Preparation method of covalent organic framework / polyacrylamide composite hydrogel electrolyte

By using covalent organic framework/polyacrylamide composite hydrogel electrolyte in aqueous zinc ion batteries, the problems of poor mechanical properties and low ionic conductivity of polymer hydrogel electrolyte are solved, and high cycle stability and electricity are achieved The improvement of chemical performance ensures the stable operation of the battery under high current density.

CN119069834APending Publication Date: 2024-12-03JIANGSU UNIV OF SCI & TECH
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411129833.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-16
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

The existing polymer hydrogel electrolytes have problems with poor mechanical properties and low ionic conductivity in aqueous zinc ion batteries, resulting in poor cell cycle stability, especially under low temperature and dry conditions, which are prone to brittle cracking and dendrite growth.

Method used

The preparation method of covalent organic framework/polyacrylamide composite hydrogel electrolyte is adopted. By mixing COF colloid with acrylamide, a covalent organic framework with high crystallinity and layered sheet structure is formed, thereby enhancing the mechanical strength and ions of the electrolyte. Conductivity and regulate the transmission path of zinc ions to avoid dendrites.

Benefits of technology

It significantly improves the mechanical strength and ionic conductivity of the composite hydrogel electrolyte, inhibits the growth of zinc dendrites, ensures the cycling stability and high electrochemical reversibility of the battery, and can maintain a capacity of 94.6% at high current density. Rate and stabilize the cycle 1000 times.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119069834A_ABST
    Figure CN119069834A_ABST
Patent Text Reader

Abstract

The invention discloses a covalent organic framework / polyacrylamide composite hydrogel electrolyte preparation method, which comprises: (1) adding acrylamide and a cross-linking agent to a ZnSO4 electrolyte, adding a COF colloid, stirring, and carrying out ultrasonic dissolution to obtain a solution A; (2) adding an initiator into the ZnSO4 electrolyte to obtain a solution B; adding the solution B into the solution A to form a uniform polymer precursor mixed solution; and (3) injecting the polymer precursor mixed solution into a mold, and standing at the temperature not higher than 80 DEG C to obtain the polyacrylamide composite hydrogel electrolyte containing the covalent organic framework. The composite gel electrolyte has the advantages of being high in mechanical strength, good in ionic conductivity and capable of effectively hindering growth of zinc dendrites, so that the water-based zinc ion battery has good cycle stability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a method for preparing a covalent organic skeleton / polyacrylamide composite hydrogel electrolyte. Background Art

[0002] In recent years, aqueous zinc ion batteries (AZIBs) with aqueous solution as electrolyte system have the advantages of intrinsic safety, low cost, large theoretical capacity, and environmental friendliness, becoming an ideal choice for high-safety energy storage devices. Among them, quasi-solid-state AZIBs based on hydrogel electrolytes have the characteristics of good flexibility and safety, which have attracted widespread attention. The commonly used hydrogel electrolytes mainly include the following:

[0003] Polyvinyl alcohol (PVA)-based hydrogel electrolytes, PVA hydrogels have good mechanical properties and biocompatibility, but their ionic conductivity is low, especially at low temperatures, resulting in unsatisfactory electrochemical performance. In addition, PVA is prone to swelling or dissolution after long-term use, which affects the stability of the electrolyte. Polyacrylamide (PAM)-based hydrogel electrolytes, PAM hydrogels have relatively low mechanical strength and are prone to brittle cracking, especially under dry or low temperature conditions. In addition, the ionic conductivity of PAM-based electrolytes is also low, which cannot meet the needs of efficient zinc-ion batteries. Polyacrylic acid (PAA)-based hydrogel electrolytes, PAA hydrogels have high ionic conductivity, but their mechanical properties are poor, especially durability and toughness. In addition, PAA is easily degraded under alkaline or acidic conditions, resulting in insufficient stability of the electrolyte. Carboxymethyl cellulose (CMC)-based hydrogel electrolytes, CMC hydrogels have good biocompatibility and water retention capacity, but their mechanical strength and ionic conductivity are not high, especially under high current density.

