Long-circulation non-aqueous sodium-ion battery electrolyte and sodium-ion battery
By using mixed ester ether electrolyte and multiple anions in sodium ion batteries, the enrichment interface is constructed, and the problem of poor stability of the electrode-electrolyte interface of sodium ion battery is solved, the circulation performance and conductivity of the battery are improved, and the sodium ion is made The commercial application of batteries provides feasibility.
Patent Information
- Application Number
- CN202411549771.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-11-01
- Publication Date
- 2024-12-03
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
There is still room for improvement in the energy density and long cycle performance of sodium ion batteries. The electrode-electrolyte interface of the existing electrolyte is poor, and the NaF component is easily soluble in organic solvents during the cycle, resulting in unstable interface. .
Using a mixed ester ether electrolyte, anion enrichment interface is constructed by introducing a variety of anion and ether-based solvents, the long cycle performance of sodium ion batteries is improved, and film-forming additives are added to the electrolyte to enhance interface stability.
A wider electrochemical window, higher ionic conductivity and better cycling stability are achieved, providing a feasible solution for commercial application of sodium ion batteries.
Smart Images

Figure CN119069792A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of sodium ion batteries, and in particular relates to a long-cycle non-aqueous sodium ion battery electrolyte and a sodium ion battery. Background Art
[0002] Lithium-ion batteries have quickly occupied a core position in the 4C field due to their high energy density and long cycle life. However, in the face of the rising demand for secondary batteries in the global energy storage market, the limited lithium resources have greatly restricted the development of lithium-ion batteries. Sodium-ion batteries have become an alternative to lithium-ion batteries with great potential and objective prospects due to their abundant resource reserves, low manufacturing costs and better comprehensive performance. However, sodium-ion batteries still have a lot of room for improvement in energy density and long cycle performance.
[0003] As one of the important components of sodium ion batteries, electrolyte is an important factor in determining the composition and interface dynamics of the electrode-electrolyte interface. As one of the important solutions to improve the performance of sodium ion batteries, it has received widespread attention from researchers. At present, most of the electrolytes that have been commercially applied in the market are carbonate electrolytes. Carbonate electrolytes have good antioxidant properties. Since the commonly used ester-based electrolytes mainly belong to strong solvation electrolytes, their conductivity is high, but the electrochemical stability of the electrode-electrolyte interface derived from their solvents is poor. However, due to its good reduction stability, ether-based solvents can achieve preferential reduction of anions in sodium salts at the negative electrode interface, thereby obtaining a stable inorganic-rich interface, effectively improving the long-cycle stability of sodium ion batteries. A mixed ester-ether electrolyte proposed in the present invention effectively improves the oxidation stability of ether-based solvents and the cycle efficiency of sodium ion batteries through ester-based solvents, and effectively achieves a balance between anion-enhanced solvation structure and high ionic conductivity by introducing ether-based solvents with weak solvation characteristics into conventional ester electrolyte systems.
[0004] NaF is an important component of the electrode-electrolyte interface of high-performance sodium ion batteries. The SEI interface layer containing NaF can effectively improve the conductivity of Na+, stabilize the sodium metal negative electrode and reduce side reactions. However, the NaF component will dissolve in the organic solvent during the continuous cycle of the battery, resulting in the instability of the interface film. The present invention introduces more types of anions to form a rich inorganic interface with rich components, thereby improving the long-cycle performance of sodium ion batteries. Summary of the invention
[0005] The present invention aims to provide a method for preparing a long-cycle non-aqueous sodium ion battery electrolyte and its application. Based on a mixed ester-ether electrolyte with high ionic conductivity, a strategy of introducing multiple anions is proposed to construct an anion-enriched interface, thereby effectively improving the long-cycle performance of the sodium ion battery.
[0006] In this technical solution, two or more mixed ester ether solvents form a base solvent, on which a variety of anions are introduced, that is, two or two sodium salts are introduced, and finally common film-forming additives are added to form an electrolyte suitable for sodium ion batteries.
[0007] In this technical solution, the ester-based solvent is one or more of ethylene carbonate (EC), propylene carbonate (PC), butylene carbonate (BC), ethyl methyl carbonate (EMC), dimethyl carbonate (DMC), and diethyl carbonate (DEC).
