electrode slurry is evenly coated on one surface of a positive electrode current collector aluminum foil with a thickness of 10μm, and dried at 110°C to obtain a positive electrode sheet with a single-sided coating of a positive electrode material layer with a thickness of 55μm. The single-sided positive electrode sheet after coating is cold pressed and then cut into a specification of 70mm×800mm for standby use. Among them, the compaction density of the positive electrode material layer is 4.23g / cm 3 .

[0117] <Preparation of negative electrode sheet>

[0118] A negative electrode sheet was selected as the second electrode sheet, and the negative electrode active materials artificial graphite, styrene-butadiene rubber, and sodium carboxymethyl cellulose were mixed in a mass ratio of 97.0:1.5:1.5, and then deionized water was added as a solvent. After stirring evenly, a negative electrode slurry with a solid content of 48wt% was obtained. The negative electrode slurry was coated on one surface of a negative electrode current collector copper foil with a thickness of 6μm, and dried at 110°C to obtain a negative electrode sheet with a negative electrode material layer coated with a thickness of 50μm. The negative electrode slurry was coated on the other surface of the negative electrode current collector copper foil, and after drying, a negative electrode sheet with a total thickness of 106μm was obtained. The negative electrode sheet after coating was cold pressed, and then cut into a specification of 74mm×824mm for standby use. Among them, the compaction density of the negative electrode material layer is 1.735g / cm 3 .

[0119] <Preparation of Electrolyte>

[0120] In a glove box filled with dry argon atmosphere, propylene carbonate (PC), diethyl carbonate (DEC), and ethylene carbonate (EC) are mixed at a mass ratio of 1:1:1 to obtain a base solvent, and then lithium hexafluorophosphate (LiPF6) is added to the base solvent to dissolve and mix well to obtain an electrolyte. Among them, based on the mass of the electrolyte, the mass percentage of LiPF6 is 4.5%, and the balance is the base solvent.

[0121] <Preparation of lithium-ion batteries>

[0122] The single-sided positive electrode sheet in <Preparation of positive electrode sheet> is placed on the outermost side of the electrode assembly as the outermost electrode sheet of the electrode assembly. The remaining positive electrode sheets in the electrode assembly are all double-sided positive electrode sheets.

[0123] The prepared outer positive electrode sheet, the first diaphragm, the outer negative electrode sheet, the third diaphragm, the second outer positive electrode sheet, the fourth diaphragm, the inner negative electrode sheet, the second diaphragm, the inner positive electrode sheet, the second diaphragm, the inner negative electrode sheet, the fourth diaphragm, the second outer positive electrode sheet, the third diaphragm, the outer negative electrode sheet, the first diaphragm, and the outer positive electrode sheet are stacked in order, and then the four corners of the entire stacking structure are fixed with tape to obtain an electrode assembly of the stacking structure, and the electrode assembly is placed in a steel shell, placed in a vacuum oven at 80°C for 12 hours to remove moisture, and the prepared electrolyte is injected, and a lithium-ion battery is obtained after vacuum packaging, standing, formation, degassing, trimming and other processes. The design potential range of the lithium-ion battery is 3.0V to 4.5V.

[0124] Example 1-2 to Example 1-18

[0125] Except for adjusting the relevant preparation parameters according to Table 1, the rest is the same as Example 1-1. Among them, when the average particle size of the same type of ceramic particles changes, the grinding time is adjusted so that the value of the average particle size is as shown in Table 1. When the thickness of the ceramic coating changes, the coating amount is adjusted so that the thickness of the ceramic coating is as shown in Table 1.

[0126] Examples 1-19

[0127] In the preparation of the second separator, the second ceramic coating slurry is applied only on one surface of the second base film, and the second ceramic coating slurry is not applied on the other surface of the second base film; in the preparation of the lithium-ion battery, the surface of the second separator coated with the second ceramic coating slurry faces the positive electrode sheet, and the relevant preparation parameters are adjusted according to Table 1. The rest is the same as Example 1-1. When the thickness of the ceramic coating changes, the coating amount is adjusted so that the thickness of the ceramic coating is as shown in Table 1.

[0128] Example 1-20 to Example 1-22

[0129] Except for adjusting the relevant preparation parameters according to Table 1, the rest is the same as Example 1-1. Among them, when the mass percentage of the first binder and the mass percentage of the second binder change, the mass ratio of the first ceramic particles to the first binder and the mass ratio of the second ceramic particles to the second binder are adjusted so that the values ​​of W1 and W2 are as shown in Table 1.