[0004] In summary, existing polymer hydrogel electrolytes generally have two major disadvantages: poor mechanical properties and low ionic conductivity. These disadvantages limit the widespread application of hydrogel electrolytes in aqueous zinc-ion batteries, especially when high energy density and long cycle life are required. Summary of the invention

[0005] Purpose of the invention: The purpose of the present invention is to provide a covalent organic skeleton / polyacrylamide composite hydrogel electrolyte, which can solve the problems of poor mechanical properties, low ionic conductivity, and easy to cause Zn dendrites and parasitic reactions during battery cycling, resulting in poor battery cycling stability in existing polymer hydrogel electrolytes; another purpose of the present invention is to provide a method for preparing the above-mentioned composite hydrogel electrolyte.

[0006] Technical solution: The method for preparing the composite hydrogel electrolyte of the present invention comprises the following steps:

[0007] (1) adding acrylamide and a crosslinking agent into a ZnSO4 electrolyte, and then adding COF colloid thereto, stirring and ultrasonically dissolving, to obtain a solution A;

[0008] (2) adding an initiator to a ZnSO4 electrolyte to obtain a solution B; adding the solution B to the solution A to form a uniform polymer precursor mixed solution;

[0009] (3) Injecting the polymer precursor mixed solution into a mold and allowing it to stand at a temperature not higher than 80 degrees Celsius to obtain a polyacrylamide composite hydrogel electrolyte containing a covalent organic skeleton.

[0010] Wherein, in step (1), the concentration of ZnSO4 electrolyte is 2 mol / L.

[0011] Wherein, in step (1), the method for preparing COF colloid comprises the following steps:

[0012] (1.1) adding melamine and 1,4,5,8-naphthalenetetracarboxylic anhydride to N-methylpyrrolidone, reacting in a high pressure reactor at 160-200° C. for 72-74 hours to obtain product A;

[0013] (1.2) washing and drying the product A to obtain a polyimide covalent organic framework material B;

[0014] (1.3) Add the covalent organic framework material B to deionized water, perform ultrasonication and centrifugal stripping to obtain a covalent organic framework COF colloid. The molecular structure of the obtained covalent organic framework COF is:

[0015]

[0016] The COF microstructure prepared by the method of the present invention is a graphene-like lamellar structure, and the lamellar structure can effectively improve the mechanical properties of the polymer hydrogel electrolyte, thereby improving the cycle stability of the polymer hydrogel electrolyte.

[0017] Wherein, in step (1), the cross-linking agent is N,N-methylenebisacrylamide; the amount of the cross-linking agent added is 0.07% of the mass of acrylamide.

[0018] Wherein, in step (1), the mass volume ratio of acrylamide to COF colloid is 1 g:50-200 μL; and the solid content of the COF colloid is 0.2 mg / mL.

[0019] Wherein, in step (1), the mass volume ratio of acrylamide to ZnSO4 electrolyte is 1g:3mL.

[0020] Wherein, in step (2), the initiator is ammonium persulfate or potassium persulfate; the amount of the initiator added is 0.45% of the mass of acrylamide.

[0021] Wherein, in step (3), the standing time is 10 to 20 minutes.

[0022] Wherein, in step (3), the thickness of the composite hydrogel electrolyte is 0.5 to 1 mm.

[0023] The composite hydrogel electrolyte prepared by the method comprises a three-dimensional network structure formed by copolymerization and cross-linking of acrylamide; COF nanoparticles are embedded in the three-dimensional network structure.

[0024] The structure of the composite hydrogel electrolyte is:

[0025]

[0026] The Zn-NVO button cell assembled with the above composite hydrogel electrolyte, ammonium vanadate (NVO) positive electrode and zinc foil negative electrode exhibits stable electrochemical performance.

[0027] Since the covalent organic framework COF has high crystallinity and lamellar structure and has a regular pore structure, it can effectively improve the mechanical strength (high toughness) and ionic conductivity of the composite hydrogel electrolyte (unlike a single PAM polymer electrolyte, which transports ions in the chain through a hopping mechanism, the well-arranged structure in COF acts as a host and provides a one-dimensional channel for ion transport). In addition, the covalent organic framework COF can regulate the transmission path of zinc ions so that they are evenly distributed on the negative electrode surface, avoiding dendrite growth caused by excessive local zinc ion concentration (COF can affect the transmission of zinc ions at the molecular level and play a role in directional conduction), making zinc deposition more uniform and hindering the growth of zinc dendrites, thereby giving the battery good cycle stability.

