Battery
By using specific content of fluorinated nitrile compounds in lithium-ion batteries and optimizing the structure of aluminum-plastic films, the problem of contact damage between electrolyte and aluminum-plastic films is solved, the circulation and safety performance of the battery is improved, and the thermal stability is achieved Sex and safety.
Patent Information
- Application Number
- CN202411368564.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-29
- Publication Date
- 2024-12-03
AI Technical Summary
During the charging and discharging process of existing lithium-ion batteries, the electrolyte and the aluminum-plastic film are easily damaged when they come into contact with each other, resulting in poor circulation and safety performance.
By adding a specific content of fluorinated nitrile compound to the electrolyte and setting an appropriate thickness and structure on the aluminum-plastic film, the matching relationship between the fluorinated nitrile compound and the aluminum-plastic film is ensured, and a protective layer is formed to prevent polymer decomposition and leakage. The design of the electrode glue and aluminum plastic film is optimized to improve the thermal stability and safety of the battery.
It significantly improves the circulation and safety performance of lithium-ion batteries, including high-temperature cycle stability, anti-needle performance and thermal safety performance, extends the battery life and reduces the risk of safety accidents.
Smart Images

Figure CN119069822A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of new energy technology, and in particular to a battery. Background Art
[0002] As a widely used energy storage device, lithium-ion batteries are now widely used in various smart electronic products, such as mobile phones, laptops, digital cameras, unmanned aerial vehicles, sweeping robots, smart watches and other devices. Lithium-ion batteries usually include a battery cell, an electrolyte, and an aluminum-plastic film, wherein the battery cell and the electrolyte are located in a cavity formed by the aluminum-plastic film.
[0003] During the charge and discharge process of the existing battery, the electrolyte contacts the inside of the aluminum-plastic film, which easily damages the aluminum-plastic film, which is not conducive to the cycle performance and safety performance of the battery. Summary of the invention
[0004] The invention provides a battery having excellent cycle performance and safety performance.
[0005] The present invention provides a battery, comprising a battery core, an electrolyte, and an aluminum-plastic film encapsulating the battery core and the electrolyte, wherein the electrolyte comprises a fluoronitrile compound;
[0006] The mass percentage D% of the fluoronitrile compound in the electrolyte and the thickness L of the aluminum-plastic film satisfy: 0.5wt%≤D%≤15wt%;
[0007] 50≤L≤130μm;
[0008] 0.005≤D / L≤0.27.
[0009] The battery as described above, wherein in the electrolyte, 3wt%≤D%≤10wt%;
[0010] And / or, the fluoronitrile compound comprises at least one of the following compounds:
[0011]
[0012] The battery as described above, wherein the aluminum-plastic film is provided with a side seal, the width of the side seal is Z, and the mass percentage content D% of the fluoronitrile compound in the electrolyte satisfies:
[0013] 1.2≤D / Z≤8.8;
[0014] The unit of Z is mm.
[0015] The battery as described above, wherein 1.5 mm ≤ Z ≤ 10 mm, preferably, 1.5 mm ≤ Z ≤ 6.5 mm.
[0016] In the battery as described above, the aluminum-plastic film is further provided with a top sealing edge, and the width H of the top sealing edge satisfies: 1.5 mm≤H≤10 mm, preferably, 1.5 mm≤H≤6.5 mm.
[0017] The battery as described above, wherein the aluminum-plastic film comprises a first layer, an aluminum layer and a second layer which are stacked, and the aluminum-plastic film satisfies at least one of the following conditions:
[0018] a. The thickness L1 of the first layer satisfies: 20μm≤L1≤50μm;
[0019] b. The thickness of the aluminum layer L2 satisfies: 30μm≤L2≤60μm;
[0020] c. The thickness L3 of the second layer satisfies: 10 μm ≤ L3 ≤ 30 μm;
[0021] d. The first layer comprises at least one of polypropylene, polyethylene and polyethylene-polypropylene copolymer;
[0022] e. The second layer includes nylon.
[0023] The battery as described above, wherein the battery further comprises a pole ear and a pole piece, wherein the pole ear is arranged on the pole piece,
[0024] The tab is provided with tab glue, and the tab glue is bonded to the aluminum-plastic film;
[0025] Preferably, the tab glue comprises a first glue layer, a second glue layer, and a third glue layer which are stacked in sequence.
[0026] The battery as described above, wherein the battery satisfies at least one of the following conditions:
[0027] f. The first adhesive layer comprises at least one of propylene-ethylene copolymer, maleic anhydride modified polypropylene, and metallocene modified polypropylene;
[0028] g. The second adhesive layer comprises at least one of polypropylene and anhydride grafted modified polypropylene;
[0029] h. The third adhesive layer comprises at least one of propylene-ethylene copolymer, maleic anhydride modified polypropylene, and metallocene modified polypropylene;
[0030] m. The melting point T1 of the first adhesive layer is less than or equal to the melting point T2 of the second adhesive layer;
[0031] n. The melting point T3 of the third adhesive layer is lower than the melting point T2 of the second adhesive layer.
