Solid-state battery and preparation method and application thereof

By introducing a second polymerization monomer at the interface between solid electrolyte layers A and B of the solid electrolyte layer of the solid state battery for self-polymerization, an interface modification layer is formed, which solves the problem of poor interface contact between the composite electrolyte membranes, reduces the battery impedance and improves the ionic conductance Improve battery performance and safety.

CN119069787APending Publication Date: 2024-12-03XIAOGAN CORNEX NEW ENERGY INNOVATION TECHNOLOGY CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202411279954.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-12
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

Poor interface contact between composite electrolyte membranes in existing solid-state batteries leads to an increase in battery impedance, and the hot pressing composite method has problems of secondary crystallization and decomposition caused by poor interface compatibility and excessive temperature, which affects the migration of lithium ions and battery performance.

Method used

The second polymerization monomer is introduced at the interface between the solid electrolyte layer A and the solid electrolyte layer B. The self-polymerization reaction is induced by the second polymerization inducing the occurrence of a self-polymerization reaction to form an interface modification layer, fill the interface defects, and make it in the solid state by hot pressing The electrolyte layer A and the solid electrolyte layer B are polymerized at the contact point to form an interface modification layer to improve ionic conductivity.

Benefits of technology

The battery impedance is reduced, the ionic conductivity of the composite solid electrolyte layer is improved, the dissociation and transmission capacity of lithium ions is enhanced, and the battery performance and safety performance are improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119069787A_ABST
    Figure CN119069787A_ABST
Patent Text Reader

Abstract

The invention provides a solid-state battery and a preparation method and application thereof, and relates to the technical field of batteries. According to the solid-state battery, a second polymerization reaction monomer is introduced into an interface of a solid-state electrolyte layer A and a solid-state electrolyte layer B, so that the solid-state battery is subjected to self-polymerization reaction under the induction action of a second polymerization reaction inducer in the solid-state electrolyte layer A and the solid-state electrolyte layer B; therefore, an interface modification layer is formed at the contact interface of the solid electrolyte layer A and the solid electrolyte layer B. The interface modification layer can fill the interface defect between the solid electrolyte layer A and the solid electrolyte layer B and reduce the impedance of the battery. Meanwhile, a polymer formed by the second polymerization reaction monomer still has a polar group which can be matched with Li < + >, so that dissociation and transmission of Li < + > are facilitated, and the ionic conductivity of the composite solid electrolyte layer (membrane) is improved. The invention also provides a preparation method of the solid-state battery, and the preparation process is simple and easy for large-scale production.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of batteries and relates to a solid-state battery and a preparation method and application thereof. Background Art

[0002] Solid-state batteries use solid electrolytes instead of traditional organic liquid electrolytes, which can effectively improve battery safety performance. Organic-inorganic composite solid electrolytes are composed of organic polymer matrix, inorganic fillers and lithium salts, and are one of the most promising directions for preparing solid-state batteries instead of diaphragms. The composite solid electrolyte prepared by adding active fillers to the polymer exhibits good ionic conductivity and mechanical properties. The high mechanical strength can effectively inhibit the growth of lithium dendrites, but it leads to poor interface contact between the composite electrolyte membrane and the electrode. At present, most of the double-layer / multi-layer composite solid electrolyte membranes with both mechanical strength and adhesion are prepared, and the double-layer / multi-layer composite solid electrolyte membranes are composited by hot pressing.

[0003] When the double-layer / multi-layer composite solid electrolyte membrane is composited by hot pressing, the interface compatibility between different polymers is poor, resulting in gaps and defects in the interface; if the hot pressing temperature is too high, the polymer will melt, and secondary crystallization will occur during cooling, and the crystallization area will hinder the migration of lithium ions; even worse, the local temperature is too high, resulting in the breakage of the polymer molecular chain, and the generation of side reactions such as decomposition, causing irreversible damage to the material. Therefore, simply using hot pressing composite will hinder the migration of ions, increase the impedance of the battery, and seriously affect the battery performance. In the prior art, gel electrolyte is also used to fill the gap at the junction of the solid electrolyte membrane, but the additional initiator has poor compatibility with the positive and negative electrodes, and the gel electrolyte has difficulty penetrating the internal electrode of the battery, and the uniformity is poor, and it is difficult to accurately control the gel process between the double-layer composite electrolyte membrane.

[0004] In view of this, the present invention is proposed. Summary of the invention

[0005] In view of the deficiencies and defects in the prior art, the present invention aims to provide a solid-state battery and a preparation method and application thereof.

[0006] In order to achieve the above purpose, the following technical solutions are adopted:

[0007] A first object of the present invention is to provide a solid-state battery, comprising:

[0008] A positive electrode sheet having a positive electrode active material layer coated on the surface and a solid electrolyte layer A coated on the surface of the positive electrode active material layer; and a negative electrode sheet having a negative electrode active material layer coated on the surface and a solid electrolyte layer B coated on the surface of the negative electrode active material layer;

[0009] The positive electrode sheet and the negative electrode sheet are stacked in sequence, the solid electrolyte layer A and the solid electrolyte layer B are arranged between two adjacent positive electrode sheets and negative electrode sheets, and an interface modification layer is also arranged at the interface where the solid electrolyte layer A and the solid electrolyte layer B contact, and the interface modification layer is mainly formed by polymerization of the second polymerization reaction monomer;

[0010] Wherein, the solid electrolyte layer A is mainly made of a first polymer matrix A, an inorganic filler A, a lithium salt A, a solvent A, and a second polymerization reaction inducer;

[0011] The solid electrolyte layer B is mainly made of a first polymer matrix B, an inorganic filler B, a lithium salt B, a solvent B and a second polymerization reaction inducer;

[0012] The second polymerization monomer is a monomer containing a polar group, capable of bulk polymerization and capable of reacting with Li + The coordinated polymer monomer, the polar group includes an ester group and / or an ether group.

[0013] Furthermore, based on the above technical solution of the present invention, the second polymerization reaction monomer includes at least one of ethylene glycol methacrylate, vinyl carbonate, methyl methacrylate, 1,3-dioxolane or vinyl carbonate.

[0014] Furthermore, based on the above technical solution of the present invention, the second polymerization reaction inducer includes azobisisobutyronitrile and / or dibenzoyl peroxide.