[0028] Beneficial effects: Compared with the prior art, the present invention has the following significant advantages: in view of the problems that the traditional PAM hydrogel electrolyte has poor mechanical properties, low ionic conductivity, and a large amount of active water still exists in the hydrogel electrolyte, which will cause Zn dendrites and parasitic reactions and thus affect the cycle stability, the present invention adopts a self-made covalent organic framework COF colloid and mixes it with acrylamide to synthesize a composite hydrogel electrolyte, and utilizes the high crystallinity and lamellar structure of the covalent organic framework COF to effectively improve the mechanical strength of the composite hydrogel electrolyte; utilizes the well-ordered pore structure of the covalent organic framework COF to provide more channels for the migration of zinc ions, thereby greatly improving the ionic conductivity of the composite hydrogel electrolyte. The composite hydrogel electrolyte of the present invention not only has a tensile strength of 163kPa and an elongation at break of 993%, but also has a strength of 21.7mS cm -1The high ionic conductivity of COF / PAM can effectively inhibit the growth of zinc dendrites. The Zn-NVO button cell assembled with COF / PAM can -1 The high current density still has stable cycling performance, and after 1000 cycles, it can still maintain 83.3mAh g -1 The specific capacity and capacity retention rate are 94.6%, indicating its excellent electrochemical reversibility. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] Figure 1 The digital photo (a) of the composite hydrogel electrolyte obtained in Example 1 and the SEM image (b) after freeze-drying;

[0030] Figure 2 1 is the stress-strain curve of the hydrogel electrolyte obtained in Example 1 and Comparative Example 1;

[0031] Figure 3 Impedance diagrams of the stainless steel gasket / / hydrogel electrolyte / / stainless steel gasket battery obtained in Example 1 and Comparative Example 1;

[0032] Figure 4 The Zn / / Zn symmetric battery test results of the hydrogel obtained in Comparative Example 1 (a) and the SEM image of the cross section of the zinc foil after cycling (b);

[0033] Figure 5 The Zn / / Zn symmetric battery test results of the hydrogel obtained in Example 1 (a) and the SEM image of the cross section of the zinc foil after cycling (b);

[0034] Figure 6 The test results of the Zn / / Zn symmetric battery at different current densities in Example 1;

[0035] Figure 7 The test results of the Zn-NVO button cell assembled with the composite hydrogel electrolyte of Example 1 after 1000 cycles at a current density of 5 A / g;

[0036] Figure 8 This is the TEM image of the PI-COF powder prepared in Example 1. DETAILED DESCRIPTION

[0037] Example 1

[0038] The preparation method of the covalent organic skeleton / polyacrylamide composite hydrogel electrolyte of the present invention comprises the following steps:

[0039] (1) 2 g of acrylamide was dissolved in 6 mL of 2 mol / L ZnSO4 electrolyte, 1.4 mg of crosslinking agent N,N-methylenebisacrylamide and 200 μL of COF colloid were added thereto, and dissolved by ultrasonic stirring to obtain solution A; the solid content of COF colloid was 0.2 mg / mL;

[0040] (2) adding 9 mg of initiator ammonium persulfate to 3 mL of 2 mol / L ZnSO4 electrolyte, and dissolving by ultrasonic stirring to obtain solution B; adding solution B to solution A and stirring thoroughly to form a uniform polymer precursor mixed solution;

[0041] (3) The polymer precursor mixture obtained in step (2) is injected into a polytetrafluoroethylene mold and allowed to stand at 80° C. for 10 minutes to obtain a polyacrylamide composite hydrogel electrolyte containing a covalent organic skeleton.