[0032] The battery as described above, wherein the pole lug has a central axis in a direction perpendicular to the pole piece, and a distance S1 between the central axis and the first end of the pole piece and a distance S2 between the central axis and the second end of the pole piece satisfy: 0.5≤S1 / S2≤5;
[0033] Preferably, 1≤S1 / S2≤2.
[0034] The battery as described above, wherein the thickness G of the battery satisfies: 1mm≤G≤105mm.
[0035] The invention can improve the cycle performance and safety performance of the battery by making the content of the fluoronitrile compound in the electrolyte of the battery and the thickness of the aluminum-plastic film meet a specific relationship. BRIEF DESCRIPTION OF THE DRAWINGS
[0036] In order to more clearly illustrate the technical solutions in the embodiments of the present invention or related technologies, the following briefly introduces the drawings required for use in the embodiments of the present invention or related technologies. Obviously, the drawings described below are only some embodiments of the present invention, and for ordinary technicians in this field, other drawings can be obtained based on these drawings without creative work.
[0037] Figure 1 Schematic diagram of the structure of aluminum-plastic film in some embodiments of the present invention;
[0038] Figure 2 It is a schematic diagram of the positional relationship between the tab and the tab glue in the first view of the present invention;
[0039] Figure 3 It is a schematic diagram of the positional relationship between the tab and the tab glue in the second view of the present invention;
[0040] Figure 4 Schematic diagram of the structure of the pole piece in some embodiments of the present invention.
[0041] Description of reference numerals:
[0042] 1: concave part;
[0043] 2: Side sealing;
[0044] 3: Ear glue;
[0045] 4: Ear;
[0046] 5: first end;
[0047] 6: Second end;
[0048] 11; first floor;
[0049] 12; second floor;
[0050] 13; Aluminum layer;
[0051] 31: first adhesive layer;
[0052] 32: second adhesive layer;
[0053] 33: The third adhesive layer. DETAILED DESCRIPTION
[0054] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0055] Figure 1 Schematic diagram of the structure of aluminum-plastic film in some embodiments of the present invention. Figure 1 As shown, the present invention provides a battery, comprising a battery cell, an electrolyte, and an aluminum-plastic film encapsulating the battery cell and the electrolyte, wherein the electrolyte comprises a fluoronitrile compound;
[0056] The mass percentage D% of the fluoronitrile compound in the electrolyte and the thickness L of the aluminum-plastic film satisfy:
[0057] 0.5wt%≤D%≤15wt%;
[0058] 50≤L≤130μm;
[0059] 0.005≤D / L≤0.27.
[0060] The aluminum-plastic film of the present invention has a recess 1, and the battery cell and the electrolyte are accommodated in the recess 1. It can be understood that the battery cell of the present invention includes a positive electrode sheet, a negative electrode sheet, and a separator. In the battery of the present invention, the positive electrode sheet, the separator, and the negative electrode sheet can be stacked to form a battery cell of a laminated structure, and then the battery cell is placed in the recess 1 of the aluminum-plastic film, and the electrolyte is injected into the recess 1, and the formation and sealing are performed, so that the battery cell and the electrolyte are encapsulated in the aluminum-plastic film, and finally the battery is formed; the positive electrode sheet, the separator, and the negative electrode sheet can also be stacked, and then wound to form a battery cell, and then the battery cell is placed in the recess 1 of the aluminum-plastic film, and the electrolyte is injected into the recess 1, and the formation and sealing are performed, so that the battery cell and the electrolyte are encapsulated in the aluminum-plastic film, and finally the battery is formed. In some embodiments, the aluminum-plastic film can be punched to form a recess 1 in the aluminum-plastic film.
[0061] The separator is used to separate the positive electrode sheet from the negative electrode sheet and provide a channel for lithium ion migration. The separator of the present invention can be selected from polypropylene separator and / or polyethylene separator.
[0062] The fluoronitrile compound of the present invention is a compound including a fluorine substituent and a cyano group. Since the fluorine substituent of the fluoronitrile compound is electronegative, it is easy to combine with hydrogen atoms in the polyolefin in the inner layer of the aluminum-plastic film (the side contacting the electrolyte) to form an aggregated fluoronitrile compound liquid film layer, which can isolate other electrolyte components from penetrating into the aluminum-plastic film, prevent the polymer in the inner layer of the aluminum-plastic film from decomposing and aging, thereby preventing the aluminum-plastic film from cracking and leaking when being punctured by an external needle; in addition, the fluoronitrile compound can also improve the oxidation resistance of the electrolyte, prevent the electrolyte from having a side reaction with the aluminum-plastic film at high temperature, and improve the stability of the aluminum-plastic film; at the same time, the cyano group in the fluoronitrile compound can absorb proton hydrogen in the electrolyte, reduce the acidity of the electrolyte, and improve the cycle stability of the battery.