[0130] Example 2-1

[0131] Except that <Preparation of the third diaphragm> is the same as <Preparation of the first diaphragm> in Example 1, the rest is the same as Example 1-1.

[0132] Example 2-2

[0133] Except that <Preparation of the fourth diaphragm> is the same as <Preparation of the first diaphragm> in Example 1, the rest is the same as Example 1-1.

[0134] Example 2-3

[0135] Except that <Preparation of the third diaphragm> and <Preparation of the fourth diaphragm> are the same as <Preparation of the first diaphragm> in Example 1, the rest is the same as Example 1-1.

[0136] Embodiment 2-4

[0137] Except that the negative electrode sheet is selected as the first electrode sheet, the corresponding positive electrode sheet is used as the second electrode sheet, and the single-sided negative electrode sheet is placed on the outermost side of the electrode assembly in <Preparation of lithium-ion battery> as the outermost electrode sheet of the electrode assembly. The remaining negative electrode sheets in the electrode assembly are all double-sided negative electrode sheets, and the positive electrode sheets in the electrode assembly are all double-sided positive electrode sheets, the rest is the same as Example 1-1. Among them, the preparation steps of the single-sided negative electrode sheet are as follows.

[0138] <Preparation of single-sided negative electrode sheet>

[0139] A negative electrode sheet was selected as the first electrode sheet, and the negative electrode active materials artificial graphite, styrene-butadiene rubber, and sodium carboxymethyl cellulose were mixed in a mass ratio of 97.0:1.5:1.5, and then deionized water was added as a solvent. After stirring evenly, a negative electrode slurry with a solid content of 48wt% was obtained. The negative electrode slurry was coated on one surface of a negative electrode current collector copper foil with a thickness of 6μm, and dried at 110°C to obtain a single-sided negative electrode sheet with a negative electrode material layer coated with a thickness of 50μm. The coated negative electrode sheet was cold pressed and then cut into a size of 74mm×824mm for standby use. Among them, the compaction density of the negative electrode material layer is 1.735g / cm 3 .

[0140] Comparative Example 1

[0141] The procedure was the same as that of Example 1-1 except that <Preparation of Second Separator> was the same as that of <Preparation of First Separator> in Example 1-1.

[0142] Comparative Example 2

[0143] Except that <Preparation of first separator> is the same as <Preparation of second separator> in Example 1-4, the rest is the same as Example 1-4.

[0144] Comparative Example 3

[0145] The procedures were the same as those in Example 1-1, except that <Preparation of the first separator> was the same as that in Example 1-1, and <Preparation of the second separator> was the same as that in Example 1-1.

[0146] The preparation parameters and performance parameters of each embodiment and comparative example are shown in Tables 1 to 3.

[0147]

[0148]

[0149] Table 2

[0150]

[0151] It can be seen from Examples 1-1 to 1-22 and Comparative Examples 1 to 3 that by adjusting the porosity of the first diaphragm to be greater than the porosity of the second diaphragm, the area of ​​lithium plating and black spots on the outer pole piece of the electrode assembly is smaller, the 500cls capacity retention rate of the lithium ion battery is improved, the 500cls thickness growth rate is reduced, and the drop test failure rate is low, indicating that the lithium ion battery of the present application can reduce the risk of black spots and lithium plating on the outer pole piece of the electrode assembly during the cycle, and the lithium ion battery has good cycle performance while taking into account the drop performance. The inner and outer diaphragms of the electrode assembly in Comparative Examples 1 and 2 are the same; the various parameters of the first diaphragm and the second diaphragm in Comparative Example 3 are exactly opposite to the various parameters of the first diaphragm and the second diaphragm in Example 1-1; the drop test failure rate of the lithium ion battery in Comparative Examples 1 and 3 is higher, and the lithium ion battery cannot take into account the drop performance while improving the cycle performance, and it shows that the safety performance of the lithium ion battery is poor. In Comparative Example 2, the lithium ion battery has a larger area of ​​lithium plating and black spots, a lower 500cls capacity retention rate, and a larger 500cls thickness growth rate, indicating that the risk of black spots and lithium plating on the outer pole piece of the electrode assembly during the cycle of the lithium ion battery is higher, and the cycle performance of the lithium ion battery is worse. In the lithium ion batteries of Examples 1-1 to 1-21, the area of ​​lithium plating and black spots on the outer first pole piece is smaller, and the 500cls capacity retention rate is higher, the 500cls thickness growth rate is lower, and the drop test failure rate is lower, indicating that the risk of black spots and lithium plating on the outer pole piece of the electrode assembly during the cycle is lower, and the lithium ion battery has good cycle performance while taking into account the drop performance.