[0042] Among them, the COF colloid was synthesized by Schiff base reaction, specifically: first, 1,4,5,8-naphthalenetetracarboxylic anhydride (0.7905g) and melamine (0.25g) were added to 20mL N-methylpyrrolidone, and ultrasonicated for 30min to form a transparent solution; the transparent solution was transferred to a high-pressure reactor and reacted at 200°C for 72 hours to obtain a brown-red product; the brown-red product was washed with NMP, DMF, H2O and ethanol in sequence to obtain a brown-red solid powder; finally, in a tube furnace, heated at 300°C for 8 hours with flowing nitrogen to obtain PI-COF powder; 2mg of PI-COF powder was taken, added to 10mL of deionized water and ultrasonicated, and centrifuged to finally obtain PI-COF colloid with a concentration of 0.2mg / mL.

[0043] It is used as an electrolyte in ss / / ss symmetric batteries to calculate the ionic conductivity, in Zn / / Zn symmetric batteries to characterize the inhibitory effect on zinc dendrites, and in Zn-NVO button batteries to characterize their cycling stability.

[0044] (ss stands for stainless steel sheet).

[0045] Example 2

[0046] The preparation method of Example 2 is the same as that of Example 1, except that the amount of COF colloid added is 100 μL, and other parameters remain unchanged.

[0047] Example 3

[0048] The preparation method of Example 3 is the same as that of Example 1, except that the amount of COF colloid added is 300 μL, and other parameters remain unchanged.

[0049] Example 4

[0050] The preparation method of Example 4 is the same as that of Example 1, the only difference being that the amount of COF colloid added is 400 μL, and the other parameters remain unchanged.

[0051] Example 5

[0052] The preparation method of Example 5 is the same as that of Example 1, except that the amount of COF colloid added is 500 μL, and other parameters remain unchanged.

[0053] Comparative Example 1

[0054] The preparation method of Comparative Example 1 is the same as that of Example 1, except that COF colloid is not added, and other parameters remain unchanged.

[0055] pass Figure 1 It can be seen that the composite hydrogel electrolyte prepared in Example 1 presents a multi-level gradient pore structure. This gradient pore structure can form a continuous transition from large pores to small pores in the hydrogel, which helps to optimize the ion transmission path. The large pores allow the electrolyte solution to penetrate and distribute quickly, while the small pores can provide a higher ion transmission channel, thereby balancing the rapid transmission and local efficient ion conductivity. This structure helps to reduce the resistance of the electrolyte, improve the overall ion transmission efficiency, and thus enhance the electrochemical performance of the battery. During the charge and discharge process, the electrode material will produce a volume change due to the deposition or deintercalation of zinc ions, which may cause cracking or peeling of the electrode material; the gradient pore structure can provide better mechanical support and stress buffering capacity for the electrode material, the large pores provide space to accommodate volume expansion, and the small pores enhance the mechanical stability, thereby effectively reducing the mechanical stress of the electrode and extending the cycle life of the battery.

[0056] pass Figure 2 It can be seen that the tensile strength, elastic modulus and elongation at break of the composite hydrogel electrolyte prepared in Example 1 are greatly improved compared with those in Comparative Example 1.

[0057] Figure 3 Impedance diagrams of the stainless steel gasket / / hydrogel electrolyte / / stainless steel gasket battery obtained in Example 1 and Comparative Example 1; it can be seen that the volume resistance of Example 1 is reduced and the ionic conductivity is improved. The fitting circuit calculates that the ionic conductivity of the composite hydrogel electrolyte of Example 1 is 21.7 mS / cm, while the ionic conductivity of Comparative Example 1 is only 10.5 mS / cm.

[0058] Figure 4 The Zn / / Zn symmetric battery test results of the hydrogel obtained in Comparative Example 1 and the SEM image of the cross section of the zinc foil after cycling are shown in Figure 1. Figure 4 It can be seen that the Zn / / Zn symmetric battery has a short circuit after 479 hours of cycling; SEM analysis of the zinc sheet after cycling shows a large number of zinc dendrite protrusions.

