Sodium ion battery with high initial coulombic efficiency

By using carbon negative electrode material with oxygen-containing functional groups implanted on the surface in sodium ion batteries to form a solid electrolyte interface film with composite electrolyte solution, the problem of low efficiency of sodium ion batteries for the first time was solved, and high-efficiency sodium ion storage and solvent screening were achieved. Significantly improves the first-time Coulomb efficiency and cycle stability of the battery.

CN119069844AInactive Publication Date: 2024-12-03NAKUN CARBON SOURCE (TIANJIN) TECHNOLOGY CO LTD +1

Patent Information

Application Number
CN202411548204.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-11-01
Publication Date
2024-12-03
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The first-time Coulomb efficiency of existing sodium ion batteries is low, mainly due to the structural defects and functional groups of carbon anode materials, poor reversibility of sodium ion storage, and weak solid electrolyte membrane stability and interface solvent screening ability.

Method used

The carbon negative electrode material with oxygen-containing functional groups implanted on the surface and the composite electrolyte are formed by contacting and reacting with the electrolyte solution to form a solid electrolyte interface film. The oxygen atom proportion on the surface of the carbon negative electrode material is regulated by specific oxidative gas heat treatment methods and The relative content of oxygen-containing functional groups forms an efficient solid electrolyte interface film to improve the ability of sodium ion-through membrane storage and solvent screening.

Benefits of technology

The first Coulomb efficiency of sodium ion batteries was significantly improved to 98.6%, and the cycle stability was improved, irreversible side reactions were avoided, and the overall performance of the battery was enhanced.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119069844A_ABST
    Figure CN119069844A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of sodium ion batteries, in particular to a sodium ion battery with high initial coulombic efficiency, which comprises a carbon negative electrode material with an oxygen-containing functional group implanted on the surface, a composite electrolyte containing sodium salt and an organic solvent, and a solid electrolyte interface film between the carbon negative electrode material and the composite electrolyte, the oxygen atom ratio of the oxygen-containing functional group on the surface in the carbon negative electrode material is 2.8%-35.7%; the oxygen-containing functional group is implanted into the surface of the negative electrode, so that the construction of the solid electrolyte interface film is accelerated, the obtained solid electrolyte interface film has efficient screening capability, sodium ion transmembrane storage can be realized, solvent molecules are blocked and shielded, and irreversible side reaction caused by decomposition is avoided; the technical problem that a solid electrolyte interface film in an existing sodium-ion battery is difficult to realize transmembrane storage of sodium ions and screening of a solvent at the same time is solved, and the first coulombic efficiency and the cycling stability of the sodium-ion battery are remarkably improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of sodium ion batteries, and in particular to a sodium ion battery with high first coulombic efficiency. Background Art

[0002] With the transformation of the global energy structure and the growing demand for new energy technologies, sodium-ion batteries have shown broad application prospects due to their abundant resources, low cost, and superior low-temperature and fast-charging characteristics, and are considered a potential substitute for lithium-ion batteries. Carbon-based materials have become a popular choice for battery negative electrode materials due to their good conductivity, thermal stability and relatively low cost.

[0003] At present, there are many different types of carbon-based negative electrode materials used in sodium-ion batteries on the market, including but not limited to hard carbon, soft carbon and graphene materials. Although these traditional carbon materials have shown a certain degree of feasibility, they still have problems such as poor first coulombic efficiency, low specific capacity and poor rate performance.

[0004] The poor first coulombic efficiency of existing sodium-ion batteries is due to the fact that the reversibility of the electrochemical storage of sodium ions on the carbon negative electrode is often troubled by carbon structural defects. Although the structural defects and functional groups of the carbon negative electrode increase the adsorption energy of sodium ions, the high adsorption energy can easily produce a "trap effect", making it more difficult for sodium ions to escape from the defects and functional groups. They will undergo irreversible parasitic interfacial reactions with the solvent in the electrolyte. The resulting solid electrolyte membrane (SEI) has poor stability and weak interfacial solvent and sodium ion screening capabilities, resulting in a decrease in the first coulombic efficiency, thereby restricting the application of carbon material negative electrodes.

[0005] In recent years, researchers have tried to modify carbon materials by various means. The existing technologies are to introduce more functional sites that are conducive to sodium storage by regulating the structure of the electrolyte or carbon negative electrode materials through physical activation, chemical oxidation or doping with other elements. For example, Yu's team synthesized porous carbon with controllable porous structure and structure-free porous carbon at 9.6 A g −1 At a current density of 66 mAh g −1 The battery has excellent rate performance, but the first coulombic efficiency is less than 60%. Although the existing technology changes the chemical state of the material surface and increases the sodium storage capacity, the SEI membrane formed thereby is difficult to simultaneously achieve transmembrane storage of sodium ions and screening of solvents, and does not have the ability of efficient screening. The first coulombic efficiency and cycle stability of the obtained sodium-ion battery are poor. Summary of the invention

[0006] In order to solve the problem of low first coulombic efficiency of the above-mentioned carbon negative electrode material, the present invention provides a sodium ion battery with high first coulombic efficiency, which significantly improves the first coulombic efficiency.