[0152] The values ​​of P1 / P2 and P2 usually affect the cycle performance of lithium-ion batteries. It can be seen from Examples 1-1 to 1-22 that when the values ​​of P1 / P2 and P2 are adjusted within the scope of this application, the area of ​​lithium plating and black spots on the first outer pole piece of the lithium-ion battery is small, and the 500cls capacity retention rate is high, the 500cls thickness growth rate is low, and the drop test failure rate is low, indicating that the risk of black spots and lithium plating on the outer pole piece of the electrode assembly during the cycle is low, and the lithium-ion battery has good cycle performance while taking into account the drop performance.

[0153] The average particle size of the first ceramic particles and the average particle size of the second ceramic particles usually affect the cycle performance of the lithium-ion battery. From Examples 1-1 to 1-5 and 1-10, it can be seen that when the average particle size of the first ceramic particles and the average particle size of the second ceramic particles are within the scope of this application, the lithium ion battery has a smaller area of ​​lithium deposition and black spots on the first outer pole piece, a higher 500cls capacity retention rate, a lower 500cls thickness growth rate, and a lower drop test failure rate, indicating that the risk of black spots and lithium deposition on the outer pole piece of the electrode assembly during the cycle is lower, and the lithium ion battery has good cycle performance while taking into account the drop performance.

[0154] The type of the first ceramic particles and the type of the second ceramic particles usually affect the cycle performance of the lithium-ion battery. It can be seen from Examples 1-1 and 1-6 that when the first ceramic particles and the second ceramic particles within the scope of this application are selected, the lithium ion battery has a smaller area of ​​lithium deposition and black spots on the first pole piece on the outside, a higher 500cls capacity retention rate, a lower 500cls thickness growth rate, and a lower drop test failure rate, indicating that the risk of black spots and lithium deposition on the outer pole piece of the electrode assembly during the cycle is lower, and the lithium-ion battery has good cycle performance while taking into account the drop performance.

[0155] The porosity of the first base film and the porosity of the second base film usually affect the cycle performance of the lithium-ion battery. It can be seen from Examples 1-1, 1-7 to 1-11 that when the porosity of the first base film and the porosity of the second base film are within the scope of this application, the lithium ion battery has a small area of ​​lithium deposition and black spots on the first pole piece on the outside, a high 500cls capacity retention rate, a low 500cls thickness growth rate, and a low drop test failure rate, indicating that the risk of black spots and lithium deposition on the outer pole piece of the electrode assembly during the cycle is low, and the lithium ion battery has good cycle performance while taking into account the drop performance.

[0156] The material of the first base film and the material of the second base film usually affect the cycle performance of the lithium-ion battery. It can be seen from Examples 1-1 and 1-12 that when the first base film and the second base film within the scope of this application are selected, the lithium ion battery has a smaller area of ​​lithium deposition and black spots on the first pole piece on the outside, a higher 500cls capacity retention rate, a lower 500cls thickness growth rate, and a lower drop test failure rate, indicating that the risk of black spots and lithium deposition on the outer pole piece of the electrode assembly during the cycle is lower, and the lithium ion battery has good cycle performance while taking into account the drop performance.

[0157] The thickness of the first ceramic coating and the thickness of the second ceramic coating usually affect the cycle performance of the lithium-ion battery. It can be seen from Example 1-1, Example 1-13 to Example 1-14, and Example 1-17 to Example 1-19 that when the thickness of the first ceramic coating and the thickness of the second ceramic coating are within the scope of this application, the lithium ion battery has a smaller area of ​​lithium deposition and black spots on the first outer pole piece, a higher 500cls capacity retention rate, a lower 500cls thickness growth rate, and a lower drop test failure rate, indicating that the risk of black spots and lithium deposition on the outer pole piece of the electrode assembly during the cycle is lower, and the lithium ion battery has good cycle performance while taking into account the drop performance.

[0158] The thickness of the first base film and the thickness of the second base film usually affect the cycle performance of the lithium-ion battery. It can be seen from Examples 1-1, 1-15 to 1-19 that when the thickness of the first base film and the thickness of the second base film are within the scope of this application, the lithium ion battery has a smaller area of ​​lithium deposition and black spots on the first pole piece on the outside, a higher 500cls capacity retention rate, a lower 500cls thickness growth rate, and a lower drop test failure rate, indicating that the risk of black spots and lithium deposition on the outer pole piece of the electrode assembly during the cycle is lower, and the lithium-ion battery has good cycle performance while taking into account the drop performance.