[0063] The inventors found in the study that when D / L is less than 0.005, the aluminum-plastic film is too thin or the content of the fluoronitrile compound is too little, and the polymer on the aluminum-plastic film cannot be effectively prevented from decomposing and aging. When D / L is greater than 0.27, the aluminum-plastic film is too thick to conduct heat in time, or the excessive content of the fluoronitrile compound leads to an increase in the internal resistance of the battery and an increase in heat generation. When the mass percentage of the fluoronitrile compound in the electrolyte and the thickness of the aluminum-plastic film meet the above relationship, the fluoronitrile compound can better match the aluminum-plastic film, further preventing the aluminum-plastic film from rupturing and causing safety accidents, and improving the cycle and safety performance of the battery.
[0064] Therefore, the present invention can improve the high temperature cycle stability, anti-puncture performance and thermal safety performance of the lithium ion battery through the interaction between the specific content of the aluminum-plastic film and the fluoronitrile compound in the electrolyte.
[0065] The present invention does not specifically limit the fluorinated nitrile compound, as long as it includes a fluorine substituent and a cyano group, it is within the scope of protection of the present invention. In some embodiments, the structural formula of the fluorinated nitrile compound is as shown in Formula 1:
[0066]
[0067] Wherein, R is selected from substituted or unsubstituted C1-C30 alkyl, substituted or unsubstituted C2-C30 alkenyl, substituted or unsubstituted C2-C30 alkynyl, substituted or unsubstituted C6-C60 aryl, carbonyl or ester; wherein R includes at least one fluorine substituent.
[0068] Exemplarily, the fluoronitrile compound is selected from the compounds shown in the following structures:
[0069]
[0070] The inventors found in their research that as the content of fluorine substituents in the fluoronitrile compound increases, the fluoronitrile compound has a stronger electronegativity, which can further prevent the electrolyte from oxidative decomposition under high voltage; and the fluoronitrile compound has a stronger interaction with the aluminum-plastic film, which helps to further improve the cycle performance and safety performance of the battery;
[0071] When the fluoronitrile compound contains a double bond, the electrolyte containing the fluoronitrile compound is more likely to polymerize into a film on the surface of the negative electrode, forming a stable SEI film on the surface of the negative electrode;
[0072] In the present invention, when the mass percentage of the fluoronitrile compound in the electrolyte and the thickness of the aluminum-plastic film meet a certain range, the fluoronitrile compound can better match the aluminum-plastic film with each other, thereby improving the cycle performance and safety performance of the battery.
[0073] In some embodiments of the present invention, in the electrolyte, 3wt%≤D%≤10wt%. When the content of the fluoronitrile compound in the electrolyte meets the above range, the fluoronitrile compound can more fully protect the inner layer of the aluminum-plastic film, reduce the corrosion of the electrolyte to the aluminum-plastic film at high temperature, and thus improve the thermal stability and safety of the lithium-ion battery.
[0074] In some embodiments of the present invention, the aluminum-plastic film includes a first layer 11, an aluminum layer 13, and a second layer 12 which are stacked, and the aluminum-plastic film satisfies at least one of the following conditions:
[0075] a. The thickness L1 of the first layer 11 satisfies: 20 μm ≤ L1 ≤ 50 μm;
[0076] b. The thickness L2 of the aluminum layer 13 satisfies: 30 μm ≤ L2 ≤ 60 μm;
[0077] c. The thickness L3 of the second layer 12 satisfies: 10 μm ≤ L3 ≤ 30 μm;
[0078] d. The first layer 11 includes at least one of polypropylene, polyethylene and ethylene-propylene copolymer;
[0079] e. The second layer 12 comprises nylon.
[0080] Among them, the first layer 11 is located inside the aluminum-plastic film, close to the electrolyte, and has excellent compatibility with the electrolyte. In addition, the first layer 11 has excellent chemical stability and heat sealing properties, and can melt and bond under the action of heat, thereby realizing the sealing of the battery; the second layer 12 has excellent impact resistance, puncture resistance, heat resistance, friction resistance and insulation, which can ensure the stability and safety of the battery; the aluminum layer 13 has excellent moisture and humidity resistance, reduces the physical damage to the battery caused by the outside world, and the aluminum layer 13 also has plasticity, which is conducive to the processing and forming of the aluminum-plastic film.
[0081] Furthermore, when the thickness L1 of the first layer 11 satisfies: 20 μm ≤ L1 ≤ 50 μm, the chemical stability and heat sealing property of the aluminum-plastic film can be improved while ensuring the energy density of the battery, thereby improving the sealing property of the battery;
[0082] When the thickness L2 of the aluminum layer 13 satisfies: 30 μm ≤ L2 ≤ 60 μm, the plasticity, moisture resistance and humidity resistance of the aluminum-plastic film can be improved while ensuring the energy density of the battery, thereby improving the safety performance and service life of the battery;
[0083] When the thickness L3 of the second layer 12 satisfies: 10 μm≤L3≤30 μm, the battery's impact resistance, puncture resistance, heat resistance, friction resistance and insulation can be improved while ensuring the battery's energy density, thereby further improving the battery's stability and safety.
