Method for manufacturing laminated iron core

By temporarily joining and formally bonding electromagnetic steel strips with controlled temperature and pressure, the method addresses the inefficiencies of thinned steel sheets, improving productivity and die longevity in laminated core manufacturing.

CN119070571APending Publication Date: 2024-12-03NIPPON STEEL CORPORATION
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202411474771.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2020-06-17
Filing Date
2021-06-17
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

The use of thinned electromagnetic steel sheets in laminated core manufacturing increases the number of punching times, necessitating higher speeds that compromise the life of the punching die, and existing methods fail to adequately improve productivity.

Method used

A method involving temporary joining of electromagnetic steel strips using a guide roller before punching, followed by formal bonding after heating, with a surface temperature of 15 to 50°C and a pressing force of 2.0 to 10.0 MPa, and subsequent heating to 180 to 250°C for complete bonding.

Benefits of technology

This approach enhances productivity by reducing the number of punching operations and extending die life, resulting in a more efficient manufacturing process.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119070571A_ABST
    Figure CN119070571A_ABST
Patent Text Reader

Abstract

Provided is a method for manufacturing a laminated iron core, in which core single plates are obtained by punching an electromagnetic steel strip provided with an insulating coating, and the core single plates are laminated, said method being characterized in that: before the punching, two or more electromagnetic steel strips are temporarily bonded by being pressed by a guide roller; and after the more than two electromagnetic steel strips which are temporarily jointed are inserted into a blanking die, the iron core single plates are obtained through blanking processing.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] This application is a divisional application of an invention patent application with an application date of June 17, 2021, application number 2021800216019, and invention name “Method for manufacturing a laminated iron core”. Technical Field

[0002] The present invention relates to a method for manufacturing a laminated core.

[0003] This application claims priority based on Japanese Patent Application No. 2020-104252 filed in Japan on June 17, 2020, the contents of which are incorporated herein by reference. Background Art

[0004] The laminated core used by the motor (rotating motor) is manufactured by punching the electromagnetic steel sheet into a predetermined shape through a punching process and then stacking it in a mold. In recent years, in order to reduce the iron loss of motor products, thinned electromagnetic steel sheets have been used in these products. However, there are problems in the thinned electromagnetic steel sheets that do not occur in the existing laminated core manufacturing method. For example, the number of punching times increases. This is because when the thickness of the electromagnetic steel sheet is reduced to half of the current one, the number of punching times doubles. In order to ensure the same productivity as before, it is necessary to increase the punching speed. It is necessary to reduce the gap of the punching die due to the thinning of the electromagnetic steel sheet. In order to increase the punching speed, there is a limit to ensuring the life of the punching die.

[0005] Patent Document 1 describes a method for manufacturing a laminated iron core. Patent Document 1 describes a technique for performing a punching process after laminating two or more electromagnetic steel sheets in order to improve productivity. However, in Patent Document 1, since heating is performed to completely cure or partially cure the bonding layer formed between the electromagnetic steel sheets, productivity cannot be sufficiently improved.

[0006] Prior art literature

[0007] Patent Literature

[0008] Patent Document 1: Japanese Patent Application Publication No. 2005-191033 Summary of the invention

[0009] Technical problem to be solved by the invention

[0010] The present invention has been made based on the above-mentioned actual situation, and an object of the present invention is to provide a method for manufacturing a laminated core with excellent productivity.

[0011] Technical means for solving technical problems

[0012] The gist of the present invention is as follows.

[0013] (1) A method for manufacturing a laminated iron core according to one embodiment of the present invention comprises: a method for manufacturing a laminated iron core by laminating iron core sheets obtained by punching out an electromagnetic steel strip having an insulating coating,

[0014] Prior to the punching process, two or more electromagnetic steel strips are temporarily joined by pressing them with a guide roller.

[0015] The two or more electromagnetic steel strips that have been temporarily joined are inserted into a punching die, and then the punching process is performed to obtain the core single plate.

[0016] (2) In the method for manufacturing a laminated iron core described in (1), the surface temperature of the two or more electromagnetic steel strips during the provisional joining may be 15 to 50°C.

[0017] (3) In the method for manufacturing a laminated iron core according to (1) or (2), the pressing force applied by the guide roller during the pressing may be 2.0 to 10.0 MPa.

[0018] (4) In the method for manufacturing a laminated iron core according to any one of (1) to (3), after the punching process, the iron core single plates may be heated to 180 to 250° C. to perform formal bonding.

[0019] (5) In the method for producing a laminated iron core according to any one of (1) to (4), the insulating film may have bonding ability.

[0020] Effects of the Invention

[0021] According to the above aspect of the present invention, it is possible to provide a method for manufacturing a laminated iron core with excellent productivity. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 It is a cross-sectional view of a rotating electrical machine including a laminated iron core.

[0023] Figure 2 It is a side view of the same laminated core.

[0024] Figure 3 yes Figure 2 A-A section view.

[0025] Figure 4 It is a top view of the raw material forming the same laminated core.

[0026] Figure 5 yes Figure 4 B-B section view.

[0027] Figure 6 yes Figure 5 An enlarged view of part C.