[0008] In this technical solution, the ether-based solvent is one or more of ethylene glycol dimethyl ether (G1), diethylene glycol dimethyl ether (G2), triethylene glycol dimethyl ether (G3), tetraethylene glycol dimethyl ether (G4), polyethylene glycol diethyl ether (PEG), tetrahydrofuran (THF), 1,4-dioxane (1,4-DX), and 1,3-dioxolane (DOL).
[0009] In this technical solution, any one or more ether-based solvents with the above-mentioned solvation characteristics are introduced into a conventional ester solvent to form a base solvent.
[0010] In this technical solution, the sodium salt is selected from one or more of sodium perchlorate (NaClO4), sodium hexafluorophosphate (NaPF6), sodium bis(fluorosulfonyl)imide (NaFSI), sodium bis(trifluoromethanesulfonyl)imide (NaTFSI), sodium difluoro(oxalate)borate (NaDFOB), sodium trifluoromethanesulfonate (NaOTF), sodium tetrafluoroborate (NaBF4), sodium difluorophosphate (NaPO2F2), sodium bis(oxalyl)borate (NaBOB), and sodium nitrate (NaNO3).
[0011] In this technical solution, the film-forming electrolyte additives are one or more conventional film-forming additives such as vinylene carbonate (VC), fluoroethylene carbonate (FEC), and vinyl ethylene carbonate (VEC). Preferably, the mass of the additives accounts for 1 to 5% of the basic electrolyte.
[0012] In this technical solution, the sodium salt concentration in the medium- and long-cycle non-aqueous sodium ion battery electrolyte is 0.5 to 3 mol / L.
[0013] In some of the embodiments, in the long-cycle non-aqueous sodium ion battery electrolyte, the mass percentage of the sodium salt is 5 to 20 wt%, the mass percentage of the carbonate solvent is 40 to 60 wt%, the mass percentage of the ether-based solvent is 20 to 60 wt%, and the mass percentage of the additive is 0.5 to 10 wt%.
[0014] The present invention provides a sodium ion battery, which includes the above-mentioned long-cycle non-aqueous sodium ion battery electrolyte. Preferably, the sodium ion battery consists of a positive electrode sheet, a diaphragm, the long-cycle non-aqueous sodium ion battery electrolyte of the present invention, and a negative electrode sheet.
[0015] Preferably, the positive electrode is a high-loading Prussian blue (PB) (12 mg cm-2).
[0016] Preferably, the separator is cellulose.
[0017] Preferably, the negative electrode sheet is hard carbon.
[0018] The present invention also provides a method for preparing a long-cycle non-aqueous sodium ion battery electrolyte, comprising the following steps: 1) Under argon atmosphere, one or more organic solvents are fully mixed and stirred to obtain a base solvent; 2) dissolving one or more sodium salts into the base solvent obtained in step 1); 3) adding molecular sieves to the mother liquor obtained in step 2), allowing to stand for 8 hours, and finally removing the molecular sieves to obtain a purified solution; 4) dissolving the electrolyte additive into the purified solution obtained in step 3), and mixing them evenly to obtain a long-cycle non-aqueous sodium ion battery electrolyte.
[0019] Preferably, the molecular sieve is a 3 Å or 4 Å molecular sieve.
[0020] The beneficial effects of the present invention are: The present invention introduces ether-based solvents into conventional ester electrolyte systems, constructs an anion-enhanced solvation structure and improves the high ionic conductivity of the electrolyte. On this basis, more types of anions are introduced into the mixed ester ether electrolyte to construct a rich inorganic interface with rich components, thereby improving the long-cycle performance of sodium ion batteries. The present invention proposes a long-cycle non-aqueous sodium ion battery electrolyte that exhibits a wider electrochemical window, higher ionic conductivity and better cycle stability than traditional electrolytes, providing a feasible solution for the commercial application of sodium ion batteries. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1 The charge-discharge curves corresponding to 2 and 100 cycles of the HC||PB full battery at room temperature assembled with the electrolytes of Example 1 and Comparative Example 1; Figure 2 Long cycle performance of HC||PB full battery cycles assembled with electrolytes of Examples 1, 2, 3 and Comparative Examples 1, 2, 3, 4; Figure 3 is the electrochemical window of the electrolyte of Example 1 and Comparative Example 1 at room temperature; Figure 4 It is the ionic conductivity of the electrolyte of Example 1 and Comparative Examples 1 and 2 at -40°C to 90°C. DETAILED DESCRIPTION
[0022] The technical solution of the present invention is further described in detail by the following specific examples, but the present invention is not limited to the following examples.