[0007] The present invention provides a sodium ion battery with high first coulombic efficiency, comprising a carbon negative electrode material with oxygen-containing functional groups implanted on the surface and a composite electrolyte, wherein a solid electrolyte interface film exists between the carbon negative electrode material with oxygen-containing functional groups implanted on the surface and the composite electrolyte; the oxygen-containing functional groups on the surface of the carbon negative electrode material account for 2.8% to 35.7% of oxygen atoms in the carbon negative electrode material; the solid electrolyte interface film is formed by the contact reaction between the carbon negative electrode material and the composite electrolyte at the negative electrode interface, and comprises an organic component and an inorganic component.

[0008] Preferably, the first coulombic efficiency of the sodium ion battery with high first coulombic efficiency is as high as 98.6%.

[0009] Furthermore, the oxygen-containing functional groups implanted on the surface of the carbon negative electrode material include at least one of hydroxyl, carboxyl, carbonyl, lactone, carboxylic anhydride, quinone, ester and ether groups; and the relative content of the oxygen-containing functional groups is 79% to 95%.

[0010] Furthermore, the carbon negative electrode material includes at least one of graphene, carbon nanotubes, porous carbon, microporous carbon, mesoporous carbon and amorphous carbon.

[0011] Furthermore, the composite electrolyte includes an organic solvent and a sodium salt.

[0012] Preferably, the organic solvent includes at least one of methyl carbonate, ethylene carbonate, propylene carbonate, diethyl carbonate, dimethyl ether, diethylene glycol dimethyl ether and tetraethylene glycol dimethyl ether.

[0013] Preferably, the sodium salt includes at least one of sodium trifluoromethanesulfonate, sodium perchlorate and sodium hexafluorophosphate.

[0014] Furthermore, the organic component in the solid electrolyte interface film includes at least one of sodium alcoholate, alkyl carbonate, ester polymer and ether polymer.

[0015] Preferably, the inorganic component in the solid electrolyte interface film includes at least one of sodium oxide, sodium carbonate, sodium fluoride and sodium sulfonate.

[0016] The proportion of oxygen atoms in the carbon negative electrode material to the oxygen-containing functional groups on the surface of the carbon negative electrode material can be regulated by changing the type and relative content of the oxygen-containing functional groups through the preparation method.

[0017] Furthermore, the preparation process of the carbon negative electrode material includes the preparation of a carbon negative electrode precursor and the preparation of implanting oxygen-containing functional groups on the surface of the carbon negative electrode material; Furthermore, the preparation process of the carbon negative electrode material comprises the following steps: Step 1, preparation of a carbon negative electrode precursor: reducing the surface of the carbon negative electrode material under an inert gas atmosphere to obtain a carbon negative electrode precursor; Step 2, preparation of carbon negative electrode material: grafting the carbon negative electrode precursor under a mixed atmosphere to implant oxygen-containing functional groups on the surface of the carbon negative electrode precursor to obtain a carbon negative electrode material with a certain oxygen atom ratio.

[0018] Furthermore, the mixed atmosphere includes an oxidizing gas and a non-oxidizing gas, and the volume of the oxidizing gas accounts for 10-30% of the total volume of the mixed atmosphere.

[0019] Preferably, the oxidizing atmosphere comprises at least one of oxygen, carbon dioxide, carbon monoxide, water vapor and ozone.

[0020] Preferably, the non-oxidizing gas includes at least one of nitrogen, argon and hydrogen.

[0021] Preferably, the temperature of the reduction treatment in step 1 is 500° C.-1600° C., and the treatment time is 2-4 hours.

[0022] Preferably, the temperature of the grafting treatment in step 2 is 200-550° C., and the treatment time is 0.5-2 h.