[0159] The thickness H2 of the second diaphragm and the value of H1 / H2 usually affect the cycle performance of the lithium-ion battery. It can be seen from Examples 1-1, 1-10, 1-13 to 1-19 that when the thickness H2 of the second diaphragm and the value of H1 / H2 are within the scope of this application, the area of ​​lithium deposition and black spots on the first pole piece on the outside of the lithium-ion battery is small, and the 500cls capacity retention rate is high, the 500cls thickness growth rate is low, and the drop test failure rate is low, indicating that the risk of black spots and lithium deposition on the outer pole piece of the electrode assembly during the cycle is low, and the lithium-ion battery has good cycle performance while taking into account the drop performance.

[0160] The type and content of the first binder, and the type and content of the second binder usually affect the cycle performance of the lithium-ion battery. It can be seen from Example 1-1, Example 1-20 to Example 1-22 that when the first binder and the second binder within the scope of this application are selected, and the content of the first binder and the content of the second binder are adjusted within the scope of this application, the lithium ion battery has a smaller area of ​​lithium deposition and black spots on the first pole piece on the outside, and a higher 500cls capacity retention rate, a lower 500cls thickness growth rate, and a lower drop test failure rate, indicating that the risk of black spots and lithium deposition on the outer pole piece of the electrode assembly during the cycle is lower, and the lithium ion battery has good cycle performance while taking into account the drop performance.

[0161] Table 3

[0162]

[0163] The relationship between the porosity of the third diaphragm and the second diaphragm usually affects the cycle performance of the lithium-ion battery. It can be seen from Examples 1-1, 2-1 and 2-3 that when the relationship between the porosity of the third diaphragm and the second diaphragm meets the requirements of this application, the lithium ion battery has a smaller area of ​​lithium deposition and black spots on the first pole piece on the outside, a higher capacity retention rate at 500cls, a lower thickness growth rate at 500cls, and a lower drop test failure rate, indicating that the risk of black spots and lithium deposition on the outer pole piece of the electrode assembly during the cycle is lower, and the lithium ion battery has good cycle performance while taking into account the drop performance.

[0164] The relationship between the porosity of the fourth diaphragm and the second diaphragm usually affects the cycle performance of the lithium-ion battery. It can be seen from Examples 1-1, 2-2 and 2-3 that when the relationship between the porosity of the fourth diaphragm and the second diaphragm meets the requirements of this application, the lithium ion battery has a smaller area of ​​lithium deposition and black spots on the first pole piece on the outside, a higher capacity retention rate at 500cls, a lower thickness growth rate at 500cls, and a lower drop test failure rate, indicating that the risk of black spots and lithium deposition on the outer pole piece of the electrode assembly during the cycle is lower, and the lithium ion battery has good cycle performance while taking into account the drop performance.

[0165] The type of the first pole piece usually affects the cycle performance of the lithium-ion battery. It can be seen from Examples 1-1 and 2-4 that when the first pole piece is a positive pole piece or a negative pole piece, the lithium ion battery has a smaller area of ​​lithium plating and black spots on the outer first pole piece, a higher 500cls capacity retention rate, a lower 500cls thickness growth rate, and a lower drop test failure rate, indicating that the risk of black spots and lithium plating on the outer pole piece of the electrode assembly during the cycle is lower, and the lithium-ion battery has good cycle performance while taking into account the drop performance.

[0166] It should be noted that, in this article, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprises" or any other variations thereof are intended to cover non-exclusive inclusion, so that a process, method or article including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method or article.

[0167] Each embodiment in this specification is described in a related manner, and the same or similar parts between the embodiments can be referenced to each other, and each embodiment focuses on the differences from other embodiments.

[0168] The above description is only a preferred embodiment of the present application and is not intended to limit the present application. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present application shall be included in the scope of protection of the present application.

Claims

1. A secondary battery, comprising a shell and an electrode assembly of a laminated structure, wherein along the thickness direction of the electrode assembly, the electrode assembly comprises a first electrode sheet and a second electrode sheet which are stacked and a diaphragm arranged between the first electrode sheet and the second electrode sheet, the first electrode sheet comprises two outer first electrode sheets, two second outer first electrode sheets and an inner first electrode sheet located between the two second outer first electrode sheets, the second electrode sheet comprises two outer second electrode sheets and an inner second electrode sheet located between the two outer second electrode sheets, the two outer first electrode sheets are respectively located at the outermost two sides of the electrode assembly, at least one of the outer first electrode sheets is a single-sided first electrode sheet, the two outer second electrode sheets are respectively located at a side of the two outer first electrode sheets away from the shell and are respectively adjacent to the two outer first electrode sheets, and the two second outer first electrode sheets are respectively located at a side of the two outer second electrode sheets away from the shell and are respectively adjacent to the two outer second electrode sheets; The diaphragm includes a first diaphragm and a second diaphragm, the first diaphragm is arranged between the single-sided first pole piece and the outer second pole piece, and the second diaphragm is arranged between the inner first pole piece and the inner second pole piece adjacent thereto; The porosity of the first diaphragm is P 1 The porosity of the second membrane is P 2 , P 1 >P 2 .