[0023] Abbreviations Sodium hexafluorophosphate: NaPF6 Sodium perchlorate: NaClO4 Sodium difluoro(oxalato)borate: NaDFOB Sodium bis(fluorosulfonyl)imide: NaFSI Ethylene carbonate: EC Propylene carbonate: PC Ethylene glycol dimethyl ether: DME Diethylene glycol dimethyl ether: G2 Tetraethylene glycol dimethyl ether: G4 Dioxolane: DOL Vinylene carbonate: VC.
[0024] Example 1. This embodiment provides a sodium ion electrolyte, and its preparation method includes the following steps: adding 335.9 mgNaPF6 and 244.8 mg NaClO4 to 2 mL G2 and 2 mL PC to make the concentration 1 mol / L, and then adding 1% VC of the total mass of the electrolyte.
[0025] Example 2 The present embodiment provides a sodium ion electrolyte, and its preparation method includes the following steps: adding 335.9 mg NaPF6 and 351.8 mg NaDFOB to 2 mL G2 and 2 mL PC to make the concentration 1 mol / L, and then adding VC accounting for 1% of the total mass of the electrolyte.
[0026] Example 3 The present embodiment provides a sodium ion electrolyte, and its preparation method includes the following steps: adding 335.9 mg NaPF6 and 406.2 mg NaFSI to 2 mL G2 and 2 mL PC to make the concentration 1 mol / L, and then adding VC accounting for 1% of the total mass of the electrolyte.
[0027] Comparative Example 1 This embodiment provides a sodium ion electrolyte, and the preparation method thereof comprises the following steps: 671.8 mgNaPF6 is added to 2 mL G2 and 2 mL PC, and then VC accounting for 1% of the total mass of the electrolyte is added.
[0028] Comparative Example 2 This embodiment provides a sodium ion electrolyte, and the preparation method thereof comprises the following steps: 489.6 mg NaClO4 is added to 2 mL G2 and 2 mL PC, and then VC accounting for 1% of the total mass of the electrolyte is added.
[0029] Comparative Example 3 This embodiment provides a sodium ion electrolyte, and the preparation method thereof comprises the following steps: 703.6 mg NaDFOB is added to 2 mL G2 and 2 mL PC, and then VC accounting for 1% of the total mass of the electrolyte is added.
[0030] Comparative Example 4 This embodiment provides a sodium ion electrolyte, and the preparation method thereof comprises the following steps: 812.4 mg NaFSI is added to 2 mL G2 and 2 mL PC, and then VC accounting for 1% of the total mass of the electrolyte is added.
[0031] Comparative Example 5 This embodiment provides a sodium ion electrolyte, and the preparation method thereof comprises the following steps: 489.6 mg NaClO4 is added to 2 mL DOL and 2 mL PC, and then VC accounting for 1% of the total mass of the electrolyte is added.
[0032] Comparative Example 6 This embodiment provides a sodium ion electrolyte, and the preparation method thereof comprises the following steps: 489.6mg NaClO4 Add to 2 mL G4 and 2 mL PC and then add VC accounting for 1% of the total mass of the electrolyte.
[0033] Comparative Example 7 This embodiment provides a sodium ion electrolyte, and the preparation method thereof comprises the following steps: 489.6 mg NaClO4 is added to 2 mL G2 and 2 mL EC, and then VC accounting for 1% of the total mass of the electrolyte is added.
[0034] Comparative Example 8 This embodiment provides a sodium ion electrolyte, and the preparation method thereof comprises the following steps: 671.8 mg NaPF6 is added to 4 ml G2 and then VC accounting for 1% of the total mass of the electrolyte is added.