[0015] Further, based on the above technical solution of the present invention, the first polymer matrix A and the first polymer matrix B are independently selected from at least one of polyethylene oxide, polyvinylidene fluoride, polyvinylidene fluoride-hexafluoropropylene, polyacrylonitrile, polymethyl methacrylate, polypropylene or polyvinyl chloride;

[0016] And / or, the inorganic filler A and the inorganic filler B are independently selected from at least one of lithium lanthanum zirconium oxide, lithium lanthanum zirconium tantalum oxide, lithium lanthanum zirconium aluminum oxide, lithium lanthanum zirconium gallium oxide, lithium lanthanum titanium oxide, lithium aluminum germanium phosphate or lithium aluminum titanium phosphate;

[0017] And / or, the lithium salt A and the lithium salt B are independently selected from at least one of lithium hexafluorophosphate, lithium tetrafluoroborate, lithium bis(trifluoromethylsulfonyl)imide or lithium perchlorate;

[0018] And / or, the solvent A and the solvent B are independently selected from at least one of N-methylpyrrolidone and acetonitrile.

[0019] Further, based on the above technical solution of the present invention, the mass ratio of the first polymer matrix A, the inorganic filler A, the lithium salt A, the second polymerization reaction inducer and the solvent A is (2-30): (2-30): (2-15): (0.02-5): 100;

[0020] And / or, the mass ratio of the first polymer matrix B, the inorganic filler B, the lithium salt B, the second polymerization reaction inducer and the solvent B is (2-30): (2-30): (2-15): (0.02-5): 100.

[0021] The second object of the present invention is to provide a method for preparing the above-mentioned solid-state battery, comprising the following steps:

[0022] (a) mixing and dispersing a first polymer matrix A, an inorganic filler A, a lithium salt A, a solvent A, and a second polymerization reaction inducer to obtain a rubber material A;

[0023] Applying the sizing material A on the surface of the positive electrode active material layer of the positive electrode sheet, and then drying, so as to form a solid electrolyte layer A on the surface of the positive electrode active material layer of the positive electrode sheet;

[0024] (b) mixing and dispersing a first polymer matrix B, an inorganic filler B, a lithium salt B, a solvent B, and a second polymerization reaction inducer to obtain a rubber material B;

[0025] Applying the sizing material B on the surface of the negative electrode active material layer of the negative electrode sheet, and then drying, so as to form a solid electrolyte layer B on the surface of the negative electrode active material layer of the negative electrode sheet;

[0026] (c) stacking a positive electrode sheet having a solid electrolyte layer A formed on its surface and a negative electrode sheet having a solid electrolyte layer B formed on its surface, and assembling them so that the solid electrolyte layer A and the solid electrolyte layer B are located between two adjacent positive electrode sheets and negative electrode sheets and in direct contact with each other to obtain an assembly;

[0027] The second polymerization reaction monomer is injected into the assembly, and then allowed to soak. After the positive electrode and the negative electrode are fully soaked, the assembly is hot pressed to allow the second polymerization reaction monomer to polymerize at the interface where the solid electrolyte layer A contacts the solid electrolyte layer B to form an interface modification layer, thereby obtaining a solid-state battery.

[0028] Further, based on the above technical solution of the present invention, in step (a), the first polymer matrix A, the inorganic filler A, the lithium salt A, and the solvent A are mixed and dispersed, the viscosity is controlled to be 50-3000 mPa·s, and then the second polymerization reaction inducer is added to obtain a rubber material A;

[0029] And / or, the coating thickness of the rubber material A is 3-50 μm.

[0030] Further, based on the above technical solution of the present invention, in step (b), the first polymer matrix B, the inorganic filler B, the lithium salt B, and the solvent B are mixed and dispersed, the viscosity is controlled to be 50-3000 mPa·s, and then the second polymerization reaction inducer is added to obtain a rubber material B;

[0031] And / or, the coating thickness of the rubber material B is 3-50 μm.

[0032] Further, based on the above technical solution of the present invention, in step (c), the injection amount of the second polymerization reaction monomer is 0.7-3.5 g / Ah;

[0033] And / or, the static infiltration time is 12-72h;

[0034] And / or, the hot pressing temperature is 50-90° C., the hot pressing pressure is 0.2-2 MPa, and the pressing time is 0.5-8 h.

[0035] The third purpose of the present invention is to provide the application of the above-mentioned solid-state battery or the solid-state battery prepared by the above-mentioned preparation method in the fields of electric vehicles, electronic communication equipment, aerospace vehicles, etc.

[0036] Compared with the prior art, the technical solution of the present invention has at least the following technical effects:

[0037] (1) The present invention provides a solid-state battery, which introduces a second polymerization reaction monomer at the interface between a solid electrolyte layer A and a solid electrolyte layer B, causing the second polymerization reaction monomer to undergo a self-polymerization reaction under the induction of a second polymerization reaction inducer in the solid electrolyte layer A and the solid electrolyte layer B, thereby forming an interface modification layer at the interface where the solid electrolyte layer A and the solid electrolyte layer B contact. The interface modification layer can fill the interface defects between the solid electrolyte layer A and the solid electrolyte layer B, reduce the battery impedance, and effectively solve the problem of poor interface contact between composite electrolyte membranes in solid-state batteries; at the same time, since the second polymerization reaction monomer can react with Li + Cooperation is beneficial to Li + dissociation and transport, thereby improving the ionic conductivity of the composite solid electrolyte layer (membrane).

[0038] (2) The present invention provides a method for preparing the above-mentioned solid-state battery, which has a simple preparation process and is easy to mass produce. BRIEF DESCRIPTION OF THE DRAWINGS

[0039] Figure 1 A schematic structural diagram of a solid-state battery provided by the present invention.

[0040] Among them, 1-negative electrode current collector; 2-negative electrode active material layer; 3-solid electrolyte layer B; 4-interface modification layer; 5-solid electrolyte layer A; 6-positive electrode active material layer; 7-positive electrode current collector. DETAILED DESCRIPTION

[0041] In order to make the purpose, technical scheme and advantages of the present invention clearer, the technical scheme in the embodiment of the present invention will be clearly and completely described below in conjunction with the embodiments of the present invention. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention. Based on the embodiments in the present invention, all other embodiments obtained by ordinary technicians in the field without making creative work are within the scope of protection of the present invention. The process parameters of the following embodiments that do not specify specific conditions are usually based on conventional conditions.

[0042] The endpoints and any values ​​of the ranges disclosed in the present invention are not limited to the precise ranges or values, and these ranges or values ​​should be understood to include values ​​close to these ranges or values. For numerical ranges, the endpoint values ​​of each range, the endpoint values ​​of each range and the individual point values, and the individual point values ​​can be combined with each other to obtain one or more new numerical ranges, which should be regarded as specifically disclosed in the present invention.