[0028] Figure 7 This is a side view of a manufacturing device used to manufacture the same laminated iron core.

[0029] Figure 8 This is a flowchart of the method for manufacturing a laminated iron core according to the present embodiment. DETAILED DESCRIPTION

[0030] The following describes a method for manufacturing a laminated core according to an embodiment of the present invention with reference to the accompanying drawings. First, a laminated core manufactured by the method for manufacturing a laminated core according to the present embodiment, a rotating electrical machine having the laminated core, and a raw material for forming the laminated core are described. It should be noted that in the present embodiment, an example of a rotating electrical machine such as an electric motor, specifically an AC motor, more specifically a synchronous motor, and more specifically a permanent magnet excitation type motor is described. This type of electric motor is suitable for, for example, electric vehicles, etc.

[0031] (Rotating electric machine 10)

[0032] like Figure 1 As shown, the rotary electric machine 10 includes a stator 20, a rotor 30, a housing 50, and a rotating shaft 60. The stator 20 and the rotor 30 are accommodated in the housing 50. The stator 20 is fixed in the housing 50.

[0033] In the present embodiment, an inner rotor type in which the rotor 30 is located radially inside the stator 20 is adopted as the rotating electrical machine 10. However, an outer rotor type in which the rotor 30 is located outside the stator 20 may be adopted as the rotating electrical machine 10. In addition, in the present embodiment, the rotating electrical machine 10 is a three-phase AC motor with 12 poles and 18 slots. However, the number of poles, the number of slots, the number of phases, etc. may be changed as appropriate.

[0034] The rotating electrical machine 10 can rotate at a rotation speed of 1000 rpm by applying an excitation current having an effective value of 10 A and a frequency of 100 Hz to each phase, for example.

[0035] The stator 20 includes a stator bonded laminated core (hereinafter referred to as a stator core) 21 and a winding (not shown).

[0036] The stator core 21 includes an annular core back 22 and a plurality of teeth 23. Hereinafter, the direction of the central axis O of the stator core 21 (or the core back 22) is referred to as the axial direction, the radial direction (the direction orthogonal to the central axis O) of the stator core 21 (or the core back 22) is referred to as the radial direction, and the circumferential direction (the direction rotating around the central axis O) of the stator core 21 (or the core back 22) is referred to as the circumferential direction.

[0037] The core back 22 is formed in an annular shape in a plan view of the stator 20 viewed from the axial direction.

[0038] A plurality of teeth 23 protrude from the inner periphery of the core back 22 toward the radial inner side (radially toward the center axis O of the core back 22). The plurality of teeth 23 are arranged at equal angular intervals in the circumferential direction. In the present embodiment, one tooth 23 is provided at every central angle of 20 degrees centered on the center axis O, and a total of 18 teeth 23 are provided. The plurality of teeth 23 are formed in the same shape and the same size. Therefore, the plurality of teeth 23 have the same thickness dimension.

[0039] The winding is wound on the tooth portion 23. The winding may be wound in a distributed manner instead of being wound in a concentrated manner.

[0040] The rotor 30 is arranged radially inward of the stator 20 (stator core 21 ). The rotor 30 includes a rotor core 31 and a plurality of permanent magnets 32 .

[0041] The rotor core 31 is formed in an annular shape (ring shape) arranged coaxially with the stator 20. The rotating shaft 60 is arranged in the rotor core 31. The rotating shaft 60 is fixed to the rotor core 31.

[0042] A plurality of permanent magnets 32 are fixed to the rotor core 31. In the present embodiment, a set of two permanent magnets 32 forms one magnetic pole. The plurality of sets of permanent magnets 32 are arranged at equal angles in the circumferential direction. In the present embodiment, a set is provided at every central angle of 30 degrees about the central axis O, and a total of 12 sets (a total of 24) of permanent magnets 32 are provided.

[0043] In the present embodiment, an embedded magnet motor is used as a permanent magnet excitation type motor. A plurality of through holes 33 are formed on the rotor core 31, which penetrate the rotor core 31 in the axial direction. The plurality of through holes 33 are provided corresponding to the configuration of the plurality of permanent magnets 32. Each permanent magnet 32 ​​is fixed to the rotor core 31 in a state of being configured in the corresponding through hole 33. The fixing of each permanent magnet 32 ​​to the rotor core 31 can be achieved, for example, by bonding the outer surface of the permanent magnet 32 ​​and the inner surface of the through hole 33 by bonding with a bonding agent. It should be noted that, as a permanent magnet excitation type motor, a surface magnet type motor can also be used instead of the embedded magnet motor.

[0044] The stator core 21 and the rotor core 31 are both laminated cores. Figure 2 As shown, it is formed by stacking a plurality of core plates 40 in a stacking direction.