[0023] The advantages of the present invention are: The present invention utilizes heat treatment of the carbon negative electrode surface with an oxidizing gas to achieve a selective oxidation method, implants specific oxygen-containing functional groups on the negative electrode surface, selectively controls the treatment temperature, the type of mixed atmosphere and the volume ratio of the oxidizing gas, selectively changes the oxygen atom ratio of the surface oxygen-containing functional groups in the carbon negative electrode material and the relative content of the oxygen-containing functional groups, and achieves adjustable oxygen-containing functional groups on the surface of the carbon negative electrode material. In a sodium ion battery, the carbon negative electrode material with adjustable oxygen-containing functional groups implanted on the surface can further enhance the adsorption of intermediates and accelerate the construction of a solid electrolyte interface membrane by contacting with a composite electrolyte. The solid electrolyte interface membrane thus formed has the ability of efficient screening, can achieve the storage of sodium ions through the membrane while blocking and shielding solvent molecules, avoids decomposition to produce irreversible side reactions, and greatly improves the first coulomb efficiency and cycle stability of sodium ions. Compared with the prior art, the first coulomb efficiency of the sodium ion battery provided by the present invention is as high as 98.6%. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 is the first charge and discharge curve diagram of Example 1 of the present invention; Figure 2 This is a graph showing the test results of the oxygen atom ratio in Example 1 of the present invention; Figure 3 is a graph showing the relative content of oxygen-containing functional groups in Example 1 of the present invention; Figure 4 is the thermogravimetric loss curve of Example 1 of the present invention; Figure 5 This is the first charge and discharge curve of Comparative Example 1; Figure 6 This is the first charge and discharge curve of Comparative Example 2. DETAILED DESCRIPTION

[0025] The following will be combined with the drawings in the embodiments of the invention to clearly and completely describe the technical solutions in the embodiments of the invention. Obviously, the described embodiments are only part of the embodiments of the invention, not all of them. Based on the embodiments in the invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the invention.

[0026] It should be noted that the various installation methods and technical terms mentioned in the invention are technical terms that have long been clearly known in the relevant technical field, so no further explanation is given. In addition, the same reference numerals are used for the same components, but this does not affect and should not constitute an accurate understanding of the technical solution by those skilled in the art.

[0027] Example 1 The carbon negative electrode material for sodium ion batteries with high initial coulombic efficiency provided in this example is prepared by the following preparation process: Step 1: subjecting the carbon negative electrode material (the carbon negative electrode material in this embodiment is graphene) to a high temperature heat treatment under a nitrogen atmosphere, wherein the heat treatment temperature is 900° C. and the heat treatment time is 2 h to obtain a carbon negative electrode precursor; Step 2: heat-treat the carbon negative electrode precursor obtained in step 1 under an oxidizing atmosphere (the oxidizing atmosphere in this embodiment is composed of 78% N2 and 22% O2) at a heat treatment temperature of 500°C and a heat treatment time of 1 hour, so that the surface of the carbon negative electrode precursor is connected with specific oxygen-containing functional groups.

[0028] XPS analysis of the carbon negative electrode material obtained in Example 1 was performed using a PHI 5000 Versa Probe II spectrometer (Al Kα). The results are as follows: Figure 2 As shown, the oxygen atom ratio of the obtained carbon negative electrode material is 10.6%, and the O1s spectrum analysis is performed, and the results are as follows Figure 3 As shown, the oxygen-containing functional groups on the surface of the carbon negative electrode material are lactone group, carboxylic anhydride group, and carboxyl group, with a relative content of 86.6%.

[0029] The sodium ion battery carbon negative electrode material with high initial coulombic efficiency of this embodiment is assembled into a sodium ion half-cell, and the specific process is as follows: Step 3, the carbon negative electrode material obtained in step 2, conductive carbon black (Super-P) with conductive function, polyvinylidene fluoride (PVDF) with bonding function and N-methylpyrrolidone (NMP) are mixed in a mass ratio of 8:1:1:100, the mixed material is coated on the surface of copper foil, and then placed in an oven and vacuum dried at 110° C. for 12 hours to obtain an electrode sheet, and the obtained electrode sheet is made into a circular electrode sheet with a diameter of 12 mm; Step 4: Assemble the circular electrode sheet with sodium metal, 100uL of composite electrolyte (the electrolyte composition of this embodiment is diethylene glycol dimethyl ether and sodium trifluoromethanesulfonate, and the concentration of sodium trifluoromethanesulfonate is 1 mol / L), and a diaphragm to obtain a sodium ion half-cell.

[0030] Example 2 The preparation method of the carbon negative electrode material for sodium ion batteries with high initial coulombic efficiency in this example is the same as that in Example 1, except that the carbon negative electrode material and the parameter conditions of the preparation process are different (as shown in Table 1): The carbon negative electrode material of this embodiment is microporous carbon; In step 1, the heat treatment temperature of this embodiment is 1000° C. and the heat treatment time is 4 hours; In step 2, the oxidizing atmosphere of this embodiment is composed of 80% N2 and 20% O2; the heat treatment temperature is 400°C, and the heat treatment time is 1 hour.