[0043] According to a first aspect of the present invention, there is provided a solid-state battery, comprising:

[0044] A positive electrode sheet having a positive electrode active material layer coated on the surface and a solid electrolyte layer A coated on the surface of the positive electrode active material layer; and a negative electrode sheet having a negative electrode active material layer coated on the surface and a solid electrolyte layer B coated on the surface of the negative electrode active material layer;

[0045] The positive electrode sheet and the negative electrode sheet are stacked in sequence, the solid electrolyte layer A and the solid electrolyte layer B are arranged between two adjacent positive electrode sheets and negative electrode sheets, and an interface modification layer is also arranged at the interface where the solid electrolyte layer A and the solid electrolyte layer B contact, and the interface modification layer is mainly formed by polymerization of the second polymerization reaction monomer;

[0046] Wherein, the solid electrolyte layer A is mainly made of a first polymer matrix A, an inorganic filler A, a lithium salt A, a solvent A, and a second polymerization reaction inducer;

[0047] The solid electrolyte layer B is mainly made of a first polymer matrix B, an inorganic filler B, a lithium salt B, a solvent B, and a second polymerization reaction inducer;

[0048] The second polymerization monomer is a polar group-containing monomer capable of bulk polymerization and capable of reacting with Li + The coordinated polymer monomer, the polar group includes an ester group and / or an ether group.

[0049] In the present invention, the basic structure of the solid-state battery includes a negative electrode sheet, a positive electrode sheet, and a solid electrolyte layer B, a solid electrolyte layer A and an interface modification layer arranged between the negative electrode sheet and the positive electrode sheet.

[0050] Specifically, the negative electrode sheet is mainly composed of a negative electrode current collector 1 (such as copper foil, etc.) and a negative electrode active material layer 2 coated on the surface of the negative electrode current collector 1. The solid electrolyte layer B3 is arranged on the surface of the negative electrode active material layer 2 of the negative electrode sheet.

[0051] The positive electrode sheet is mainly composed of a positive electrode current collector 7 (such as aluminum foil, etc.) and a positive electrode active material layer 6 coated on the surface of the positive electrode current collector. The solid electrolyte layer A5 is arranged on the surface of the positive electrode active material layer 6 of the positive electrode sheet.

[0052] The positive electrode sheet and the negative electrode sheet are stacked in sequence (e.g., negative electrode sheet, positive electrode sheet, negative electrode sheet, positive electrode sheet, ... negative electrode sheet), the solid electrolyte layer A 5 and the solid electrolyte layer B 3 are arranged between two adjacent positive electrode sheets and negative electrode sheets, and an interface modification layer 4 is also arranged at the interface where the solid electrolyte layer A and the solid electrolyte layer B contact. The specific structural schematic diagram is shown in FIG. Figure 1 shown.

[0053] In the present invention, both the solid electrolyte layer A and the solid electrolyte layer B are polymer-based electrolyte membranes, which are mainly made of a polymer matrix (a first polymer matrix A or a first polymer matrix B), an inorganic filler (an inorganic filler A or an inorganic filler B), and a lithium salt (a lithium salt A or a lithium salt B). The inorganic filler improves the mechanical strength of the polymer matrix, and is a solid electrolyte that can conduct lithium ions. The lithium salt maintains the dissociation balance of lithium ions and improves the ionic conductivity of the electrolyte.

[0054] However, unlike conventional solid electrolyte layers (polymer-based electrolyte membranes), the solid electrolyte layer A and the solid electrolyte layer B in the present invention are further added with a second polymerization reaction inducer. The second polymerization reaction inducer is mainly used to induce the second polymerization reaction monomer to self-polymerize. Adding the second polymerization reaction inducer to the solid electrolyte layer can reduce the amount of the second polymerization reaction inducer and accurately control the polymerization process of the second polymerization reaction monomer.

[0055] The second polymerization monomer is mainly used to form an interface modification layer at the interface where the solid electrolyte layer A contacts the solid electrolyte layer B. By limiting the polar groups on the second polymerization monomer, it is easier to cooperate with lithium ions, which is beneficial to the migration of lithium ions between molecular chains.

[0056] The present invention introduces a second polymerization reaction monomer at the interface between the solid electrolyte layer A and the solid electrolyte layer B, so that the second polymerization reaction inducing agent in the solid electrolyte layer A and the solid electrolyte layer B induces a self-polymerization reaction, thereby forming an interface modification layer at the interface where the solid electrolyte layer A and the solid electrolyte layer B contact, and the interface modification layer can fill the interface defects between the solid electrolyte layer A and the solid electrolyte layer B, thereby reducing the battery impedance. At the same time, since the polymer formed by the second polymerization reaction monomer still has polar groups, it can react with Li + Cooperation is beneficial to Li + dissociation and transport, thereby improving the ionic conductivity of the composite solid electrolyte layer (membrane).

[0057] The solid-state battery prepared by the present invention has high energy and good energy utilization efficiency. Adding a small amount of monomers also causes bulk polymerization inside the battery, so that the safety performance of the battery is greatly improved.

[0058] As an optional embodiment of the present invention, the second polymerization monomer includes at least one of ethylene glycol methacrylate, vinyl carbonate, methyl methacrylate, 1,3-dioxolane (DOL) or vinyl carbonate, preferably 1,3-dioxolane.

[0059] By further limiting the specific type of the second polymerization reaction monomer, it is made capable of fully wetting the pole piece and can be polymerized by thermal initiation.

[0060] As an optional embodiment of the present invention, the second polymerization inducing agent includes azobisisobutyronitrile (AIBN) and / or dibenzoyl peroxide (BPO).

[0061] By further defining the second polymerization reaction inducing agent, the second polymerization reaction monomer can be smoothly initiated to undergo the second polymerization reaction.

[0062] As an optional embodiment of the present invention, the first polymer matrix A and the first polymer matrix B are independently selected from at least one of polyethylene oxide, polyvinylidene fluoride, polyvinylidene fluoride-hexafluoropropylene, polyacrylonitrile, polymethyl methacrylate, polypropylene or polyvinyl chloride.

[0063] The first polymer matrix A and the first polymer matrix B may be the same or different, and may be selected based on compatibility with the electrode and electrochemical stability.

[0064] As an optional embodiment of the present invention, the inorganic filler A and the inorganic filler B are independently selected from at least one of lithium lanthanum zirconium oxide (LLZO), lithium lanthanum zirconium tantalum oxide (LLZTO), lithium lanthanum zirconium aluminum oxide (LLAZO), lithium lanthanum zirconium gallium oxide (LLGZO), lithium lanthanum titanium oxide (LLTO), lithium aluminum germanium phosphate (LAGP) or lithium aluminum titanium phosphate (LATP).