[0045] It should be noted that the stacking thickness (total length along the center axis O) of each of the stator core 21 and the rotor core 31 is, for example, 50.0 mm. The outer diameter of the stator core 21 is, for example, 250.0 mm. The inner diameter of the stator core 21 is, for example, 165.0 mm. The outer diameter of the rotor core 31 is, for example, 163.0 mm. The inner diameter of the rotor core 31 is, for example, 30.0 mm. However, these values ​​are only examples, and the stacking thickness, outer diameter or inner diameter of the stator core 21, and the stacking thickness, outer diameter or inner diameter of the rotor core 31 are not limited to these values. Here, the inner diameter of the stator core 21 is based on the front end of the tooth portion 23 of the stator core 21. That is, the inner diameter of the stator core 21 is the diameter of a virtual circle inscribed in the front end portions of all the tooth portions 23.

[0046] Each core single plate 40 forming the stator core 21 and the rotor core 31 is formed by, for example, punching Figures 4 to 6 The raw material 1 shown in the figure is formed. The raw material 1 is a steel plate (electromagnetic steel plate) which is a base material of the core single plate 40. As the raw material 1, for example, a strip-shaped steel plate or a cut plate or the like is used.

[0047] In the description of the laminated core, the raw material 1 is described below. It should be noted that in this specification, the strip-shaped steel plate of the base material of the core single plate 40 may be referred to as the raw material 1 or the electromagnetic steel strip 1. The steel plate that is punched into the shape for the laminated core by the raw material 1 or the electromagnetic steel strip 1 may be referred to as the core single plate 40.

[0048] (Raw material 1)

[0049] The raw material 1 is handled in a state of being wound into a steel coil 1A, for example. In the present embodiment, a non-oriented electromagnetic steel sheet is used as the raw material 1. As the non-oriented electromagnetic steel sheet, a non-oriented electromagnetic steel strip of JIS C 2552:2014 can be used. However, as the raw material 1, a oriented electromagnetic steel sheet can also be used instead of the non-oriented electromagnetic steel sheet. As the oriented electromagnetic steel sheet in this case, a oriented electromagnetic steel strip of JIS C 2553:2019 can be used. In addition, a non-oriented thin electromagnetic steel strip and a directional thin electromagnetic steel strip of JIS C 2558:2015 can be used.

[0050] Considering the case where the material 1 is used as the core single plate 40 , the upper and lower limits of the average plate thickness t0 of the material 1 are set as shown below, for example.

[0051] As the raw material 1 becomes thinner, the manufacturing cost of the raw material 1 increases. Therefore, in consideration of the manufacturing cost, the lower limit of the average plate thickness t0 of the raw material 1 is 0.10 mm, preferably 0.15 mm, and more preferably 0.18 mm.

[0052] On the other hand, if the raw material 1 is too thick, the manufacturing cost becomes better, but when the raw material 1 is used as the core single plate 40, the eddy current loss increases and the core iron loss deteriorates. Therefore, considering the core iron loss and the manufacturing cost, the upper limit of the average plate thickness t0 of the raw material 1 is 0.65 mm, preferably 0.35 mm, and more preferably 0.30 mm.

[0053] The material 1 that satisfies the above-mentioned range of the average plate thickness t0 of the material 1 is, for example, 0.20 mm.

[0054] It should be noted that the average plate thickness t0 of the raw material 1 is not limited to the thickness of the base steel plate 2 described later, but also includes the thickness of the insulating film 3. In addition, the method for measuring the average plate thickness t0 of the raw material 1 is, for example, the following measurement method. For example, when the raw material 1 is coiled into the shape of a steel coil 1A, at least a portion of the raw material 1 is rolled out in a flat state. In the raw material 1 rolled out in the shape of a flat plate, a predetermined position in the length direction of the raw material 1 is selected (for example, a position that is 10% of the total length of the raw material 1 from the end edge in the length direction of the raw material 1). In the selected position, the raw material 1 is divided into 5 areas along its width direction. The plate thickness of the raw material 1 is measured at 4 points on the boundaries of these 5 areas. The average value of the plate thickness at the 4 points can be used as the average plate thickness t0 of the raw material 1.

[0055] The upper and lower limits of the average thickness t0 of the raw material 1 can naturally be adopted as the upper and lower limits of the average thickness t0 of the core single plate 40. It should be noted that the method for measuring the average thickness t0 of the core single plate 40 is, for example, the following measurement method. For example, the stacking thickness of the laminated core is measured at 4 locations with equal intervals in the circumferential direction (i.e., every 90 degrees with the central axis O as the center). The stacking thicknesses at the 4 locations measured are divided by the number of layers of the stacked core single plates 40 to calculate the thickness of each sheet. The average value of the thickness at the 4 locations can be used as the average thickness t0 of the core single plate 40.

[0056] like Figure 5 and Figure 6 As shown, the raw material 1 includes a base steel plate 2 and an insulating film 3. Both surfaces of the strip-shaped base steel plate 2 of the raw material 1 are covered with the insulating film 3. In the present embodiment, most of the raw material 1 is formed by the base steel plate 2, and the insulating film 3 thinner than the base steel plate 2 is formed on the surface of the base steel plate 2.

[0057] The chemical composition of the base steel plate 2 is as follows in mass %, containing 2.5% to 4.5% Si in mass %. By setting the chemical composition in this range, the yield strength of the raw material 1 (core single plate 40) can be set to, for example, 380 to 540 MPa.