2. The secondary battery according to claim 1, in, 1.30≤P 1 / P 2 ≤2.17,30%≤P 2 ≤50%。 3. The secondary battery according to claim 1 or 2, in, The first pole piece is a positive pole piece.

4. The secondary battery according to claim 3, in, The first diaphragm comprises a first base film and a first ceramic coating located on at least one surface of the first base film, the first ceramic coating comprising first ceramic particles, the second diaphragm comprises a second base film and a second ceramic coating located on at least one surface of the second base film, the second ceramic coating comprising second ceramic particles, the first ceramic particles and the second ceramic particles are independently selected from boehmite, Al 2 O 3 、ZrO 2 or TiO 2 At least one of the above; the average particle size of the first ceramic particles is D 1 μm, 0.10≤D 1 ≤1.50; the average particle size of the second ceramic particles is D 2 μm, 0.50≤D 2 ≤5.

00.

5. The secondary battery according to claim 4, in, 0.02≤D 1 / D 2 ≤1.00。 6. The secondary battery according to claim 4, in, The thickness of the first ceramic coating layer is 1.0 μm to 8.0 μm, and the thickness of the second ceramic coating layer is 1.0 μm to 5.0 μm.

7. The secondary battery according to claim 4, in, The material of the first base film and the material of the second base film are independently selected from at least one of polyethylene and polypropylene; the porosity of the first base film is p 1 , 50% ≤ p 1 ≤65%, the porosity of the second base film is p 2 , 30%≤p 2 ≤50%.

8. The secondary battery according to claim 7, in, 1.30≤p 1 / p 2 ≤2.17。 9. The secondary battery according to claim 7, in, The first base film has a thickness of 4.0 μm to 12.0 μm, and the second base film has a thickness of 4.0 μm to 9.0 μm.

10. The secondary battery according to claim 4, in, The first ceramic coating also includes a first binder, and the second ceramic coating also includes a second binder, the first binder and the second binder are each independently selected from at least one of polyvinylidene fluoride, polyacrylic acid, carboxymethyl cellulose or sodium alginate; based on the mass of the first ceramic coating, the mass percentage of the first binder is 1.0% to 10.0%; based on the mass of the second ceramic coating, the mass percentage of the second binder is 1.0% to 10.0%.

11. The secondary battery according to claim 3, in, The shell is an aluminum-plastic film.

12. The secondary battery according to claim 4, in, The thickness of the first diaphragm is H 1 μm, the thickness of the second diaphragm is H 2 μm, 1.0≤H 1 / H 2 ≤5.8,5.0≤H 2 ≤19.

0.

13. The secondary battery according to claim 1, in, The diaphragm further comprises a third diaphragm, the third diaphragm is arranged between the outer second pole piece and the second outer first pole piece, and the porosity of the third diaphragm is P 3 , P 3 >P 2 .

14. The secondary battery according to claim 1, in, The diaphragm further includes a fourth diaphragm, which is disposed between the second outer first pole piece and the inner second pole piece adjacent thereto, and the porosity of the fourth diaphragm is P 4 , P 4 >P 2 . 15 . An electronic device comprising the secondary battery according to claim 1 .

Citation Information

Patent Citations

  • Lithium ion battery lamination unit, battery cell, battery cell preparing method and lithium ion battery

    CN105336976A

  • Lithium ion battery and pole piece thereof

    CN110429230A

  • Secondary battery and electric device

    CN117203800A

  • Secondary battery and electronic device

    CN117977015A

  • Secondary battery and electronic apparatus

    WO2024159521A1

Cited By

  • Battery cell, battery and energy storage device or energy storage system

    CN122393563A

  • Secondary battery and electronic device

    WO2026045631A1

  • Secondary battery and electronic device

    WO2026066429A1

  • Secondary battery and electronic apparatus

    WO2026158242A1

  • Secondary battery and electronic device

    WO2026193695A1