[0065] As an optional embodiment of the present invention, lithium salt A and lithium salt B are independently selected from at least one of lithium hexafluorophosphate, lithium tetrafluoroborate, lithium bis(trifluoromethylsulfonyl)imide or lithium perchlorate.

[0066] By further limiting the specific types of inorganic fillers and lithium salts, lithium ion migration channels are effectively provided to maintain the dissociation balance of lithium ions.

[0067] As an optional embodiment of the present invention, the solvent A and the solvent B are independently selected from at least one of N-methylpyrrolidone and acetonitrile.

[0068] As an optional embodiment of the present invention, the mass ratio of the first polymer matrix A, the inorganic filler A, the lithium salt A, the second polymerization reaction inducer and the solvent A is (2-30): (2-30): (2-15): (0.02-5): 100, preferably (2-15): (2-28): (2-10): (0.02-2): 100, and further preferably (2-12): (2-28): (2-8): (0.2-1.14): 100. Typical but non-limiting mass ratios of the first polymer matrix A, the inorganic filler A, the lithium salt A, the second polymerization inducing agent and the solvent A are 2:2:2:0.02:100, 10:2:2:0.02:100, 20:2:2:0.02:100, 30:2:2:0.02:100, 2:10:2:0.02:100, 2:20:2:0.02:100, 2.48:26:2:0.32:100, 2.48:26:2:0.65:100, 2.30:2:2:0.02:100. : 0.02:100, 2:2:5:0.02:100, 2:2:10:0.02:100, 2:2:15:0.02:100, 10:10:2:0.02:100, 20:20:2:0.02:100, 30:30:2:0.02:100, 100, 10:10:10:0.02:100, 20:20:10:0.1:100, 30:30:15:1:100, 30:30:15:2:100, 30:30:15:4:100 or 30:30:15:5:100 etc.

[0069] As an optional embodiment of the present invention, the mass ratio of the first polymer matrix B, the inorganic filler B, the lithium salt B, the second polymerization reaction inducer and the solvent B is (2-30): (2-30): (2-15): (0.02-5): 100, preferably (2-15): (2-28): (2-10): (0.02-2): 100, and further preferably (2-12): (2-28): (2-8): (0.2-1.14): 100. Typical but non-limiting mass ratios of the first polymer matrix B, the inorganic filler B, the lithium salt B, the second polymerization inducing agent and the solvent B are 2:2:2:0.02:100, 10:2:2:0.02:100, 20:2:2:0.02:100, 30:2:2:0.02:100, 2:10:2:0.02:100, 2:20:2:0.02:100, 2:30:2:0.02:100, 2:2:5:0.02:100, 2:2:10:0.02:100, 2:2:15:0.02:100, 4:2:17:0. .3:3.3:1.12:100, 9.7:4.1:2.4:0.3:100, 9.7:4.1:2.4:0.58:100, 10:10:2:0.02:100, 20:20:2:0.02:100, 30:30:2:0.02:100, 100, 10:10:10:0.02:100, 20:20:10:0.1:100, 30:30:15:1:100, 30:30:15:2:100, 30:30:15:4:100 or 30:30:15:5:100, etc.

[0070] The amount of the second polymerization reaction inducer added should not be too much, otherwise the addition of inactive materials will affect the performance of the battery. At the same time, the amount of the second polymerization reaction inducer added should not be too little, otherwise it will be difficult to initiate the polymerization of the second polymerization reaction monomer (such as DOL) or the polymerization degree of the second polymerization reaction monomer is low and is still in a liquid state, which will corrode the solid electrolyte layer.

[0071] According to a second aspect of the present invention, there is also provided a method for preparing the above-mentioned solid-state battery, comprising the following steps:

[0072] (a) mixing and dispersing a first polymer matrix A, an inorganic filler A, a lithium salt A, a solvent A, and a second polymerization reaction inducer to obtain a rubber material A;

[0073] Applying the sizing material A on the surface of the positive electrode active material layer of the positive electrode sheet, and then drying, so as to form a solid electrolyte layer A on the surface of the positive electrode active material layer of the positive electrode sheet;

[0074] (b) mixing and dispersing a first polymer matrix B, an inorganic filler B, a lithium salt B, a solvent B, and a second polymerization reaction inducer to obtain a rubber material B;

[0075] Applying the sizing material B on the surface of the negative electrode active material layer of the negative electrode sheet, and then drying, so as to form a solid electrolyte layer B on the surface of the negative electrode active material layer of the negative electrode sheet;

[0076] (c) stacking a positive electrode sheet having a solid electrolyte layer A formed on its surface and a negative electrode sheet having a solid electrolyte layer B formed on its surface, and assembling them so that the solid electrolyte layer A and the solid electrolyte layer B are located between two adjacent positive electrode sheets and negative electrode sheets and in direct contact with each other to obtain an assembly;

[0077] The second polymerization reaction monomer is injected into the assembly, and then allowed to soak. After the positive electrode and the negative electrode are fully soaked, the assembly is hot pressed to allow the second polymerization reaction monomer to polymerize at the interface where the solid electrolyte layer A contacts the solid electrolyte layer B to form an interface modification layer, thereby obtaining a solid-state battery.

[0078] Specifically, step (a) mainly includes preparing a rubber material A for forming a solid electrolyte layer A, and preparing the solid electrolyte layer A using the rubber material A;

[0079] Step (b) mainly involves preparing a rubber material B for forming a solid electrolyte layer B, and using the rubber material B to prepare the solid electrolyte layer B.

[0080] In step (c), the positive electrode sheet and the negative electrode sheet are first stacked, and during the stacking, it is necessary to ensure that the solid electrolyte layer A and the solid electrolyte layer B are located between two adjacent positive electrode sheets and negative electrode sheets and are in direct contact. Then, the second polymerization reaction monomer is injected therein, and the second polymerization reaction monomer is fully infiltrated into the electrode sheet. In the subsequent hot pressing and compounding process, under the induction of the second polymerization reaction inducer and the thermal initiation of the hot pressing process, the second polymerization reaction monomer self-polymerizes to form an interface modification layer, and the interface modification layer can fill the interface defects between the solid electrolyte layer A and the solid electrolyte layer B, thereby reducing the battery impedance.

[0081] The preparation method of the solid-state battery provided by the present invention performs molecular-level interface regulation between the solid electrolyte layer A and the solid electrolyte layer B, so that the polymerization reaction can be precisely controlled; at the same time, the polymerization at the interface can effectively prevent the second polymerization reaction monomer injected in liquid form from corroding the composite electrolyte membrane, causing the collapse of the composite solid electrolyte membrane on the surface of the electrode, thereby reducing the risk of micro-short circuit in the battery.