[0058] Si: 2.5% to 4.5%

[0059] Al: 0.001%~3.0%

[0060] Mn: 0.05%~5.0%

[0061] The rest: Fe and impurities

[0062] When the raw material 1 is used as the core single plate 40, the insulating film 3 exerts the insulating performance between the core single plates 40 adjacent to each other in the stacking direction. In addition, in the present embodiment, the insulating film 3 has the bonding ability to bond the core single plates 40 adjacent to each other in the stacking direction. The insulating film 3 may be a single-layer structure or a multi-layer structure. More specifically, for example, the insulating film 3 may be a single-layer structure having both insulating performance and bonding performance, or a multi-layer structure including a base insulating film with excellent insulating performance and an upper insulating film with excellent bonding performance.

[0063] In the present embodiment, the insulating film 3 covers both surfaces of the base steel plate 2 without gaps over the entire surface. However, within the range of ensuring the above-mentioned insulation performance or bonding performance, a part of the layer of the insulating film 3 may not cover both surfaces of the base steel plate 2 without gaps. In other words, a part of the layer of the insulating film 3 may be intermittently provided on the surface of the base steel plate 2. However, in order to ensure the insulation performance, it is necessary to cover both surfaces of the base steel plate 2 with the insulating film 3 in a manner that is not fully exposed. Specifically, in the case where the insulating film 3 does not have a base insulating film with excellent insulation performance, but is a single-layer structure having both insulation performance and bonding performance, it is necessary to form the insulating film 3 over the entire surface of the base steel plate 2 without gaps. On the other hand, in the case where the insulating film 3 is a multilayer structure including a base insulating film with excellent insulating performance and an upper insulating film with excellent bonding performance, in addition to forming both the base insulating film and the upper insulating film without gaps over the entire surface of the base steel plate 2, it is also possible to take into account both the insulating performance and the bonding performance by forming the base insulating film without gaps over the entire surface of the base steel plate and discontinuously providing the upper insulating film.

[0064] The coating composition for forming the base insulating film is not particularly limited, and for example, a general treatment agent such as a treatment agent containing chromic acid or a treatment agent containing phosphate can be used.

[0065] The insulating film with bonding ability is formed by applying the coating composition for electromagnetic steel sheet described later to the base steel sheet. The insulating film with bonding ability is, for example, a single-layer insulating film having both insulation performance and bonding ability, or an upper insulating film provided on a base insulating film. The insulating film with bonding ability is in an uncured state or a semi-cured state (B stage) before heat pressing during the manufacture of the laminated core, and exhibits bonding ability by undergoing a curing reaction by heating during heat pressing.

[0066] A general insulating film has insulating properties but does not have bonding ability. As described above, the insulating film of this embodiment is greatly different from a general insulating film and a bonding layer formed of a bonding agent in that it has bonding ability and insulating properties.

[0067] In addition, as a method of joining the base steel plates 2 formed with an insulating film that does not have bonding ability, there is a method of joining the base steel plates 2 to each other through a bonding agent composed of a thermosetting resin that exhibits bonding properties. The core single plate 40 joined and manufactured by this method is self-bonded before punching because two or more base steel plates 2 are joined to each other, but the two or more joined core single plates 40 are not joined to each other. Therefore, it is necessary to apply a bonding agent to either the front or back surface of these core single plates 40, which is poor in productivity. Since the space factor is reduced when a bonding agent is further used on the insulating film having bonding ability and insulation performance, it is a laminated core with poor magnetic properties.

[0068] The coating composition for the electromagnetic steel sheet is not particularly limited, and is, for example, a composition containing an epoxy resin and an epoxy resin curing agent. That is, as an insulating film having bonding ability, a film containing an epoxy resin and an epoxy resin curing agent is given as an example.

[0069] As epoxy resin, general epoxy resin can be used, specifically, epoxy resin containing more than 2 epoxy groups in one molecule can be used without special restrictions. As such epoxy resin, for example: bisphenol A type epoxy resin, bisphenol F type epoxy resin, phenol novolac type epoxy resin, cresol novolac type epoxy resin, alicyclic epoxy resin, glycidyl ester type epoxy resin, glycidyl amine type epoxy resin, hydantoin type epoxy resin, isocyanurate type epoxy resin, acrylic modified epoxy resin (epoxy acrylate), phosphorus-containing epoxy resin, and their halides (brominated epoxy resin, etc.) or hydrides, etc. As epoxy resin, one can also be used alone, or two or more can be used in combination.

[0070] The coating composition for an electrical steel sheet may contain an acrylic resin.

[0071] There is no particular limitation on the acrylic resin. Examples of monomers used for the acrylic resin include unsaturated carboxylic acids such as acrylic acid and methacrylic acid, methyl (meth)acrylate, ethyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, cyclohexyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, 2-hydroxyethyl (meth)acrylate, hydroxypropyl (meth)acrylate and other (meth)acrylates. It should be noted that (meth)acrylates represent acrylic acid esters or methacrylates. One acrylic resin may be used alone, or two or more acrylic resins may be used in combination.