[0031] XPS detection was performed using the method in Example 1, and the oxygen-containing functional groups on the surface obtained accounted for 6.3% of oxygen atoms in the carbon material. The oxygen-containing functional groups on the surface of the carbon negative electrode material were lactone groups, ester groups, carboxylic anhydride groups, and carboxyl groups, with a relative content of 83.6%.

[0032] The preparation process of assembling the high first coulomb efficiency sodium ion battery carbon negative electrode material into a sodium ion half-cell in this embodiment is the same as that in Example 1, except that the electrolyte in this embodiment is dimethyl ether, diethylene glycol dimethyl ether and sodium trifluoromethanesulfonate, the concentration of sodium trifluoromethanesulfonate is 1 mol / L, dimethyl ether and diethylene glycol dimethyl ether (50%:50%).

[0033] Example 3 The preparation method of the carbon negative electrode material for sodium ion batteries with high initial coulombic efficiency in this example is the same as that in Example 1, except that the carbon negative electrode material and the parameter conditions of the preparation process are different (as shown in Table 1): The carbon negative electrode material of this embodiment is graphene; In step 2, the heat treatment temperature of this embodiment is 300° C. and the heat treatment time is 2 hours.

[0034] XPS detection was performed using the method in Example 1, and the oxygen-containing functional groups on the surface obtained accounted for 3.8% of oxygen atoms in the carbon material. The oxygen-containing functional groups on the surface of the carbon negative electrode material were lactone groups, ester groups, carboxylic anhydride groups, and carboxyl groups, with a relative content of 80.1%.

[0035] The preparation process of assembling the high first coulomb efficiency sodium ion battery carbon negative electrode material into a sodium ion half-cell in this embodiment is the same as that in Example 1, except that the electrolyte in this embodiment is tetraethylene glycol dimethyl ether, diethylene glycol dimethyl ether and sodium hexafluorophosphate, the concentration of sodium hexafluorophosphate is 1 mol / L, tetraethylene glycol dimethyl ether and diethylene glycol dimethyl ether (50%:50%).

[0036] Example 4 The preparation method of the carbon negative electrode material for sodium ion batteries with high initial coulombic efficiency in this example is the same as that in Example 1, except that the carbon negative electrode material and the parameter conditions of the preparation process are different (as shown in Table 1): The carbon negative electrode material of this embodiment is mesoporous carbon; In step 1, the heat treatment time in this embodiment is 4 hours; In step 2, the heat treatment temperature of this embodiment is 500° C., and the heat treatment time is 0.5 h.

[0037] XPS detection was performed using the method in Example 1, and the oxygen-containing functional groups on the surface of the obtained carbon negative electrode material accounted for 7.6% of the oxygen atoms in the carbon material. The oxygen-containing functional groups on the surface of the obtained carbon negative electrode material were lactone groups, ester groups, and carboxylic anhydride groups, with a relative content of 81.3%.

[0038] The preparation process of assembling the high first coulombic efficiency sodium ion battery carbon negative electrode material into a sodium ion half-cell in this embodiment is the same as that in Example 1, except that the electrolyte in this embodiment is diethylene glycol dimethyl ether and sodium hexafluorophosphate, and the concentration of sodium hexafluorophosphate is 1 mol / L.

[0039] Example 5 The preparation method of the carbon negative electrode material for sodium ion batteries with high initial coulombic efficiency in this example is the same as that in Example 1, except that the carbon negative electrode material and the parameter conditions of the preparation process are different (as shown in Table 1): The carbon negative electrode material of this embodiment is graphene; In step 1, the heat treatment temperature of this embodiment is 800° C. and the heat treatment time is 4 hours; In step 2, the oxidizing atmosphere of this embodiment is composed of 70% N2 and 30% O2; the heat treatment temperature is 500°C, and the heat treatment time is 2h.

[0040] XPS detection was performed using the method in Example 1, and the oxygen-containing functional groups on the surface of the obtained carbon negative electrode material accounted for 23.1% of the oxygen atoms in the carbon material. The oxygen-containing functional groups on the surface of the obtained carbon negative electrode material were lactone groups, ester groups, carboxylic anhydride groups, and carboxyl groups, with a relative content of 66.7%.

[0041] The preparation process of assembling the high first coulomb efficiency sodium ion battery carbon negative electrode material into a sodium ion half-cell in this embodiment is the same as that in Example 1, except that the electrolyte in this embodiment is ethylene carbonate, diethyl carbonate, and sodium perchlorate, the concentration of sodium perchlorate is 1 mol / L, and the concentration of ethylene carbonate and diethyl carbonate is (50%:50%).