[0084] In some embodiments of the present invention, the aluminum-plastic film includes a side seal 2,
[0085] The width Z of the side seal 2 and the mass percentage D% of the fluoronitrile compound in the electrolyte satisfy:
[0086] 0.25≤D / Z≤8.8.
[0087] In the present invention, the fluoronitrile compound is gathered on the polymer surface inside the aluminum-plastic film, the molecular movement of the fluoronitrile compound is reduced, thereby improving its thermal stability, and can improve the gas generation caused by the fluoronitrile compound at high temperature. When the width of the side seal 2 and the mass percentage of the fluoronitrile compound in the electrolyte meet the above relationship, the problem of cracking of the side seal 2 of the aluminum-plastic film caused by high-temperature gas generation can be better suppressed, the heat sealing property and stability of the aluminum-plastic film are improved, the performance of the battery under high temperature and high pressure is improved, and the service life of the battery is extended.
[0088] Furthermore, when 1.5 mm ≤ Z ≤ 10 mm, the aluminum-plastic film can have better sealing performance and weather resistance. Preferably, 1.5 mm ≤ Z ≤ 6.5 mm.
[0089] In some embodiments of the present invention, the aluminum-plastic film is further provided with a top seal, and when the width H of the top seal satisfies: 1.5 mm ≤ H ≤ 10 mm, the sealing performance and weather resistance of the aluminum-plastic film can be further improved. Preferably, 1.5 mm ≤ H ≤ 6.5 mm.
[0090] Figure 2 It is a schematic diagram of the positional relationship between the tab and the tab glue in the first view of the present invention; Figure 3 It is a schematic diagram of the positional relationship between the tab and the tab glue in the second view of the present invention; Figure 4 Schematic diagram of the structure of the pole piece in some embodiments of the present invention. Figure 2-4As shown, in some embodiments of the present invention, the battery further includes a pole ear 4 and a pole piece, and the pole ear 4 is arranged on the pole piece.
[0091] The tab 4 is provided with tab glue 3, and the tab glue 3 is bonded to the aluminum-plastic film.
[0092] In the present invention, a pole piece (including a positive pole piece and a negative pole piece) is provided with a pole ear 4, one end of the pole ear 4 is connected to the pole piece, and the other end of the pole ear 4 is connected to an external circuit. The pole ear 4 of the present invention is provided with a pole ear glue 3, the pole ear glue 3 is bonded to the aluminum-plastic film, and the pole ear 4 is led out of the aluminum-plastic film.
[0093] In practical applications, the ear glue 3 is heated to be hot-melt-sealed and bonded with the aluminum-plastic film to form a sealing structure, which can prevent battery leakage.
[0094] Furthermore, the ear glue 3 includes a first glue layer 31, a second glue layer 32, and a third glue layer 33 which are stacked in sequence. In actual application, the first glue layer 31 of the ear glue 3 is bonded to the aluminum-plastic film, and the third glue layer 33 is bonded to the ear 4. The first glue layer 31, the second glue layer 32 and the third glue layer 33 are heated and hot-melt sealed with the aluminum-plastic film to form a sealing structure, thereby further preventing battery leakage.
[0095] In some embodiments of the present invention, the battery satisfies at least one of the following conditions:
[0096] f. The first adhesive layer 31 includes at least one of propylene-ethylene copolymer, maleic anhydride modified polypropylene, and metallocene modified polypropylene;
[0097] g. The second adhesive layer 32 includes at least one of polypropylene and anhydride grafted modified polypropylene;
[0098] h. The third adhesive layer 33 includes at least one of propylene-ethylene copolymer, maleic anhydride modified polypropylene, and metallocene modified polypropylene;
[0099] m. The melting point T1 of the first adhesive layer 31 is less than or equal to the melting point T2 of the second adhesive layer 32;
[0100] n. The melting point T3 of the third adhesive layer 33 is lower than the melting point T2 of the second adhesive layer 32 .
[0101] Specifically, the fluorinated nitrile compound in the electrolyte can form hydrogen bonds with the modified or unmodified polyolefin polymers in the first adhesive layer 31, the second adhesive layer 32 and the third adhesive layer 33, thereby preventing the acidic components generated by the decomposition of the hydrogen atom components of the electrolyte at high temperature from corroding the first adhesive layer 31, the second adhesive layer 32 and the third adhesive layer 33, thereby improving the high temperature performance of the battery.
[0102] Furthermore, when the melting point T1 of the first adhesive layer 31, the melting point T2 of the metal layer, and the melting point T3 of the third layer satisfy:
[0103] T2 ≥ T1; and / or,
[0104] When T2>T3, the overall fusion between the glue layers of the ear glue 3 and the ear glue 3 and the aluminum-plastic film can be improved to prevent the decomposition of the ear glue 3 glue layer or the ear glue 3 and the aluminum-plastic film due to the large difference in melting points during the thermal runaway test; at the same time, the fluoronitrile compound can improve the stability of the electrolyte, prevent the aluminum-plastic film in contact with the first glue layer 31 and / or the third glue layer 33 from melting and cracking under the thermal runaway state, and further improve the thermal safety performance of the battery. In some embodiments, the melting point of the first glue layer 31 can be 80-165°C, the melting point of the second glue layer 32 can be 130°C-170°C, and the melting point of the third glue layer 33 can be 80-140°C.