[0072] The propylene resin may also have a constituent unit derived from other monomers other than the propylene monomer. Examples of the other monomers include ethylene, propylene, and styrene. The other monomers may be used alone or in combination of two or more.

[0073] When an acrylic resin is used, the acrylic resin may be grafted onto an epoxy resin to be used as an acrylic-modified epoxy resin. The coating composition for an electrical steel sheet may contain a monomer for forming an acrylic resin.

[0074] As epoxy resin curing agent, a latent heat curing type can be used, for example: aromatic polyamines, acid anhydrides, phenolic curing agents, dicyandiamide, boron trifluoride-amine complex, organic hydrazide, etc. As aromatic polyamines, for example: m-phenylenediamine, diaminodiphenylmethane, diaminodiphenyl sulfone, etc. As phenolic curing agent, for example: phenol novolac resin, cresol novolac resin, bisphenol novolac resin, triazine modified phenol novolac resin, phenol resol phenolic resin, etc. Among them, as epoxy resin curing agent, phenolic curing agent is preferably used, and phenol resol phenolic resin is more preferably used. As epoxy resin curing agent, one kind can be used alone, or two or more kinds can be used in combination.

[0075] The content of the epoxy resin curing agent in the coating composition for an electrical steel sheet is preferably 5 to 35 parts by mass, more preferably 10 to 30 parts by mass, based on 100 parts by mass of the epoxy resin.

[0076] The coating composition for an electrical steel sheet may be mixed with additives such as a curing accelerator (curing catalyst), an emulsifier, and a defoaming agent. As the additive, only one type may be used, or two or more types may be used in combination.

[0077] Taking into account the case where the raw material 1 is used as the core single plate 40, the upper and lower limits of the average thickness t1 of the insulating film 3 are set, for example, as follows. When the raw material 1 is used as the core single plate 40, the average thickness t1 of the insulating film 3 (the thickness per single surface of the core single plate 40 (raw material 1)) is adjusted so as to ensure the insulation performance and bonding performance between the core single plates 40 stacked on each other.

[0078] When the insulating film 3 has a single-layer structure, the average thickness t1 of the insulating film 3 (the thickness per single surface of the core single plate 40 (raw material 1 )) can be set to, for example, 1.5 μm or more and 8.0 μm or less.

[0079] When the insulating film 3 has a multilayer structure, the average thickness of the base insulating film can be, for example, 0.3 μm to 1.2 μm, preferably 0.7 μm to 0.9 μm. The average thickness of the upper insulating film is, for example, 1.5 μm to 8.0 μm.

[0080] The average thickness t1 of the insulating film 3 of the raw material 1 can be measured by finding the thickness of the insulating film 3 at a plurality of locations and averaging the thicknesses in the same way as the average thickness t0 of the raw material 1 .

[0081] The upper and lower limits of the average thickness t1 of the insulating film 3 of the raw material 1 can naturally also be adopted as the upper and lower limits of the average thickness t1 of the insulating film 3 of the core single plate 40. It should be noted that the method for measuring the average thickness t1 of the insulating film 3 of the core single plate 40 is, for example, the following measurement method. For example, among the plurality of core single plates 40 forming the laminated core, the core single plate 40 located on the outermost side in the lamination direction (the core single plate 40 whose surface is exposed in the lamination direction) is selected. On the surface of the selected core single plate 40, a predetermined radial position (for example, the middle (center) position between the inner periphery and the outer periphery of the core single plate 40) is selected. At the selected position, the thickness of the insulating film 3 of the core single plate 40 is measured at 4 locations (i.e., every 90 degrees centered on the central axis O) at equal intervals in the circumferential direction. The average value of the measured thicknesses at the 4 locations can be used as the average thickness t1 of the insulating film 3.

[0082] The reason why the average thickness t1 of the insulating film 3 is measured in the outermost core plates 40 in the stacking direction is that the insulating film 3 is manufactured so that its thickness hardly changes at stacking positions along the stacking direction of the core plates 40 .

[0083] The core single plate 40 is manufactured by punching the above-mentioned raw material 1 , and a laminated core (the stator core 21 or the rotor core 31 ) is manufactured from the core single plate 40 .

[0084] (Laminate method of laminated core)

[0085] Now let's return to the description of the laminated core. The plurality of core sheets 40 forming the stator core 21 are as follows. Figure 3 As shown, the insulating film 3 is sandwiched and stacked.

[0086] The adjacent core plates 40 in the stacking direction are joined on the entire surface by the insulating film 3. In other words, in the core plate 40, the surface facing the stacking direction (hereinafter referred to as the first surface) is the entire surface that becomes the joining area. However, the adjacent core plates 40 in the stacking direction may not be joined on the entire surface. In other words, on the first surface of the core plate 40, the joining area 41a and the non-joining area (not shown) may be mixed.

[0087] In this embodiment, the plurality of core plates forming the rotor core 31 are formed by Figure 1 However, the plurality of core plates forming the rotor core 31 may have a stacked structure fixed by the insulating film 3 similarly to the stator core 21 .

[0088] In addition, the laminated cores such as the stator core 21 and the rotor core 31 may be formed by so-called rotational lamination.