[0042] Example 6 The preparation method of the carbon negative electrode material for sodium ion batteries with high initial coulombic efficiency in this example is the same as that in Example 1, except that the carbon negative electrode material and the parameter conditions of the preparation process are different (as shown in Table 1): The carbon negative electrode material of this embodiment is graphene; In step 1, the heat treatment temperature of this embodiment is 800° C. and the heat treatment time is 4 hours; In step 2, the oxidizing atmosphere of this embodiment is composed of 90% Ar2 and 10% O2; the heat treatment temperature is 500°C, and the heat treatment time is 2h.

[0043] XPS detection was performed using the method in Example 1, and the surface oxygen-containing functional groups obtained accounted for 5.9% of the oxygen atoms in the carbon material. The oxygen-containing functional groups on the surface of the carbon negative electrode material were lactone groups, ester groups, carboxylic anhydride groups, and carboxyl groups, with a relative content of 87.3%.

[0044] The preparation process and electrolyte of the high first coulombic efficiency sodium ion battery carbon negative electrode material assembled into a sodium ion half-cell in this embodiment are the same as those in Example 1.

[0045] Example 7 The preparation method and carbon negative electrode material of the sodium ion battery with high initial coulombic efficiency of this example are the same as those of Example 1, except that the parameter conditions of the preparation process are different (as shown in Table 1): In step 1, the heat treatment time in this embodiment is 4 hours; In step 2, the oxidizing atmosphere of this embodiment is composed of 90% Ar2 and 10% H2O; the heat treatment temperature is 500°C, and the heat treatment time is 0.5h.

[0046] XPS detection was performed using the method in Example 1, and the surface oxygen-containing functional groups obtained accounted for 5.5% of the oxygen atoms in the carbon material. The oxygen-containing functional groups on the surface of the carbon negative electrode material were lactone groups, ester groups, carboxylic anhydride groups, and hydroxyl groups, with a relative content of 79.3%.

[0047] Example 8 The preparation method and carbon negative electrode material of the sodium ion battery with high initial coulombic efficiency of this example are the same as those of Example 1, except that the parameter conditions of the preparation process are different (as shown in Table 1): In step 1, the heat treatment temperature of this embodiment is 1600° C. and the heat treatment time is 4 hours; In step 2, the oxidizing atmosphere of this embodiment is composed of 80% Ar2 and 20% CO; the heat treatment temperature is 500°C, and the heat treatment time is 1 hour.

[0048] XPS detection was performed using the method in Example 1, and the oxygen-containing functional groups on the surface of the obtained carbon negative electrode material accounted for 8.3% of the oxygen atoms in the carbon material. The oxygen-containing functional groups on the surface of the obtained carbon negative electrode material were lactone groups, ester groups, and carboxylic anhydride groups, with a relative content of 86.2%.

[0049] The preparation process and electrolyte of the high first coulombic efficiency sodium ion battery carbon negative electrode material assembled into a sodium ion half-cell in this embodiment are the same as those in Example 1.

[0050] Example 9 The preparation method and carbon negative electrode material of the sodium ion battery with high initial coulombic efficiency of this example are the same as those of Example 1, except that the parameter conditions of the preparation process are different (as shown in Table 1): In step 1, the heat treatment time in this embodiment is 4 hours; In step 2, the oxidizing atmosphere of this embodiment is composed of 80% Ar2 and 20% CO2; the heat treatment temperature is 500°C, and the heat treatment time is 1 hour.

[0051] XPS detection was performed using the method in Example 1, and the oxygen-containing functional groups on the surface of the obtained carbon negative electrode material accounted for 7.3% of the oxygen atoms in the carbon material. The oxygen-containing functional groups on the surface of the obtained carbon negative electrode material were carboxyl and carboxylic anhydride, with a relative content of 88.3%.

[0052] The preparation process and electrolyte of the high first coulombic efficiency sodium ion battery carbon negative electrode material assembled into a sodium ion half-cell in this embodiment are the same as those in Example 1.

[0053] Example 10 The preparation method and carbon negative electrode material of the sodium ion battery with high initial coulombic efficiency of this example are the same as those of Example 1, except that the parameter conditions of the preparation process are different (as shown in Table 1): In step 1, the heat treatment temperature of this embodiment is 500° C. and the heat treatment time is 2 h; In step 2, the oxidizing atmosphere of this embodiment is composed of 78% N2 and 22% O2; the heat treatment temperature is 500°C, and the heat treatment time is 1 hour.

[0054] XPS detection was performed using the method in Example 1, and the oxygen-containing functional groups on the surface of the obtained carbon negative electrode material accounted for 8.2% of the oxygen atoms in the carbon material. XPS detection was performed using the method in Example 1, and the oxygen-containing functional groups on the surface of the carbon negative electrode material were carboxyl, carboxylic anhydride, hydroxyl, and carbonyl, with a relative content of 79.1%.