[0105] In some embodiments of the present invention, the pole lug 4 has a central axis in a direction perpendicular to the pole piece, and the distance S1 between the central axis and the first end 5 of the pole piece and the distance S2 between the central axis and the second end 6 of the pole piece satisfy: 0.5≤S1 / S2≤5.
[0106] In the present invention, the first end 5 of the pole piece refers to the pole piece along the length direction ( Figure 2 The second end 6 of the pole piece refers to the end of the pole piece that is close to the central axis of the pole ear 4 along the length direction.
[0107] When the distance between the central axis of the pole ear 4 and the first end 5 of the pole piece, and the distance between the central axis and the second end of the pole piece satisfy the above relationship, the electron transmission path can be shortened, the internal resistance and polarization of the battery can be reduced, the temperature rise of the battery can be reduced, and electrons can be uniformly transmitted to the active layer to prevent current instability, maintain the solvation structure of the fluoronitrile compound in the electrolyte and the inner surface of the aluminum-plastic film, stabilize the fluoronitrile compound to form a uniform liquid film on the inner surface of the aluminum-plastic film, and improve the stability and safety of the battery.
[0108] Furthermore, 1≤S1 / S2≤2.
[0109] In some embodiments of the present invention, when the thickness G of the battery satisfies: 1 mm ≤ G ≤ 105 mm, the electrolyte permeability of the battery can be improved while ensuring the energy density of the battery, thereby improving the cycle performance of the battery.
[0110] It is understood that the electrolyte of the present invention also includes a lithium salt and a non-aqueous organic solvent.
[0111] Specifically, the lithium salt may include one or more of lithium bis(trifluoromethylsulfonyl)imide, lithium hexafluorophosphate (LiPF6), lithium difluorophosphate (LiPO2F2), lithium difluorooxalatoborate (LiDFOB), lithium bis(trifluoromethylsulfonyl)imide, lithium difluorobis(oxalatophosphate), lithium tetrafluoroborate, lithium bis(oxalatoborate), lithium hexafluoroantimonate, lithium hexafluoroarsenate, lithium bis(trifluoromethylsulfonyl)imide, lithium bis(pentafluoroethylsulfonyl)imide, tris(trifluoromethylsulfonyl)methyllithium or lithium bis(trifluoromethylsulfonyl)imide.
[0112] The non-aqueous organic solvent may include carbonate solvents and / or carboxylate solvents. The carbonate solvents are selected from one or more of fluoro or unsubstituted ethylene carbonate (EC), propylene carbonate (PC), dimethyl carbonate, diethyl carbonate (DEC), and ethyl methyl carbonate; the carboxylate solvents are selected from one or more of fluoro or unsubstituted propyl acetate, n-butyl acetate, isobutyl acetate, n-amyl acetate, isoamyl acetate, propyl propionate (PP), ethyl propionate (EP), methyl butyrate, and ethyl butyrate.
[0113] The electrolyte may further include functional additives, wherein the functional additives include one or more of nitrile additives, cyclic carbonate additives, and cyclic sultone additives.
[0114] Specifically, the nitrile additive may include at least one of ethylene glycol bis(propionitrile) ether, adiponitrile, succinonitrile, 1,3,6-hexanetrinitrile, glutaronitrile, trans-butenedinitrile, and trans-hexenedinitrile;
[0115] The cyclic carbonate additive comprises at least one of fluoroethylene carbonate, difluoroethylene carbonate, vinylene carbonate and vinylethylene carbonate;
[0116] The cyclic sultone additive may be at least one selected from 1,3-propane sultone, 1,3-propylene sultone, 2,4-butane sultone, 1,4-butane sultone, and methylene methane disulfonate.
[0117] In some embodiments, the content of the functional additive in the electrolyte can be 3wt% to 20wt%, for example, it can be any one of 3wt%, 5wt%, 8wt%, 10wt%, 12wt%, 14wt%, 16wt%, 18wt%, 20wt% or a range consisting of any two of them.
[0118] In the present invention, the positive electrode sheet includes a positive electrode current collector and a positive electrode active layer located on at least one surface of the positive electrode current collector, wherein the positive electrode current collector can be selected from aluminum foil; the positive electrode active layer can include, by mass percentage, 80% to 99.8% of positive electrode active material, 0.1% to 10% of conductive agent, and 0.1% to 10% of binder. Preferably, the positive electrode active layer includes, by mass percentage, 90% to 99.6% of positive electrode active material, 0.2% to 5% of conductive agent, and 0.2% to 5% of binder.
[0119] The positive electrode active material of the present invention may include at least one of lithium cobalt oxide, lithium nickel oxide, lithium manganese oxide, lithium nickel cobalt manganese oxide, lithium nickel cobalt aluminum oxide, lithium nickel manganese oxide, lithium iron phosphate and ternary materials. In some embodiments, lithium cobalt oxide may be doped with elements to obtain a positive electrode active material with better internal structural stability, wherein the doping element is selected from one or more of Ti, Mg, Al and Ni.