[0089] (Method for manufacturing laminated core)

[0090] The following reference Figure 7 and 8 , a method for manufacturing a laminated core according to an embodiment of the present invention is described. It should be noted that, Figure 7 is a side view of a manufacturing device used for manufacturing a laminated iron core. Figure 8 1 is a flowchart of the method for manufacturing a laminated iron core according to the present embodiment. In the following, regarding the description of the manufacturing method, first, a manufacturing apparatus 100 for a laminated iron core (hereinafter simply referred to as manufacturing apparatus 100) will be described.

[0091] In the manufacturing apparatus 100, the raw material 1 is fed from two steel coils 1A (strip steel) to the upstream side in the conveying direction ( Figure 7 The two raw materials 1 are temporarily joined by the guide roller 2A. Then, the two temporarily joined raw materials 1 are further sent to the upstream side in the conveying direction, and are gradually formed into the shape of the core single plate 40 by multiple punching by the molds arranged on each workbench. Furthermore, the punched core single plates 40 are stacked and conveyed to a heating device (not shown) to be pressurized while being heated. As a result, the core single plates 40 adjacent to each other in the stacking direction are joined by the insulating film 3 (that is, the portion of the insulating film 3 located in the joining area 41a exerts the joining ability), and the formal joining is completed.

[0092] exist Figure 7 In the embodiment, the manufacturing apparatus 100 includes two steel coils 1A, but may include three or more steel coils 1A.

[0093] In addition, the manufacturing device 100 includes a plurality of punching stations 110. The punching stations 110 may be two-stage or three-stage or more. Each punching station 110 includes a female die 111 disposed below the raw material 1 and a male die 112 disposed above the raw material 1. It should be noted that the plurality of punching stations 110 may be collectively referred to as punching dies.

[0094] The manufacturing method of the laminated iron core of the present embodiment is to obtain an iron core single plate by punching out an electromagnetic steel strip having an insulating coating, and to stack the iron core single plates to manufacture the laminated iron core. Before the punching process, two or more electromagnetic steel strips are temporarily joined by pressurizing them with a guide roller, and the two or more electromagnetic steel strips temporarily joined are inserted into a punching die, and then the iron core single plate is obtained by performing the punching process.

[0095] The details are described below.

[0096] (Temporary bonding by pressure)

[0097] First, before the blanking process is performed by the blanking die, two or more raw materials 1 (electromagnetic steel strips) are temporarily joined by pressurization with the guide roller 2A. The temporarily joined raw materials 1 have an insulating film 3 on both sides. The insulating film 3 is preferably formed in a manner such that the average thickness t1 is within the above range. In addition, as described above, the insulating film 3 has insulating performance and joining ability.

[0098] It should be noted that the guide roller 2A is a roller for conveying the raw material 1 to the punching die, and is arranged on the upstream side of the conveying direction of the punching die ( Figure 7 ). In addition, before blanking processing means that no processing is performed after temporary joining and before blanking processing.

[0099] In this embodiment, temporary joining means joining two or more raw materials 1 before punching by pressurization without heating. After temporary joining, the raw materials are temporarily fixed to each other. The two or more raw materials 1 after temporary joining are formally joined by heating described later after punching.

[0100] It should be noted that in this embodiment, no bonding agent is used when bonding two or more raw materials 1. Since the space factor is reduced when bonding is performed by bonding agent instead of by pressurization, a laminated core with poor magnetic properties will be obtained. Therefore, it is not desirable to use a bonding agent.

[0101] As described above, in the present embodiment, it is not necessary to heat more than two pieces of raw material 1 during temporary joining. In order to heat the raw material 1 during temporary joining, a heating device is required, and the heating of the raw material 1 takes time, so the productivity is significantly reduced. The surface temperature of more than two pieces of raw material 1 during temporary joining can be room temperature, for example, 15 to 50°C. The surface temperature of the raw material 1 is obtained by using an infrared radiation thermometer to measure the temperature of the central part of the width direction of more than two pieces of raw material 1 during temporary joining, and calculating their average value.

[0102] The pressure from the guide roller 2A during provisional joining is preferably 2.0 to 10.0 MPa. By setting the pressure within this range, two or more raw materials 1 can be provisionally joined reliably.

[0103] Whether or not two or more raw materials 1 are in a state of being temporarily joined is determined by the following method.

[0104] A test piece of a predetermined size was taken and used for a tensile test (shear tensile test in accordance with JIS K 6850:1999). The peel strength per unit area obtained by the tensile test was set at 5 N / cm 2 In the above case, it is determined that two or more raw materials 1 are in a temporarily joined state.

[0105] (Punching)

[0106] The two or more temporarily joined raw materials 1 are inserted into the punching die ( Figure 7 The desired shape is, for example, the shape of the core single plate 40 having the shape of the stator core 21 or the rotor core 31. The core single plates 40 punched into the desired shape are stacked in the female die 111 located in the most downstream direction of the punching die. By repeating the punching and stacking described above in sequence, a predetermined number of core single plates 40 are stacked.