[0055] The preparation process and electrolyte of the high first coulombic efficiency sodium ion battery carbon negative electrode material assembled into a sodium ion half-cell in this embodiment are the same as those in Example 1.

[0056] Example 11 The preparation method and carbon negative electrode material of the high first coulombic efficiency sodium ion battery in this example are the same as those in Example 1, except that the parameter conditions of the preparation process are different (as shown in Table 1): In step 1, the heat treatment time in this embodiment is 4 hours; In step 2, the oxidizing atmosphere of this embodiment is composed of 78% N2 and 22% O2; the heat treatment temperature is 200°C, and the heat treatment time is 1 hour.

[0057] XPS detection was performed using the method in Example 1, and the surface oxygen-containing functional groups obtained accounted for 3.3% of the oxygen atoms in the carbon material. The oxygen-containing functional groups on the surface of the carbon negative electrode material were lactone groups, ester groups, carboxylic anhydride groups, and carboxyl groups, with a relative content of 80.2%.

[0058] The preparation process and electrolyte of the high first coulombic efficiency sodium ion battery carbon negative electrode material assembled into a sodium ion half-cell in this embodiment are the same as those in Example 1.

[0059] Example 12 The preparation method and carbon negative electrode material of the sodium ion battery with high initial coulombic efficiency of this example are the same as those of Example 1, except that the parameter conditions of the preparation process are different (as shown in Table 1): In step 1, the heat treatment time in this embodiment is 4 hours; In step 2, the oxidizing atmosphere of this embodiment is composed of 78% N2 and 22% O2; the heat treatment temperature is 550°C, and the heat treatment time is 0.5h.

[0060] XPS detection was performed using the method in Example 1, and the surface oxygen-containing functional groups obtained accounted for 16.3% of the oxygen atoms in the carbon material. The oxygen-containing functional groups on the surface of the carbon negative electrode material were lactone groups, ester groups, carboxylic anhydride groups, and carboxyl groups, with a relative content of 81.2%.

[0061] The preparation process and electrolyte of the high first coulombic efficiency sodium ion battery carbon negative electrode material assembled into a sodium ion half-cell in this embodiment are the same as those in Example 1.

[0062] Comparative Example 1 The difference between this comparative example and Example 1 is that the carbon negative electrode material of this comparative example is not subjected to oxidation treatment and the sodium ion half-cell is directly assembled.

[0063] Comparative Example 2 The difference between this comparative example and Example 1 is that the electrolyte composition of this comparative example is ethylene carbonate, ethyl methyl carbonate, and sodium perchlorate, the concentration of sodium perchlorate is 1 mol / L, and the ratio of ethylene carbonate to ethyl methyl carbonate is 50%:50%.

[0064] Comparative Example 3 The difference between this comparative example and Example 1 is that the preparation conditions of the carbon negative electrode material are different (as shown in Table 1): In step 1, the heat treatment temperature of this comparative example is 1700°C and the time is 2h; In step 2, the oxidizing atmosphere composition of this comparative example is 78% of N2 and 22% of O2; the heat treatment temperature is 500°C, the heat treatment time is 0.5h, and XPS detection shows that the surface oxygen-containing functional groups account for 1.3% of the oxygen atoms in the carbon material, and the oxygen-containing functional groups on the surface of the carbon negative electrode material are hydroxyl and carbonyl, with a relative content of 85.1%.

[0065] Comparative Example 4 The difference between this comparative example and Example 1 is that the preparation conditions of the carbon negative electrode material are different (as shown in Table 1): In step 1, the heat treatment temperature of this comparative example is 800°C and the time is 4h; In step 2, the oxidizing atmosphere of this comparative example consists of 78% N2 and 22% O2; the heat treatment temperature is 50°C, and the heat treatment time is 1 hour.

[0066] Comparative Example 5 The difference between this comparative example and Example 1 is that the preparation conditions of the carbon negative electrode material are different (as shown in Table 1): In step 2, the oxidizing atmosphere composition of this comparative example is 95% N2 and 5% O2; the heat treatment temperature is 400°C, the heat treatment time is 0.5h, and the surface oxygen-containing functional groups obtained by XPS detection account for 2.6% of the oxygen atoms in the carbon material. The oxygen-containing functional groups on the surface of the carbon negative electrode material are hydroxyl and carbonyl, and the relative content is 86.7%.

[0067] Comparative Example 6 The difference between this comparative example and Example 1 is that the preparation conditions of the carbon negative electrode material are different (as shown in Table 1): In step 2, the oxidizing atmosphere composition of this comparative example is 60% N2 and 40% O2; the heat treatment temperature is 400°C, the heat treatment time is 0.5h, and the surface oxygen-containing functional groups obtained by XPS detection account for 36.0% of the oxygen atoms in the carbon material. The oxygen-containing functional groups on the surface of the carbon negative electrode material are carbonyl and carboxylic acid groups, with a relative content of 90.7%.