[0120] The conductive agent may include at least one of conductive carbon black, acetylene black, Ketjen black, conductive graphite, conductive carbon fiber, carbon nanotubes, metal powder, and carbon fiber.
[0121] The binder may include at least one of sodium carboxymethyl cellulose, styrene-butadiene latex, polytetrafluoroethylene, and polyethylene oxide.
[0122] In some embodiments, the positive electrode sheet can be prepared by the following method: the positive electrode active material, the conductive agent and the binder are dispersed in a solvent to obtain a positive electrode slurry, and then the positive electrode slurry is applied to at least one surface of the positive electrode collector, and the positive electrode sheet can be obtained after drying.
[0123] The negative electrode sheet includes a negative electrode current collector and a negative electrode active layer located on at least one surface of the negative electrode current collector, wherein the negative electrode current collector can be selected from copper foil; the negative electrode active layer includes, by mass percentage: 80% to 99.8% of negative electrode active material, 0.1% to 10% of conductive agent, and 0.1% to 10% of binder. Preferably, the negative electrode active layer includes, by mass percentage: 90% to 99.6% of negative electrode active material, 0.2% to 5% of conductive agent, and 0.2% to 5% of binder.
[0124] The negative electrode active material includes at least one of artificial graphite, natural graphite, mesophase carbon microspheres, hard carbon, soft carbon, silicon-carbon material, and silicon-oxygen material;
[0125] The conductive agent includes at least one of conductive carbon black, acetylene black, Ketjen black, conductive graphite, conductive carbon fiber, carbon nanotubes, metal powder, and carbon fiber;
[0126] The binder includes at least one of sodium carboxymethyl cellulose, styrene-butadiene latex, polytetrafluoroethylene and polyethylene oxide.
[0127] In some embodiments, the negative electrode sheet can be prepared by the following method: the negative electrode active material, the conductive agent and the binder are dispersed in a solvent to form a negative electrode slurry; the negative electrode slurry is then coated on at least one surface of the negative electrode collector, and the negative electrode sheet can be obtained after drying and rolling.
[0128] The technical solution of the present invention will be further described below in conjunction with specific embodiments.
[0129] Example 1
[0130] The battery of this embodiment is prepared by a method comprising the following steps:
[0131] 1) Preparation of positive electrode
[0132] Lithium cobalt oxide, binder polyvinylidene fluoride (PVDF 500), and conductive carbon material (Super P) are mixed in N-methylpyrrolidone (NMP) solvent at a weight ratio of 97.5:2:2.5, and continuously stirred in a stirrer to form a uniform, flowing positive electrode slurry;
[0133] The positive electrode slurry was coated on both surfaces of an aluminum foil with a thickness of 10 μm, placed in a vacuum oven at 120° C. and dried for 6 h, and then rolled and cut to obtain a positive electrode sheet.
[0134] 2) Preparation of negative electrode
[0135] Graphite, conductive carbon black (Ketjen black), sodium carboxymethyl cellulose (CMC), and styrene-butadiene rubber are mixed in a water solvent in a weight ratio of 98:1:0.5:0.5, and continuously stirred in a stirrer to form a uniform, flowing negative electrode slurry;
[0136] The negative electrode slurry was coated on both surfaces of a copper foil with a thickness of 10 μm, placed in a vacuum oven at 120° C. for drying for 6 h, and then rolled and cut to obtain a negative electrode sheet.
[0137] 3) Preparation of electrolyte
[0138] In a glove box filled with argon (water <1ppm, oxygen <1ppm), ethylene carbonate, propylene carbonate, propyl propionate and ethyl propionate solvents were mixed into a uniform solvent in a mass ratio of 20:10:50:20, 14.5wt% of LiPF6, 2wt% of 1,3-propane sultone, and 3wt% of 1,3,6-hexanetrinitrile were slowly added, and a certain proportion of fluoronitrile compound A4 (specific parameters are shown in Table 1) was added, and after stirring evenly, an electrolyte was obtained.
[0139] 4) Preparation of batteries
[0140] A positive electrode ear is arranged on the positive electrode sheet in step 1), a negative electrode ear is arranged on the negative electrode sheet in step 2), and the positive electrode sheet provided with the positive electrode ear, the separator, and the negative electrode sheet provided with the negative electrode ear are stacked and arranged, and then wound to obtain a battery cell; the battery cell is placed in an aluminum-plastic film, the positive electrode ear and the negative electrode ear are led out of the aluminum-plastic film, the electrolyte in step 3) is injected into the aluminum-plastic film, and then vacuum packaging, room temperature standing, and high-temperature formation are performed to obtain a battery;
[0141] Wherein, both the positive and negative ears are provided with ear glue, and the ear glue includes a first glue layer, a second glue layer and a third glue layer stacked, the first glue layer is bonded to the aluminum-plastic film, and the third glue layer is bonded to the ear; the melting point of the first glue layer is 120±5°C, and the material is maleic anhydride modified polypropylene; the melting point of the second glue layer is 160±5°C, and the material is polypropylene; the melting point of the third glue layer is 120±5°C, and the material is maleic anhydride modified polypropylene;
[0142] The width of the top sealing edge of the aluminum-plastic film is 3.5 mm. The aluminum-plastic film includes a first layer, an aluminum layer and a second layer which are stacked. The first layer is an inner layer (close to the electrolyte) and is made of ethylene-propylene copolymer. The second layer is an outer layer and is made of nylon.