[0059] Figure 5 The Zn / / Zn symmetric battery test results of the hydrogel obtained in Example 1 and the SEM image of the cross section of the zinc foil after cycling are shown in FIG. Figure 5 It can be seen that the Zn / / Zn symmetric battery remains stable after cycling for more than 1000 h without short circuit or voltage polarization (at 1 mA cm -2 At a current density of , the Zn / / Zn symmetric battery exhibits a consistent low polarization voltage of less than 100 mV for more than 1000 hours), which indicates that the composite hydrogel electrolyte of the present invention has high cycle stability; SEM analysis of the zinc sheet after the Zn / / Zn symmetric battery cycle shows that the surface of the zinc sheet remains smooth after the cycle, confirming that it can effectively inhibit the growth of zinc dendrites.

[0060] Figure 6 The Zn / / Zn symmetric battery test at different current densities in Example 1 is shown in Figure 1. When the current density increases from 0.5 to 10 mA / cm 2 The polarization voltage remains below 170 mV, confirming that the electrolyte is capable of achieving stable Zn deposition / stripping behavior.

[0061] Figure 7 The Zn-NVO button cell assembled with the composite hydrogel electrolyte of Example 1 was tested for 1000 cycles at a current density of 5 A / g. The cell had good cycle stability and maintained a capacity of 83.3 mAh g after 1000 cycles. -1 The specific capacity and capacity retention rate are 94.6%.

Claims

1. A method for preparing a covalent organic framework / polyacrylamide composite hydrogel electrolyte, characterized in that: The steps include: (1) adding acrylamide and a crosslinking agent into a ZnSO4 electrolyte, and then adding COF colloid thereto, stirring and ultrasonically dissolving, to obtain a solution A; (2) adding an initiator to a ZnSO4 electrolyte to obtain a solution B; adding solution B to solution A to form a uniform polymer precursor mixture; (3) Injecting the polymer precursor mixed solution into a mold and allowing it to stand at high temperature to obtain a polyacrylamide composite hydrogel electrolyte containing a covalent organic skeleton.

2. The method for preparing the composite hydrogel electrolyte according to claim 1, characterized in that: In step (1), the concentration of the ZnSO4 electrolyte is 2 to 3 mol / L.

3. The method for preparing the composite hydrogel electrolyte according to claim 1, characterized in that: In step (1), the cross-linking agent is N,N-methylenebisacrylamide; the amount of the cross-linking agent added is 0.07-0.075% of the mass of acrylamide.

4. The method for preparing the composite hydrogel electrolyte according to claim 1, characterized in that: In step (1), the mass volume ratio of acrylamide to COF colloid is 1 g: 50-200 μL.

5. The method for preparing the composite hydrogel electrolyte according to claim 4, characterized in that: The preparation method of COF colloid comprises the following steps: (1.1) adding melamine and 1,4,5,8-naphthalenetetracarboxylic anhydride to N-methylpyrrolidone, reacting in a high pressure reactor at 160-200° C. for 72-74 hours to obtain product A; (1.2) washing and drying the product A to obtain a polyimide covalent organic framework material B; (1.3) Adding the covalent organic framework material B into deionized water, ultrasonicating and centrifuging to obtain a covalent organic framework COF colloid; the solid content of the COF colloid is 0.2 to 0.25 mg / mL.

6. The method for preparing the composite hydrogel electrolyte according to claim 1, characterized in that: In step (1), the mass volume ratio of acrylamide to ZnSO4 electrolyte is 1g:3-5mL.

7. The method for preparing the composite hydrogel electrolyte according to claim 1, characterized in that: In step (2), the initiator is ammonium persulfate or potassium persulfate; the amount of the initiator added is 0.45-0.50% of the mass of acrylamide.

8. The method for preparing the composite hydrogel electrolyte according to claim 1, characterized in that: In step (3), the mixture is allowed to stand at a temperature not higher than 80° C. for 10 to 20 minutes.

9. The method for preparing the composite hydrogel electrolyte according to claim 1, characterized in that: In step (3), the thickness of the composite hydrogel electrolyte is 0.5 to 1 mm.

10. The method for preparing the composite hydrogel electrolyte according to claim 9, characterized in that: The composite hydrogel electrolyte comprises a three-dimensional network structure formed by copolymerization and cross-linking of acrylamide; COF nanoparticles are embedded in the three-dimensional network structure.

Citation Information

Cited By

  • Preparation method for in-situ polymerization of sodium polyacrylate hydrogel containing covalent organic framework material

    CN119978434A