[0068] Comparative Example 7 The difference between this comparative example and Example 1 is that the preparation conditions of the carbon negative electrode material are different (as shown in Table 1): In step 2, the oxidizing atmosphere of this comparative example consists of 30% O2, 20% CO and 50% O2; the heat treatment temperature is 400°C, the heat treatment time is 0.5h, and the surface oxygen-containing functional groups obtained by XPS detection account for 38.7% of the oxygen atoms in the carbon material. The oxygen-containing functional groups on the surface of the obtained carbon negative electrode material are carbonyl and carboxylic acid groups, with a relative content of 89.2%.

[0069] Table 1 Different parameter conditions of examples and comparative examples

[0070] Test Case The sodium ion half-cells of Examples 1-13 and Comparative Examples 1-8 were subjected to electrochemical performance tests, and the first coulombic efficiency results obtained are shown in Table 2: Table 2 Content and performance effect table of embodiments and comparative examples

[0071] Result analysis: From the data in Table 2, it can be seen that the oxygen atoms in the oxygen-containing functional groups on the surface of the carbon negative electrode material obtained after the two-step heat treatment should account for 2.8% to 35.7% of the total mass. The first coulombic efficiency within this range is excellent, but the first coulombic efficiency corresponding to the minimum and maximum values ​​will decrease slightly. A certain value within this range has the optimal value of the first coulombic efficiency. Among them, the oxygen atoms in the oxygen-containing functional groups on the surface of the carbon negative electrode material of Example 1 account for 10.6%, and the relative content of its specific oxygen-containing functional groups is 86.6%. The performance of the prepared sodium ion half-battery is the best, and the first coulombic efficiency is as high as 98.6% (such as Figure 1 As shown), it is the best embodiment of the present invention. The thermogravimetric loss curve of Example 1 is as shown Figure 4 As shown, it can be seen that when the heat treatment temperature is too high, it will cause material burning.

[0072] By comparing the results of Examples 2-12 with those of Example 1, it can be seen that in the preparation process of the carbon negative electrode material, although the relative mass of the oxygen-containing functional groups and the proportion of oxygen atoms in the carbon negative electrode material will be changed by changing the processing temperature, the type of mixed atmosphere and the volume ratio of the oxidizing gas, it does not exceed a specific range. When the obtained carbon negative electrode material comes into contact with the composite electrolyte, the solid electrolyte interface membrane formed thereby still has the efficient screening ability to simultaneously screen sodium ions and solvent molecules, and still exhibits excellent first coulombic efficiency.

[0073] However, by comparing the results of Comparative Examples 3-7 with those of Example 1, it can be seen that when the preparation condition parameters are adjusted out of the range, the relative mass of the oxygen-containing functional groups and the proportion of oxygen atoms in the carbon negative electrode material are exceeded, and the solid electrolyte interface film formed by the obtained carbon negative electrode material and the composite electrolyte has a weak screening ability for sodium ions and solvent molecules, resulting in a significant decrease in the first coulombic efficiency.

[0074] like Figure 5 and Figure 6 As shown, compared with the results of the embodiment, examples 1 and 2 show that without using the carbon negative electrode material with oxygen-containing functional groups implanted on the surface and the composite electrolyte of the present application, the formed solid electrolyte membrane does not have the ability of efficient screening, and its first coulombic efficiency is significantly reduced.

[0075] It can be seen that according to the composition of the composite electrolyte, by selectively controlling the treatment temperature, the type of mixed atmosphere and the volume ratio of the oxidizing gas within a certain range, the proportion of oxygen atoms in the surface oxygen-containing functional groups in the carbon negative electrode material and the relative content of the oxygen-containing functional groups can be changed, so that the range of the oxygen-containing functional groups on the surface of the carbon negative electrode material can be adjusted. The obtained carbon negative electrode material with adjustable surface oxygen-containing functional groups can accelerate the construction of the solid electrolyte interface membrane by strengthening the adsorption of intermediates. The solid electrolyte interface membrane thus formed has the ability of efficient screening, and can achieve simultaneous screening of sodium ions and solvent molecules, greatly improving the first coulomb efficiency and cycle stability.

[0076] For those skilled in the art, the invention is not limited to the details of the above exemplary embodiments, and can be implemented in other specific forms without departing from the spirit or basic characteristics of the invention; therefore, no matter from which point of view, the embodiments should be regarded as exemplary and non-restrictive, and the scope of the invention is defined by the appended claims rather than the above description, so it is intended to include all changes within the meaning and scope of the equivalent elements of the claims. Any reference numerals in the claims should not be regarded as limiting the claims involved.