[0082] As an optional embodiment of the present invention, in step (a), a first polymer matrix A, an inorganic filler A, a lithium salt A, and a solvent A are mixed and dispersed, and the viscosity is controlled to be 50-3000mPa·s (for example, 50mPa·s, 100mPa·s, 200mPa·s, 400mPa·s, 500mPa·s, 600mPa·s, 800mPa·s, 1000mPa·s, 1200mPa·s, 1400mPa·s, 1500mPa·s, 1600mPa·s, 1800mPa·s, 2000mPa·s, 2200mPa·s, 2400mPa·s, 2500mPa·s, 2600mPa·s, 2800mPa·s or 3000mPa·s, etc.), and then a second polymerization reaction inducer is added to obtain rubber material A.

[0083] In the preparation process of rubber material A, attention should be paid to the timing of adding the second polymerization inducer. Since the second polymerization inducer has a certain reactivity, its exposure time in the environment should be minimized.

[0084] As an optional embodiment of the present invention, in step (a), the coating thickness of the rubber material A is 3-50 μm. Typical but non-limiting coating thickness of the rubber material A is 3 μm, 5 μm, 8 μm, 10 μm, 12 μm, 15 μm, 20 μm, 22 μm, 25 μm, 30 μm, 32 μm, 35 μm, 40 μm, 42 μm, 45 μm or 50 μm, etc.

[0085] As an optional embodiment of the present invention, in step (b), a first polymer matrix B, an inorganic filler B, a lithium salt B, and a solvent B are mixed and dispersed, and the viscosity is controlled to be 50-3000mPa·s (for example, 50mPa·s, 100mPa·s, 200mPa·s, 400mPa·s, 500mPa·s, 600mPa·s, 800mPa·s, 1000mPa·s, 1200mPa·s, 1400mPa·s, 1500mPa·s, 1600mPa·s, 1800mPa·s, 2000mPa·s, 2200mPa·s, 2400mPa·s, 2500mPa·s, 2600mPa·s, 2800mPa·s or 3000mPa·s, etc.), and then a second polymerization reaction inducer is added to obtain a rubber material B.

[0086] Similarly, during the preparation of rubber compound B, since the second polymerization reaction inducer has a certain reactivity, it is still necessary to control the timing of adding the second polymerization reaction inducer to minimize its exposure time in the environment.

[0087] As an optional embodiment of the present invention, in step (b), the coating thickness of the rubber material B is 3-50 μm. Typical but non-limiting coating thickness of the rubber material B is 3 μm, 5 μm, 8 μm, 10 μm, 12 μm, 15 μm, 20 μm, 22 μm, 25 μm, 30 μm, 32 μm, 35 μm, 40 μm, 42 μm, 45 μm or 50 μm, etc.

[0088] As an optional embodiment of the present invention, in step (c), the injection amount of the second polymerization reaction monomer is 0.7-3.5 g / Ah, which can be understood as the injection coefficient. Typical but non-limiting injection amounts of the second polymerization reaction monomer are 0.7 g / Ah, 1.0 g / Ah, 1.2 g / Ah, 1.5 g / Ah, 1.8 g / Ah, 2.0 g / Ah, 2.2 g / Ah, 2.5 g / Ah, 2.8 g / Ah, 3.0 g / Ah, 3.2 g / Ah or 3.5 g / Ah, etc.

[0089] As an optional embodiment of the present invention, in step (c), the time of standing and soaking is 12-72 hours. Typical but non-limiting standing and soaking time is 12 hours, 16 hours, 20 hours, 24 hours, 30 hours, 36 hours, 40 hours, 45 hours, 48 ​​hours, 50 hours, 55 hours, 60 hours, 65 hours, 70 hours or 72 hours, etc.

[0090] As an optional embodiment of the present invention, in step (c), the temperature of hot pressing is 50-90°C (for example, 50°C, 55°C, 60°C, 65°C, 70°C, 75°C, 80°C, 85°C, 90°C, etc.), the pressure of hot pressing is 0.2-2MPa (for example, 0.2MPa, 0.5MPa, 0.6MPa, 0.8MPa, 1.0MPa, 1.2MPa, 1.5MPa, 1.6MPa, 1.8MPa or 2.0MPa, etc.), and the pressurizing time is 0.5-8h (for example, 0.5h, 1h, 2h, 3h, 4h, 5h, 6h, 7h or 8h, etc.).

[0091] By further limiting the process parameters of the hot pressing process, the second polymer monomer can fully undergo polymerization reaction on the surface of the coating layer to obtain a good interface.

[0092] According to the third aspect of the present invention, there is also provided the application of the above-mentioned solid-state battery or the solid-state battery prepared by the above-mentioned preparation method in the fields of electric vehicles, electronic communication equipment, aerospace vehicles, etc.

[0093] In view of the advantages of the above-mentioned solid-state battery of the present invention, it has good application prospects in the fields of electric vehicles, electronic communication equipment, aerospace vehicles, etc.

[0094] The present invention will be further described in detail below with reference to specific embodiments and comparative examples.

[0095] Example 1

[0096] This embodiment provides a solid-state battery, comprising:

[0097] A positive electrode sheet having a positive electrode active material layer coated on the surface and a solid electrolyte layer A coated on the surface of the positive electrode active material layer; and a negative electrode sheet having a negative electrode active material layer coated on the surface and a solid electrolyte layer B coated on the surface of the negative electrode active material layer;

[0098] The positive electrode sheet and the negative electrode sheet are stacked in sequence, the solid electrolyte layer A and the solid electrolyte layer B are arranged between two adjacent positive electrode sheets and negative electrode sheets, and an interface modification layer is also arranged at the interface where the solid electrolyte layer A and the solid electrolyte layer B contact, and the interface modification layer is mainly formed by polymerization of the second polymerization reaction monomer;

[0099] Among them, the solid electrolyte layer A is mainly made of a first polymer matrix A, an inorganic filler A, a lithium salt A, a solvent A and a second polymerization reaction inducer; the first polymer matrix A is polyvinylidene fluoride, the inorganic filler A is LLZO, the lithium salt A is lithium bis(trifluoromethylsulfonyl)imide, the solvent A is NMP, and the second polymerization reaction inducer is azobisisobutyronitrile AIBN.