[0143] Other parameters are shown in Table 1.
[0144] Examples 2-31, 35, Comparative Examples 1-3
[0145] The preparation methods of the batteries of Examples 2-31, 35 and Comparative Examples 1-3 are substantially the same as that of Example 1, and the differences are shown in Table 1.
[0146] Embodiment 32
[0147] The preparation method of the battery of this embodiment is basically the same as that of embodiment 1, except that:
[0148] 4) Preparation of batteries
[0149] The positive electrode sheet in step 1), the separator, and the negative electrode sheet in step 2) are stacked to obtain a battery cell with a laminate structure.
[0150] Examples 33-34
[0151] The preparation method of the battery of Examples 33-34 is basically the same as that of Example 33, and the differences are shown in Table 1.
[0152] Performance Testing
[0153] The following performance tests were performed on the batteries in the examples and comparative examples, and the results are shown in Table 2;
[0154] 1) High temperature cycle test experiment
[0155] The battery was placed in an oven at a temperature of (55±2)℃, and charged to 4.45V at a current density of 1.2C (cut-off current of 0.05C). After the battery was fully charged, it was left for 5 minutes, and then discharged at a current density of 0.5C (cut-off voltage of 3.0V). The discharge capacity was recorded as the initial capacity Q1. When the cycle reached 300 cycles, the last discharge capacity of the battery was recorded as Q2.
[0156] Capacity retention rate (%) = Q2 / Q1×100%.
[0157] 2) Furnace temperature test experiment
[0158] Fully charge the battery at an ambient temperature of (25±2)℃, then place it horizontally on a tray in an oven, set the equipment to heat up to 130℃ at a heating rate of (5±2)℃ / min, and place it in this environment for 60min. After completion, observe the battery status after standing for 2h. When the battery does not leak, catch fire, or explode, it can be judged as passed.
[0159] 3) Acupuncture test
[0160] Fully charge the battery at an ambient temperature of (25±2)℃, and test the center of the battery cell with a 2.5mm stainless steel needle at a speed of 100mm / sec. Penetrate the center of the battery cell in a direction perpendicular to the battery plate. The puncture position should be close to the geometric center of the punctured surface (the needle stays in the battery). Record the battery status. The battery has passed if it does not catch fire or explode.
[0161] 4) Temperature shock test
[0162] The batteries obtained in the above embodiments and comparative examples were fully charged at an ambient temperature of (25±2)°C, and the battery core was placed in a test box, heated to 72±2°C and left to stand for 6 hours, and then cycled 10 times. After standing for 30 minutes, the battery core was cooled to -40±2°C and left to stand for 6 hours, and then cycled 10 times. After completion, the battery status was observed after being left to stand for 2 hours at an ambient temperature of (25±2)°C. When the battery does not leak, catch fire, or explode, it can be judged as passed.
[0163] Table 1
[0164]
[0165]
[0166] Table 2
[0167]
[0168]
[0169]
[0170] As can be seen from Table 2, the battery in the embodiment of the present invention has more excellent cycle performance, furnace temperature, needle puncture and temperature shock performance, indicating that the present invention can improve the cycle performance and safety performance of the battery by matching the content of the fluoronitrile compound in the electrolyte with the thickness of the aluminum-plastic film;
[0171] Further, it can be seen from Examples 5, 6 and 9 that by further selecting the content of the fluoronitrile compound in the electrolyte, the cycle performance, furnace temperature and temperature shock performance of the battery can be further improved without affecting the acupuncture performance of the battery; in particular, it can be seen from Examples 5 and 6 that by further selecting the content of the fluoronitrile compound in the electrolyte, the width of the side sealing edge of the aluminum-plastic film and the ratio of the fluoronitrile compound in the electrolyte can be regulated to further improve the cycle performance, furnace temperature and temperature shock performance of the battery;
[0172] It can be seen from Examples 1, 10, 11 and 12 that the cycle performance, furnace temperature, needle puncture and temperature shock performance of the battery can be further improved by selecting the thickness of the first layer in the aluminum-plastic film.