[0035] Comparative Example 9 This embodiment provides a sodium ion electrolyte, and the preparation method thereof comprises the following steps: 671.8 mg NaPF6 is added to 4 ml PC and then VC accounting for 1% of the total mass of the electrolyte is added.
[0036] Comparative Example 10 This embodiment provides a sodium ion electrolyte, and the preparation method thereof comprises the following steps: 489.6 mg NaClO4 is added to 4 ml G2 and then VC accounting for 1% of the total mass of the electrolyte is added.
[0037] Comparative Example 11 This embodiment provides a sodium ion electrolyte, and the preparation method thereof comprises the following steps: 489.6 mg NaClO4 is added to 4 ml PC and then VC accounting for 1% of the total mass of the electrolyte is added.
[0038] Normal temperature cycle performance test: At 25°C, the assembled sodium ion battery was activated at 0.1C for 1 cycle, charged at 1C constant current to 3.7 V, and discharged at 1C constant current to 1.5 V. (1C = 150 mAh g-1) The first cycle coulomb efficiency is the first cycle discharge capacity corresponding to 0.1C / first cycle discharge capacity, and its calculation formula is: First cycle discharge capacity / first cycle discharge capacity×100%; The average coulomb efficiency calculation formula is: The sum of 100 cycles of coulombic efficiency / number of cycles (100) × 100%; After 100 cycles of charge / discharge, the 100th cycle capacity retention rate is calculated using the following formula: Capacity retention rate: cycle discharge capacity / first cycle discharge capacity after activation × 100%, and the number of cycles corresponding to a capacity retention rate of 80% is calculated.
[0039] Table 1 shows the performance test results of batteries assembled with the electrolytes of Examples 1, 2, 3 and Comparative Examples 1-11.
[0040] As can be seen from the above table, through comparative examples 1, 2 and 8, 9, 10, and 11, it can be seen that compared with a single solvent, the mixed ester ether system has better cycle performance, and the capacity retention rate after 551 cycles is still 80%; from comparative examples 2, 5, 6, and 7, it can be seen that through preliminary screening of the ester ether system, PC / G2 has better cycle performance; through experimental examples 1-3 and comparative examples 1-4, it can be seen that the introduction of polyanions can improve the cycle performance of sodium ion full batteries.
[0041] Figure 1 The charge-discharge curves corresponding to 2 and 100 cycles of the HC||PB full battery at room temperature assembled with the electrolytes of Example 1 and Comparative Example 1; Figure 2 Long cycle performance of HC||PB full battery cycles assembled with electrolytes of Examples 1, 2, 3 and Comparative Examples 1, 2, 3, 4; Figure 3 is the electrochemical window of the electrolyte of Example 1 and Comparative Example 1 at room temperature; Figure 4 is the ionic conductivity of the electrolytes of Example 1 and Comparative Examples 1 and 2 at -40°C to 90°C; Figure 1 The charge and discharge curves corresponding to 2 and 100 cycles of the HC||PB full battery assembled with the electrolytes of Example 1 and Comparative Example 1; Figure 2 Long cycle performance of HC||PB high-load sodium ion batteries assembled with electrolytes of Examples 1-3 and Comparative Examples 1-4 at 25°C. Figure 1 and Figure 2 It can be seen that under the test conditions of 1.5-3.7 V and 1C (1C=150 mAh g-1), the introduction of polyanions in the mixed ester ether system can effectively improve the cycling performance of high-load sodium batteries, and the capacity retention rate can be achieved at 80% after 500 cycles.
[0042] Figure 3 It is the electrochemical window of the electrolyte of Example 1 and Comparative Example 2 at room temperature 25°C. Figure 4 The ionic conductivity of the electrolytes of Example 1 and Comparative Examples 1 and 2 at -40°C to 90°C, the experimental results show that the electrolytes introducing more anions have a wider electrochemical window and higher ionic conductivity than the electrolytes of a single salt system.