[0100] The solid electrolyte layer B is mainly made of a first polymer matrix B, an inorganic filler B, a lithium salt B, a solvent B and a second polymerization reaction inducer; the first polymer matrix B is polyethylene oxide PEO, the inorganic filler B is LLZO, the lithium salt B is lithium bis(trifluoromethylsulfonyl)imide, the solvent B is acetonitrile, and the second polymerization reaction inducer is azobisisobutyronitrile AIBN.

[0101] The method for preparing the solid-state battery of this embodiment comprises the following steps:

[0102] (a) The first polymer matrix A polyvinylidene fluoride (6.95 g) was dissolved in the solvent A NMP (80 g) and stirred evenly, then the lithium salt A lithium bistrifluoromethylsulfonyl imide (6.5 g) was added and dispersed evenly at high speed, then the inorganic filler A LLZO (73.05 g) and the solvent A NMP (200 g) were added to adjust the viscosity to 800 mPa·s, and finally the second polymerization inducer AIBN (1.81 g) was added to obtain a rubber material A;

[0103] The sizing agent A is evenly coated on the surface of the positive electrode active material layer (ternary positive electrode material, NCM811) of the positive electrode sheet, the coating layer thickness is about 10 μm, and then dried to obtain a positive electrode sheet with a solid electrolyte layer A formed on the surface;

[0104] (b) dissolving the first polymer matrix B polyethylene oxide PEO (8.70 g) in the solvent B acetonitrile (80 g) and stirring evenly, adding the lithium salt B lithium bistrifluoromethylsulfonyl imide (2.17 g) and dispersing evenly at high speed, adding the inorganic filler B LLZO (3.73 g) and the solvent B acetonitrile (10 g) to adjust the viscosity to 1500 mPa·s, and finally adding the second polymerization inducer AIBN (0.52 g) to obtain the rubber material B;

[0105] The glue B is evenly coated on the negative electrode active material layer (graphite is the active material) of the negative electrode sheet, the coating layer thickness is about 10 μm, and then dried to obtain a negative electrode sheet with a solid electrolyte layer B formed on the surface;

[0106] (c) A positive electrode sheet with a solid electrolyte layer A formed on the surface and a negative electrode sheet with a solid electrolyte layer B formed on the surface are stacked (13 positive electrode sheets and 14 negative electrode sheets), and the solid electrolyte layer A and the solid electrolyte layer B are located between two adjacent positive electrode sheets and negative electrode sheets and in direct contact, and then assembled, and a second polymerization reaction monomer 1,3-dioxolane (7.5 g) is added, and the injection amount of the second polymerization reaction monomer is 1.53 g / Ah. Pre-packaging, standing and soaking for 24 hours, and extracting excess 1,3-dioxolane by secondary packaging. Then, hot pressing is performed, that is, by applying a pressure of 0.8 MPa and heating at 60°C for 4 hours, 1,3-dioxolane can be fully polymerized at the interface where the solid electrolyte layer A contacts the solid electrolyte layer B to form an interface modification layer, thereby obtaining a solid-state battery.

[0107] Example 2

[0108] This embodiment provides a solid-state battery and a preparation method thereof. Except for adjusting the mass of the second polymerization reaction inducer AIBN in the solid electrolyte layer A from 1.81g to 0.90g, and adjusting the mass of the second polymerization reaction inducer AIBN in the solid electrolyte layer B from 0.52g to 0.26g, the rest of the preparation method and process parameters are the same as those in Example 1.

[0109] Example 3

[0110] This embodiment provides a solid-state battery and a preparation method thereof. Except for adjusting the mass of the second polymerization reaction inducer AIBN in the solid electrolyte layer A from 1.81g to 0.36g, and adjusting the mass of the second polymerization reaction inducer AIBN in the solid electrolyte layer B from 0.52g to 0.10g, the rest of the preparation method and process parameters are the same as those in Example 1.

[0111] Example 4

[0112] The present embodiment provides a solid-state battery and a preparation method thereof. Except for adjusting the mass of the second polymerization reaction inducer AIBN in the solid electrolyte layer A from 1.81 g to 0.04 g, and adjusting the mass of the second polymerization reaction inducer AIBN in the solid electrolyte layer B from 0.52 g to 0.02 g, the rest of the preparation method and process parameters are the same as those in Example 1.

[0113] Example 5

[0114] This embodiment provides a solid-state battery and a preparation method thereof. Except for adjusting the mass of the second polymerization reaction inducer in the solid electrolyte layer A from 1.81 g to 3.62 g, and adjusting the mass of the second polymerization reaction inducer in the solid electrolyte layer B from 0.52 g to 1.04 g, the rest of the preparation method and process parameters are the same as those in Example 1.

[0115] Example 6

[0116] This embodiment provides a solid-state battery and a preparation method thereof. Except that the second polymerization reaction inducer in the solid electrolyte layer A and the solid electrolyte layer B is adjusted from azobisisobutyronitrile AIBN to dibenzoyl peroxide BPO, the rest of the preparation method and process parameters are the same as those in Example 1.

[0117] Example 7

[0118] This embodiment provides a solid-state battery and a preparation method thereof. Except for adjusting the type of the second polymerization reaction monomer from 1,3-dioxolane to vinyl ethylene carbonate, the rest of the preparation method and process parameters are the same as those in Example 1.

[0119] Example 8

[0120] This embodiment provides a solid-state battery and a preparation method thereof. Except for adjusting the type of the second polymerization reaction monomer from 1,3-dioxolane to methyl methacrylate, the rest of the preparation method and process parameters are the same as those in Example 1.

[0121] Example 9

[0122] This embodiment provides a solid-state battery, comprising:

[0123] A positive electrode sheet having a positive electrode active material layer coated on the surface and a solid electrolyte layer A coated on the surface of the positive electrode active material layer; and a negative electrode sheet having a negative electrode active material layer coated on the surface and a solid electrolyte layer B coated on the surface of the negative electrode active material layer;

[0124] The positive electrode sheet and the negative electrode sheet are stacked in sequence, the solid electrolyte layer A and the solid electrolyte layer B are arranged between two adjacent positive electrode sheets and negative electrode sheets, and an interface modification layer is also arranged at the interface where the solid electrolyte layer A and the solid electrolyte layer B contact, and the interface modification layer is mainly formed by polymerization of the second polymerization reaction monomer;

[0125] Among them, the solid electrolyte layer A is mainly made of a first polymer matrix A, an inorganic filler A, a lithium salt A, a solvent A and a second polymerization reaction inducer; the first polymer matrix A is polyvinylidene fluoride-hexafluoropropylene, the inorganic filler A is LATP, the lithium salt A is lithium tetrafluoroborate, the solvent A is NMP, and the second polymerization reaction inducer is azobisisobutyronitrile AIBN.