[0173] It can be seen from Examples 1, 13, 14 and 15 that by further selecting the thickness of the aluminum layer in the aluminum-plastic film, a battery with better cycle performance, furnace temperature, needle puncture and temperature shock performance can be obtained;
[0174] It can be seen from Examples 1, 16, 17 and 18 that by further selecting the thickness of the second layer in the aluminum-plastic film, the cycle performance, needle puncture and temperature impact performance of the battery can be further improved;
[0175] It can be seen from Example 19 and Examples 21 and 24 that the cycle performance, furnace temperature and temperature shock performance of the battery can be further improved by selecting the side sealing width of the aluminum-plastic film;
[0176] It can be seen from Examples 1, 25 and 26 that by further selecting the position of the tabs in the battery, the cycle performance, furnace temperature, acupuncture and temperature shock performance of the battery can be improved; it can be seen from Examples 33, 34 and 32 that by further selecting the position of the tabs in the battery, the cycle performance, furnace temperature and acupuncture performance of the battery can be improved;
[0177] It can be seen from Examples 1, 27 and 28 that when the thickness of the battery meets a specific range, the battery has better cycle performance, furnace temperature, needle puncture and temperature shock performance;
[0178] It can be seen from Example 1 and Example 31 that when the content of fluorine substituents in the fluorinated nitrile compound increases, the cycle performance of the battery can be further improved.
[0179] Each embodiment in this specification is described in a related manner, and the same or similar parts between the embodiments can be referred to each other, and each embodiment focuses on the differences from other embodiments. The above are only preferred embodiments of the present invention and are not intended to limit the scope of protection of the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention are included in the scope of protection of the present invention.
Claims
1. A battery, characterized in that: It comprises a battery cell, an electrolyte, and an aluminum-plastic film encapsulating the battery cell and the electrolyte, wherein the electrolyte comprises a fluoronitrile compound; The mass percentage D% of the fluoronitrile compound in the electrolyte and the thickness L of the aluminum-plastic film satisfy: 0.5wt%≤D%≤15wt%; 50≤L≤130μm; 0.005≤D / L≤0.
27.
2. The battery according to claim 1, characterized in that In the electrolyte, 3wt%≤D%≤10wt%; And / or, the fluoronitrile compound comprises at least one of the following compounds:
3. The battery according to any one of claims 1 to 2, characterized in that: The aluminum-plastic film is provided with a side seal, the width of the side seal is Z, and the mass percentage content D% of the fluoronitrile compound in the electrolyte satisfies: 0.25≤D / Z≤8.8; The unit of Z is mm.
4. The battery according to claim 3, characterized in that 1.5mm≤Z≤10mm, preferably, 1.5mm≤Z≤6.5mm.
5. The battery according to any one of claims 1 to 4, characterized in that: The aluminum-plastic film is also provided with a top edge seal, and the width H of the top edge seal satisfies: 1.5mm≤H≤10mm, preferably, 1.5mm≤H≤6.5mm.
6. The battery according to claim 1, characterized in that The aluminum-plastic film comprises a first layer, an aluminum layer and a second layer which are stacked, and the aluminum-plastic film satisfies at least one of the following conditions: a. The thickness L1 of the first layer satisfies: 20μm≤L1≤50μm; b. The thickness of the aluminum layer L2 satisfies: 30μm≤L2≤60μm; c. The thickness L3 of the second layer satisfies: 10 μm ≤ L3 ≤ 30 μm; d. The first layer comprises at least one of polypropylene, polyethylene and ethylene-propylene copolymer; e. The second layer includes nylon.
7. The battery according to claim 1, characterized in that The battery further comprises a pole ear and a pole piece, wherein the pole ear is arranged on the pole piece. The tab is provided with tab glue, and the tab glue is bonded to the aluminum-plastic film; Preferably, the tab glue comprises a first glue layer, a second glue layer, and a third glue layer which are stacked in sequence.
8. The battery according to claim 7, characterized in that The battery meets at least one of the following conditions: f. The first adhesive layer comprises at least one of propylene-ethylene copolymer, maleic anhydride modified polypropylene, and metallocene modified polypropylene; g. The second adhesive layer comprises at least one of polypropylene and anhydride grafted modified polypropylene; h. The third adhesive layer comprises at least one of propylene-ethylene copolymer, maleic anhydride modified polypropylene, and metallocene modified polypropylene; m. The melting point T1 of the first adhesive layer is less than or equal to the melting point T2 of the second adhesive layer; n. The melting point T3 of the third adhesive layer is lower than the melting point T2 of the second adhesive layer.
9. The battery according to claim 7 or 8, characterized in that: The pole lug has a central axis in a direction perpendicular to the pole piece, and a distance S1 between the central axis and the first end of the pole piece and a distance S2 between the central axis and the second end of the pole piece satisfy: 0.5≤S1 / S2≤5; Preferably, 1≤S1 / S2≤2.
10. The battery according to any one of claims 1 to 9, characterized in that: The thickness G of the battery satisfies: 1mm≤G≤105mm.
Citation Information
Patent Citations
Aluminum-plastic film and flexible package battery
CN111640883A
Battery and electronic equipment
CN114597495A
Electrolyte and battery
CN115295876A
Electrolyte and lithium ion battery
CN115986212A
Negative plate and manufacturing method thereof and lithium ion battery as well as preparation method and application thereof
WO2021037266A1