[0043] Cycle Test No. First-cycle Coulomb efficiency Average Coulombic efficiency Capacity retention rate is 80% corresponding to the number of cycles Example 1 85.98 99.95 551 Example 2 85.86 99.91 345 Example 3 84.70 99.96 434 Comparative Example 1 84.96 99.76 297 Comparative Example 2 84.54 99.95 319 Comparative Example 3 84.54 99.85 277 Comparative Example 4 85.04 99.95 300 Comparative Example 5 78.22 98.64 79 Comparative Example 6 83.31 99.78 108 Comparative Example 7 81.06 99.36 61 Comparative Example 8 80.21 99.74 75 Comparative Example 9 84.47 99.89 348 Comparative Example 10 81.20 99.72 112 Comparative Example 11 84.18 99.89 351
[0044] The above is only a preferred embodiment of the present invention, which further illustrates and describes the technical solution of the present invention, and is not intended to limit the protection scope of the present invention. Any equivalent replacement or partial modification using the contents of the present invention specification and drawings shall be deemed to be within the patent protection scope of the present invention.
Claims
1. A long-cycle non-aqueous sodium ion battery electrolyte, characterized in that: The invention comprises sodium salt, organic solvent and conventional film-forming additives, wherein the organic solvent comprises ether-based solvent and carbonate-based solvent, the carbonate-based solvent comprises one or more combinations of cyclic carbonate solvent and chain carbonate solvent, the cyclic carbonate solvent is one or more combinations of ethylene carbonate (EC), propylene carbonate (PC) and butylene carbonate (BC), and the chain carbonate solvent is one or more combinations of ethyl methyl carbonate (EMC), dimethyl carbonate (DMC) and diethyl carbonate (DEC).
2. A long-cycle non-aqueous sodium ion battery electrolyte according to claim 1, characterized in that: The ether-based solvent is one or more of ethylene glycol dimethyl ether (G1), diethylene glycol dimethyl ether (G2), triethylene glycol dimethyl ether (G3), tetraethylene glycol dimethyl ether (G4), polyethylene glycol diethyl ether (PEG), tetrahydrofuran (THF), 1,4-dioxane (1,4-DX), and 1,3-dioxolane (DOL).
3. The long-cycle non-aqueous sodium ion battery electrolyte according to claim 1, characterized in that: The sodium salt is one or more of sodium perchlorate (NaClO4), sodium hexafluorophosphate (NaPF6), sodium tetrafluoroborate (NaBF4), sodium bis(fluorosulfonyl)imide (NaFSI), sodium bis(trifluoromethanesulfonyl)imide (NaTFSI), sodium difluoro(oxalate)borate (NaDFOB), sodium trifluoromethanesulfonate (NaOTF), sodium difluorophosphate (NaPO2F2), sodium bis(oxalato)borate (NaBOB), and sodium nitrate (NaNO3).
4. The long-cycle non-aqueous sodium ion battery electrolyte according to claim 1, characterized in that: The conventional film-forming additive is at least one of fluoroethylene carbonate (FEC), vinylene carbonate (VC), and vinyl ethylene carbonate (VEC).
5. A long-cycle non-aqueous sodium ion battery electrolyte according to any one of claims 1 to 4, characterized in that: The mass percentages of sodium salt, carbonate solvent, ether-based solvent and conventional film-forming additives are: 5-20 wt%: 40-60 wt%: 20-60 wt%: 0.5-10 wt%.
6. A use of a long-cycle non-aqueous sodium ion battery electrolyte according to claim 5 in a sodium ion battery, characterized in that: A positive electrode comprising a high-load positive electrode active material, a negative electrode comprising a high-load negative electrode active material, a separator and an electrolyte; the positive electrode active material is one or more of sodium vanadium phosphate, a polyanion compound, a layered oxide, and a Prussian blue analogue; the negative electrode active material is one or more of hard carbon, soft carbon, graphite, bismuth alloy, and metallic sodium; the separator comprises one or more of a cellulose separator, a polyolefin separator, and a glass fiber separator.
Citation Information
Patent Citations
Electrolyte, preparation method thereof and sodium ion battery
CN116895843A
Double-salt ether-based low-temperature / high-voltage electrolyte, sodium-ion battery containing electrolyte and preparation method of sodium-ion battery
CN117317369A
Application of neutral red in sodium ion battery
CN118198499A
Sodium secondary battery, battery module, battery pack, and electric device
CN118352605A
Cited By
Low-concentration electrolyte suitable for prussian blue and hard carbon sodium-ion battery and application of low-concentration electrolyte
CN119447476A