[0126] The solid electrolyte layer B is mainly made of a first polymer matrix B, an inorganic filler B, a lithium salt B, a solvent B and a second polymerization reaction inducer; the first polymer matrix B is polyacrylonitrile, the inorganic filler B is LATP, the lithium salt B is lithium tetrafluoroborate, the solvent B is NMP, and the second polymerization reaction inducer is azobisisobutyronitrile AIBN.

[0127] The method for preparing the solid-state battery of this embodiment comprises the following steps:

[0128] (a) a first polymer matrix A polyvinylidene fluoride-hexafluoropropylene (7.56 g) was dissolved in a solvent A NMP (80 g) and stirred evenly, then a lithium salt A lithium tetrafluoroborate (6.0 g) was added and dispersed evenly at high speed, then an inorganic filler A LATP (31.14 g) and a solvent A NMP (100 g) were added to adjust the viscosity to 1000 mPa·s, and finally a second polymerization inducing agent AIBN (2.03 g) was added to obtain a rubber material A;

[0129] The sizing agent A is evenly coated on the surface of the positive electrode active material layer (ternary positive electrode material, NCM811) of the positive electrode sheet, the coating layer thickness is about 15 μm, and then dried to obtain a positive electrode sheet with a solid electrolyte layer A formed on the surface;

[0130] (b) dissolving the first polymer matrix B polyacrylonitrile (7.56 g) in the solvent B NMP (80 g) and stirring evenly, adding the lithium salt B lithium tetrafluoroborate (6.0 g) and dispersing evenly at high speed, adding the inorganic filler BLATP (31.14 g) and the solvent B NMP (100 g) to adjust the viscosity to 1700 mPa·s, and finally adding the second polymerization inducer AIBN (2.03 g) to obtain the rubber material B;

[0131] The glue B is evenly coated on the negative electrode active material layer (graphite is the active material) of the negative electrode sheet, the coating layer thickness is about 15 μm, and then dried to obtain a negative electrode sheet with a solid electrolyte layer B formed on the surface;

[0132] (c) A positive electrode sheet with a solid electrolyte layer A formed on the surface and a negative electrode sheet with a solid electrolyte layer B formed on the surface are stacked (13 positive electrode sheets and 14 negative electrode sheets), and the solid electrolyte layer A and the solid electrolyte layer B are located between two adjacent positive electrode sheets and negative electrode sheets and in direct contact, and then assembled, and a second polymerization reaction monomer 1,3-dioxolane (8.15 g) is added, and the injection amount of the second polymerization reaction monomer is 1.66 g / Ah. Pre-packaging, standing and soaking for 24 hours, and extracting excess 1,3-dioxolane by secondary packaging. Then, hot pressing is performed, that is, by applying a pressure of 0.8 MPa and heating at 60°C for 4 hours, so that 1,3-dioxolane can be fully polymerized at the interface where the solid electrolyte layer A contacts the solid electrolyte layer B to form an interface modification layer, thereby obtaining a solid-state battery.

[0133] Comparative Example 1

[0134] This comparative example provides a solid-state battery and a preparation method thereof. Except that no second polymerization reaction inducer is added to the solid electrolyte layer A and the solid electrolyte layer B, the rest of the preparation method and process parameters are the same as those in Example 1.

[0135] Comparative Example 2

[0136] This comparative example provides a solid-state battery, which has the same structure as Example 1, except that no second polymerization reaction inducer is added to the solid electrolyte layer A and the solid electrolyte layer B, and no interface modification layer is provided at the interface where the solid electrolyte layer A and the solid electrolyte layer B contact.

[0137] The preparation method of the solid-state battery in this comparative example is the same as that in Example 1, except that no second polymerization reaction inducer is added to the rubber material A in step (a), and no second polymerization reaction inducer is added to the rubber material A in step (b), and in step (c), the second polymerization reaction monomer is not injected after stacking and assembling the positive electrode sheet with the solid electrolyte layer A formed on the surface and the negative electrode sheet with the solid electrolyte layer B formed on the surface. Instead, the solid electrolyte layer A and the solid electrolyte layer B are pressed together by heating, the temperature is set to 120°C, the pressure is set to 1.5T, and the time is 15min.

[0138] Comparative Example 3

[0139] This comparative example provides a solid-state battery and a preparation method thereof, except that the second polymerization reaction inducer is not added to the solid electrolyte layer B, and the second polymerization reaction inducer AIBN (2.33 g) is added to the solid electrolyte layer A, and the rest of the preparation method and process parameters are the same as those in Example 1.

[0140] Comparative Example 4

[0141] This comparative example provides a solid-state battery and a preparation method thereof, except that the second polymerization reaction inducer is not added to the solid electrolyte layer A and the solid electrolyte layer B, but the second polymerization reaction inducer is injected together with the second polymerization reaction monomer 1,3-dioxolane, and the amount of the second polymerization reaction inducer AIBN used is 0.037 g. The rest of the preparation method and process parameters are the same as those in Example 1.

[0142] In order to compare the technical effects of the above embodiments and comparative examples, the following experimental examples are specially designed.

[0143] Experimental Example 1

[0144] The performance test of 4.9Ah all-solid-state soft-pack battery was carried out on the above-mentioned embodiment and comparative example, specifically including:

[0145] In the voltage range of 2.5-4.2V, the first charge and discharge test was carried out at 0.2C, and then a cycle test was carried out at 0.5C charging and 1C discharging for 200 cycles, and the capacity retention rate of the battery was recorded. The test results are shown in Table 1.

[0146] Table 1

[0147]

[0148] It can be seen from the examples and comparative examples in Table 1 that the addition of the second polymerization reaction inducer AIBN and the second polymerization reaction monomer DOL can effectively improve the battery performance, and the battery cycle performance is greatly improved, mainly because the defects of the composite solid electrolyte layer interface are improved. With the increase of the amount of the second polymerization reaction inducer AIBN, the battery performance decreases slightly, and excessive AIBN affects the battery performance; however, if too little or no AIBN is added, the battery first cycle performance can be exerted, but with the increase of the number of cycles, the capacity retention rate decreases, mainly because the second polymerization reaction monomer DOL is not completely polymerized, the degree of polymerization is low, and the second polymerization reaction monomer will exist in liquid form. The second polymerization reaction monomer in liquid form will corrode the solid electrolyte layer, resulting in a decrease in battery cycle performance.

[0149] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention are within the scope of protection of the pending claims of the present invention.