[0077] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any minor modifications, equivalent substitutions and improvements made to the above embodiments based on the technical essence of the present invention should be included in the protection scope of the technical solution of the present invention.

Claims

1. A sodium ion battery with high initial coulombic efficiency, comprising a carbon negative electrode material and an electrolyte, characterized in that: The carbon negative electrode material is a carbon negative electrode material with oxygen-containing functional groups implanted on the surface, the electrolyte is a composite electrolyte containing sodium salt and an organic solvent, and a solid electrolyte interface film exists between the carbon negative electrode material and the composite electrolyte; Among them, the oxygen-containing functional groups on the surface of the carbon negative electrode material account for 2.8% to 35.7% of the oxygen atoms in the carbon negative electrode material; the solid electrolyte interface film is formed by the contact reaction between the carbon negative electrode material and the composite electrolyte at the negative electrode interface, including organic components and inorganic components.

2. The sodium ion battery with high initial coulombic efficiency according to claim 1, characterized in that: The oxygen-containing functional groups implanted on the surface of the carbon negative electrode material include at least one of hydroxyl, carboxyl, carbonyl, lactone, carboxylic anhydride, quinone, ester and ether groups; the relative content of the oxygen-containing functional groups is 79% to 95%.

3. The sodium ion battery with high initial coulombic efficiency according to claim 1, characterized in that: The carbon negative electrode material includes at least one of graphene, carbon nanotubes, porous carbon, microporous carbon, mesoporous carbon and amorphous carbon.

4. The sodium ion battery with high initial coulombic efficiency according to claim 2, characterized in that: The organic solvent includes at least one of methyl carbonate, ethylene carbonate, propylene carbonate, diethyl carbonate, dimethyl ether, diethylene glycol dimethyl ether and tetraethylene glycol dimethyl ether; the sodium salt includes at least one of sodium trifluoromethanesulfonate, sodium perchlorate and sodium hexafluorophosphate.

5. The sodium ion battery with high initial coulombic efficiency according to claim 4, characterized in that: The organic component in the solid electrolyte interface film includes at least one of sodium alcoholate, alkyl carbonate, ester polymer and ether polymer; the inorganic component in the solid electrolyte interface film includes at least one of sodium oxide, sodium carbonate, sodium fluoride and sodium sulfonate.

6. The sodium ion battery with high initial coulombic efficiency according to any one of claims 1 to 5, characterized in that: The proportion of oxygen atoms in the carbon negative electrode material to the oxygen-containing functional groups on the surface of the carbon negative electrode material can be regulated by changing the type and relative content of the oxygen-containing functional groups through the preparation method.

7. The sodium ion battery with high initial coulombic efficiency according to claim 6, characterized in that: The preparation process of the carbon negative electrode material comprises the following steps: Step 1, preparation of a carbon negative electrode precursor: reducing the surface of the carbon negative electrode material under an inert gas atmosphere to obtain a carbon negative electrode precursor; Step 2, preparation of carbon negative electrode material: grafting the carbon negative electrode precursor under a mixed atmosphere to implant oxygen-containing functional groups on the surface of the carbon negative electrode precursor to obtain a carbon negative electrode material with a certain oxygen atom ratio; Wherein, the mixed atmosphere includes oxidizing gas and non-oxidizing gas, and the volume of the oxidizing gas accounts for 10-30% of the total volume of the mixed atmosphere.

8. The sodium ion battery with high initial coulombic efficiency according to claim 7, characterized in that: The temperature of the reduction treatment in step 1 is 500° C.-1600° C., and the treatment time is 2-4 hours.

9. The sodium ion battery with high initial coulombic efficiency according to claim 7, characterized in that: The temperature of the grafting treatment in step 2 is 200-550° C., and the treatment time is 0.5-2 h.

10. The sodium ion battery with high initial coulombic efficiency according to claim 8, characterized in that: The oxidizing gas includes at least one of oxygen, carbon dioxide, carbon monoxide, water vapor and ozone; the non-oxidizing gas includes at least one of nitrogen, argon and hydrogen.

Citation Information

Patent Citations

  • Carbon material applied to negative electrode of lithium ion power battery and preparation method of carbon material

    CN103325997A

  • Direction control method of surface oxygen functional groups on coal-based hard carbon for sodium-storing cathodes

    CN109796003A

  • Biomass-based sodium ion battery negative electrode material as well as preparation method and application thereof

    CN117963880A

  • Reaction inducer composition and Latex modified concrete composition

    KR102087251B1

  • Negative electrode active material, secondary battery, and electronic apparatus

    WO2024178610A1

Cited By

  • Detection method and device for testing crosstalk characteristic of lithium battery

    CN119758110A