[0107] (Formal Engagement)

[0108] The stacked core sheets 40 are conveyed to a heating device (not shown) and heated to a temperature range of, for example, 180 to 250° C. by the heating device to be formally joined. The bonding agent (insulating film 3) is cured by the heating to form a joining region 41a. When conveyed to the heating device, the stacked core sheets 40 are held by clamps (not shown) from both sides in the stacking direction and then conveyed.

[0109] The laminated core can be manufactured by the method described above.

[0110] It should be noted that in this embodiment, as in the judgment of temporary bonding, a shear tensile test is performed to determine whether the core plate 40 is in a formally bonded state. 2 The above situation is judged as the core single plate 40 being in a fully joined state.

[0111] Example

[0112] (Example 1)

[0113] As a method of the present invention, two steel coils of non-oriented electrical steel strips are prepared, each having an insulating film formed on the surface and processed to a predetermined cutting width and a plate thickness of 0.20 mm. As the non-oriented electrical steel strip, a non-oriented electrical steel strip containing, by mass%, 3.3% Si, 0.7% Al, 0.2% Mn, and the remainder Fe and impurities is used. The insulating film uses a single-layer insulating film having insulating properties and bonding performance. The average thickness of the insulating film is 1.5 μm or more and 8.0 μm or less per single surface of each core plate. Two sheets of non-oriented electrical steel strips are temporarily bonded by pressurizing them using a guide roller. It should be noted that the pressure of the guide roller is 2.0 to 10.0 MPa, and the surface temperature of the non-oriented electrical steel strips during temporary bonding is 15 to 50°C. The two non-oriented electrical steel strips after temporary bonding are used in a shear tensile test in accordance with JIS K 6850:1999, and the peel strength per unit area obtained is 5 N / cm 2 above.

[0114] Then, the temporarily joined non-oriented electromagnetic steel strip is inserted into the punching die, and punched into the predetermined core single plate shape in the temporarily joined state. By synchronizing and repeating this action, the core single plates are stacked in the female die located in the most downstream direction of the punching die. The stacked core single plates are conveyed to the heating device and formally joined by heating to 180-250°C. The formally joined non-oriented electromagnetic steel sheet is used for the shear tensile test in accordance with JIS K 6850:1999, and the peel strength per unit area obtained is 250N / cm 2 above.

[0115] An insulating film having bonding ability is formed on the non-oriented electrical steel strip. Therefore, the core single plates stacked in the female mold are heated by a heating device to obtain a fully bonded laminated core.

[0116] (Example 2)

[0117] A non-oriented electrical steel strip having a thickness of 0.20 mm and containing, by mass%, 3.3% Si, 0.7% Al, and 0.2% Mn, with the remainder being Fe and impurities, and having an insulating film on the surface was prepared. As the insulating film, a treatment agent containing chromic acid was used as a coating composition for forming a base insulating film, and as an upper insulating film provided on the base insulating film, an insulating film having insulating properties and bonding performance was formed. The average thickness of the base insulating film of the insulating film was 0.3 μm to 1.2 μm, and the average thickness of the upper insulating film was 1.5 μm to 8.0 μm. The non-oriented electrical steel strip was cut into pieces of 25 mm × 200 mm, overlapped in an area of ​​25 mm × 25 mm, and pressed with various pressing forces as shown in Table 1. Then, the overlapped portion was subjected to a shear tensile test in accordance with JIS K 6850:1999 at a test speed of 3 mm / min with the overlapped portion facing the sheared direction.

[0118] Table 1

[0119]

[0120] In the test numbers 1 and 2 where the applied pressure was small, sufficient peel strength could not be obtained, and thus a temporary bonding state could not be achieved. In contrast, since the applied pressure in the test numbers 3 to 6 was within an appropriate range, the peel strength was also within an appropriate range, and an excellent temporary bonding state was achieved.

[0121] (Example 3)

[0122] Two coils of non-oriented electrical steel strips processed to a predetermined cutting width and a plate thickness of 0.20 mm were prepared. As the non-oriented electrical steel strip, a non-oriented electrical steel strip containing, by mass%, 3.3% Si, 0.7% Al, 0.2% Mn, and the remainder Fe and impurities was used.

[0123] No. 7 and 9 have an insulating film formed on the surface. The insulating film is a single-layer insulating film having insulating performance and bonding performance. The average thickness of the insulating film is 1.5 μm or more and 8.0 μm or less per single surface of the core plate.

[0124] In No. 8, no insulating film was formed.

[0125] In No. 7, two non-oriented electrical steel strips were heated and then pressed using a guide roll.

[0126] In No. 8, after applying an adhesive between the non-oriented electrical steel strips, the strips were pressed with a guide roll.

[0127] In No. 9, an adhesive was applied between the non-oriented electrical steel strips having the insulating coating, and then pressed with a guide roll.

[0128] In addition, the pressure of the guide roll in No. 7 to 9 was 2.0 to 10.0 MPa. In No. 7, the surface temperature of the non-oriented electrical steel strip during pressurization exceeded 50° C. In No. 8 and 9, a thermosetting resin exhibiting adhesiveness was used as an adhesive, and the surface temperature of the non-oriented electrical steel strip during pressurization was 15 to 50° C.