Claims

1. A solid-state battery, characterized in that: Include: A positive electrode sheet having a positive electrode active material layer coated on the surface and a solid electrolyte layer A coated on the surface of the positive electrode active material layer; and a negative electrode sheet having a negative electrode active material layer coated on the surface and a solid electrolyte layer B coated on the surface of the negative electrode active material layer; The positive electrode sheet and the negative electrode sheet are stacked in sequence, the solid electrolyte layer A and the solid electrolyte layer B are arranged between two adjacent positive electrode sheets and negative electrode sheets, and an interface modification layer is also arranged at the interface where the solid electrolyte layer A and the solid electrolyte layer B contact, and the interface modification layer is mainly formed by polymerization of the second polymerization reaction monomer; Wherein, the solid electrolyte layer A is mainly made of a first polymer matrix A, an inorganic filler A, a lithium salt A, a solvent A, and a second polymerization reaction inducer; The solid electrolyte layer B is mainly made of a first polymer matrix B, an inorganic filler B, a lithium salt B, a solvent B and a second polymerization reaction inducer; The second polymerization monomer is a monomer containing a polar group, capable of bulk polymerization and capable of reacting with Li + The coordinated polymer monomer, the polar group includes an ester group and / or an ether group.

2. The solid-state battery according to claim 1, characterized in that: The second polymerization monomer includes at least one of ethylene glycol methacrylate, vinyl ethylene carbonate, methyl methacrylate, 1,3-dioxolane or ethylene carbonate.

3. The solid-state battery according to claim 2, characterized in that: The second polymerization inducing agent includes azobisisobutyronitrile and / or dibenzoyl peroxide.

4. The solid-state battery according to claim 1, characterized in that: The first polymer matrix A and the first polymer matrix B are independently selected from at least one of polyethylene oxide, polyvinylidene fluoride, polyvinylidene fluoride-hexafluoropropylene, polyacrylonitrile, polymethyl methacrylate, polypropylene or polyvinyl chloride; And / or, the inorganic filler A and the inorganic filler B are independently selected from at least one of lithium lanthanum zirconium oxide, lithium lanthanum zirconium tantalum oxide, lithium lanthanum zirconium aluminum oxide, lithium lanthanum zirconium gallium oxide, lithium lanthanum titanium oxide, lithium aluminum germanium phosphate or lithium aluminum titanium phosphate; And / or, the lithium salt A and the lithium salt B are independently selected from at least one of lithium hexafluorophosphate, lithium tetrafluoroborate, lithium bis(trifluoromethylsulfonyl)imide or lithium perchlorate; And / or, the solvent A and the solvent B are independently selected from at least one of N-methylpyrrolidone and acetonitrile.

5. The solid-state battery according to any one of claims 1 to 4, characterized in that: The mass ratio of the first polymer matrix A, the inorganic filler A, the lithium salt A, the second polymerization reaction inducer and the solvent A is (2-30): (2-30): (2-15): (0.02-5): 100; And / or, the mass ratio of the first polymer matrix B, the inorganic filler B, the lithium salt B, the second polymerization reaction inducer and the solvent B is (2-30): (2-30): (2-15): (0.02-5):

100.

6. The method for preparing a solid-state battery according to any one of claims 1 to 5, characterized in that: The following steps are involved: (a) mixing and dispersing a first polymer matrix A, an inorganic filler A, a lithium salt A, a solvent A, and a second polymerization reaction inducer to obtain a rubber material A; Applying the sizing material A on the surface of the positive electrode active material layer of the positive electrode sheet, and then drying, so as to form a solid electrolyte layer A on the surface of the positive electrode active material layer of the positive electrode sheet; (b) mixing and dispersing a first polymer matrix B, an inorganic filler B, a lithium salt B, a solvent B, and a second polymerization reaction inducer to obtain a rubber material B; Applying the sizing material B on the surface of the negative electrode active material layer of the negative electrode sheet, and then drying, so as to form a solid electrolyte layer B on the surface of the negative electrode active material layer of the negative electrode sheet; (c) stacking a positive electrode sheet having a solid electrolyte layer A formed on its surface and a negative electrode sheet having a solid electrolyte layer B formed on its surface, and assembling them so that the solid electrolyte layer A and the solid electrolyte layer B are located between two adjacent positive electrode sheets and negative electrode sheets and in direct contact with each other to obtain an assembly; The second polymerization reaction monomer is injected into the assembly, and then allowed to soak. After the positive electrode and the negative electrode are fully soaked, the assembly is hot pressed to allow the second polymerization reaction monomer to polymerize at the interface where the solid electrolyte layer A contacts the solid electrolyte layer B to form an interface modification layer, thereby obtaining a solid-state battery.

7. The method for preparing a solid-state battery according to claim 6, characterized in that: In step (a), a first polymer matrix A, an inorganic filler A, a lithium salt A, and a solvent A are mixed and dispersed, the viscosity is controlled to be 50-3000 mPa·s, and then a second polymerization inducer is added to obtain a rubber material A; And / or, the coating thickness of the rubber material A is 3-50 μm.

8. The method for preparing a solid-state battery according to claim 6, characterized in that: In step (b), a first polymer matrix B, an inorganic filler B, a lithium salt B, and a solvent B are mixed and dispersed, the viscosity is controlled to be 50-3000 mPa·s, and then a second polymerization reaction inducer is added to obtain a rubber material B; And / or, the coating thickness of the rubber material B is 3-50 μm.

9. The method for preparing a solid-state battery according to any one of claims 6 to 8, characterized in that: In step (c), the injection amount of the second polymerization reaction monomer is 0.7-3.5 g / Ah; And / or, the static infiltration time is 12-72h; And / or, the hot pressing temperature is 50-90° C., the hot pressing pressure is 0.2-2 MPa, and the pressing time is 0.5-8 h.

10. Application of the solid-state battery according to any one of claims 1 to 5 or the solid-state battery prepared by the preparation method according to any one of claims 6 to 9 in the fields of electric vehicles, electronic communication equipment or aerospace vehicles.

Citation Information

Patent Citations

  • Double in-situ polymerization reaction preparation method of solid-state battery containing solid-state electrolyte

    CN110380111A

  • Solid electrolyte, preparation method thereof and solid-state battery

    CN113258132A

  • In-situ polymerization solid-state battery with multi-layer structure electrolyte and preparation method of in-situ polymerization solid-state battery

    CN114335716A

  • Integrally-designed positive and negative pole pieces, semi-solid-state battery and preparation method of semi-solid-state battery

    CN117613404A

  • Composite solid electrolyte as well as preparation method and application thereof

    CN118173864A