[0129] Then, the pressurized non-oriented electromagnetic steel strip is inserted into the punching die and punched into the predetermined core single plate shape. By synchronizing and repeating this action, the core single plates are stacked in the female die located in the most downstream direction of the punching die. The stacked core single plates are transported to the heating device and heated to 180-250°C for bonding.

[0130] In No. 7, since heating was performed before pressing, the non-oriented electromagnetic steel strips before punching were joined, but the core sheets after punching were not joined. In order to join such core sheets, it is necessary to join with a bonding agent, rivet, welding, etc., which deteriorates productivity.

[0131] In No. 8, since the non-oriented electrical steel strips were bonded to each other by a bonding agent without forming an insulating film, the non-oriented electrical steel strips before punching were bonded, but the core single plates after punching were not bonded, similarly to No. 7. In addition, since no insulating film was formed, the insulation property was deteriorated, and the magnetic properties were deteriorated.

[0132] In No. 9, since an adhesive was applied on the insulating film, the space factor was inferior to that of Example 1 in which no adhesive was used.

[0133] An embodiment and examples of the present invention have been described above, but the technical scope of the present invention is not limited to the embodiment and examples described above, and various modifications can be added without departing from the gist of the present invention.

[0134] For example, the shape of the stator core 21 is not limited to the shape shown in the above embodiment. Specifically, the outer diameter and inner diameter of the stator core 21, the stacking thickness, the number of slots, the circumferential and radial dimension ratios of the teeth 23, and the radial dimension ratios of the teeth 23 and the core back 22 can be arbitrarily designed according to the desired characteristics of the rotating electrical machine.

[0135] In the rotor 30 of the above embodiment, a set of two permanent magnets 32 forms one magnetic pole, but the present invention is not limited to this form. For example, one permanent magnet 32 ​​may form one magnetic pole, or three or more permanent magnets 32 may form one magnetic pole.

[0136] In the above embodiment, a permanent magnet excitation type motor is used as an example to explain the rotating electrical machine 10, but the structure of the rotating electrical machine 10 is not limited to the permanent magnet excitation type motor as shown below, and various well-known structures not shown below may be adopted.

[0137] In the above embodiment, a permanent magnet excitation motor is described as an example of the rotating electrical machine 10, but the present invention is not limited thereto. For example, the rotating electrical machine 10 may be a reluctance motor or an electromagnetic excitation motor (winding excitation motor).

[0138] In the above embodiment, a synchronous motor is described as an example of an AC motor, but the present invention is not limited to this. For example, the rotating electric machine 10 may be an induction motor.

[0139] In the above embodiment, an AC motor is described as an example of the rotating electrical machine 10, but the present invention is not limited thereto. For example, the rotating electrical machine 10 may be a DC motor.

[0140] In the above embodiment, an electric motor is used as an example to explain the rotating electric machine 10, but the present invention is not limited to this. For example, the rotating electric machine 10 may be a generator. In addition, it is also applicable to a transformer.

[0141] Furthermore, the components of the above-described embodiments may be appropriately replaced with well-known components without departing from the spirit of the present invention, and the above-described modifications may be appropriately combined.

[0142] Description of Reference Numerals

[0143] 1Raw materials, electromagnetic steel strip

[0144] 1A Steel Coil

[0145] 2. Base steel plate

[0146] 3 Insulation coating

[0147] 10 Rotating motor

[0148] 21 stator core

[0149] 22 Core back

[0150] 23 teeth

[0151] 30 Rotor

[0152] 31 Rotor core

[0153] 32 Permanent magnet

[0154] 33 Through hole

[0155] 40 core single board

[0156] 41a Junction area

[0157] 50 Shell

Claims

1. A method for manufacturing a laminated iron core, wherein an iron core single plate is obtained by punching an electromagnetic steel strip having an insulating film, and the iron core single plates are stacked to manufacture the laminated iron core, wherein the insulating film has bonding ability, characterized in that: Prior to the punching process, two or more electromagnetic steel strips are overlapped so that the insulating films on the respective electromagnetic steel strips are in contact with each other, and are temporarily bonded by applying pressure with a guide roller without applying a bonding agent. After the two or more electromagnetic steel strips that have been temporarily joined are inserted into a punching die, the core single plate is obtained by performing the punching process. The pressure applied by the guide roller during the pressurization is 2.0 to 10.0 MPa, The peel strength of the electromagnetic steel strip after the temporary bonding is 5.0 N / cm 2 above, However, the method does not include applying a bonding agent when stacking the core sheets, and does not include heating before the pressurizing, heating during the pressurizing, or heating after the pressurizing and before the punching process.

2. The method for manufacturing a laminated core according to claim 1, wherein: The surface temperature of the two or more electromagnetic steel strips during the provisional joining is 15 to 50°C.

3. The method for manufacturing a laminated core according to claim 1 or 2, characterized in that: After the punching process, the core single plates are heated to 180 to 250° C. to perform formal bonding.

Citation Information

Patent Citations

  • Method of manufacturing laminated core

    JP2005191033A