Formation method of semiconductor structure
By forming a protective layer with a material different from the buffer layer on the initial isolation structure surface of the second groove during the manufacturing process of the Nor Flash device, the problem of difficulty in precise control of the size and spacing of the floating gate electrode is solved, and reliability and process are improved Adjustability reduces process deviation.
Patent Information
- Application Number
- CN202310636675.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-31
- Publication Date
- 2024-12-03
AI Technical Summary
During the manufacturing process, existing Nor Flash devices have problems such as difficult to accurately control the size and spacing of floating gates, resulting in reduced reliability and process deviation.
The protective layer is formed on the surface of the initial isolation structure of the second groove. The material is different from the buffer layer to protect the sidewalls of the initial isolation structure from damage, and to protect the initial isolation structure when removing the buffer layer, ensuring that its width loss is small, and precise control of floating The size and spacing of the gate structure.
Through the use of the protective layer, the width of the initial isolation structure and the size and spacing of the floating gate structure are accurately controlled, which avoids the reliability reduction caused by too small spacing of the floating gate structure, reduces process deviations, and improves process adjustability .
Smart Images

Figure CN119072123A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of semiconductor manufacturing, and in particular to a method for forming a semiconductor structure. Background Art
[0002] NOR Flash is a non-volatile flash memory technology. The feature of NOR Flash is on-chip execution (eXecute InPlace, referred to as XIP), so that the application can run directly in the flash memory without having to read the code into the system RAM. NOR Flash has a very high transmission efficiency.
[0003] However, Nor Flash devices manufactured using existing processes still have some potential problems or bottlenecks. Summary of the invention
[0004] The technical problem solved by the present invention is to provide a method for forming a semiconductor structure to improve the performance of a Nor Flash device.
[0005] To solve the above technical problems, the technical solution of the present invention provides a method for forming a semiconductor structure, including: providing a substrate; forming a buffer layer on the surface of the substrate; forming a hard mask structure on the buffer layer, wherein the hard mask structure has a plurality of first grooves parallel to a first direction, wherein the first grooves expose the surface of the buffer layer, and the first direction is parallel to the surface of the substrate; etching the buffer layer and the substrate using the hard mask structure as a mask to form an isolation groove in the substrate at the bottom of the first groove; forming an initial isolation structure in the first groove and in the isolation groove; after forming the initial isolation structure, removing the hard mask structure, forming a plurality of second grooves between the initial isolation structures, wherein the second grooves expose the surface of the buffer layer; forming a protective layer on the surface of the initial isolation structure on the sidewalls of the second grooves, wherein the material of the protective layer is different from that of the buffer layer; after forming the protective layer, removing the buffer layer at the bottom of the second groove; after removing the buffer layer, forming a floating gate structure in the second groove, wherein the floating gate structure exposes the top surface of the initial isolation structure.
[0006] Optionally, the width of the first groove in the second direction is greater than the width of the isolation structure at the bottom of the first groove in the second direction, and the second direction is parallel to the substrate surface and perpendicular to the first direction.
[0007] Optionally, before forming the initial isolation structure in the first groove and the isolation groove, the method further includes: removing a portion of the hard mask structure on the sidewall of the first groove.
[0008] Optionally, the process of removing a portion of the hard mask structure on the sidewall of the first groove includes a wet etching process.
[0009] Optionally, in the process of removing the buffer layer at the bottom of the second groove, an etching rate of the buffer layer is greater than an etching rate of the protective layer.
[0010] Optionally, the process of removing the buffer layer at the bottom of the second groove includes a wet etching process.
[0011] Optionally, the material of the buffer layer includes a dielectric material, and the dielectric material includes a combination of one or more of silicon oxide, silicon nitride, silicon carbide, silicon oxycarbide, silicon nitride oxide, aluminum oxide, aluminum nitride, silicon carbide nitride and silicon carbon nitride oxide; the material of the protective layer includes a dielectric material, and the dielectric material includes a combination of one or more of silicon oxide, silicon nitride, silicon carbide, silicon oxycarbide, silicon nitride oxide, aluminum oxide, aluminum nitride, silicon carbide nitride and silicon carbon nitride oxide.
[0012] Optionally, the material of the buffer layer includes silicon oxide; and the material of the protective layer includes silicon nitride.
[0013] Optionally, the floating gate structure includes: a tunneling oxide layer located on the bottom surface of the second groove, and a floating gate layer located on the tunneling oxide layer.
[0014] Optionally, the method for forming a floating gate structure in the second groove includes: removing the protective layer after removing the buffer layer at the bottom of the second groove; after removing the protective layer, forming a tunneling oxide material layer and a floating gate material layer located on the tunneling oxide material layer in the second groove; planarizing the floating gate material layer and the tunneling oxide material layer until the top surface of the initial isolation structure is exposed, and forming a tunneling oxide layer and a floating gate layer located on the tunneling oxide layer in the second groove.
[0015] Optionally, the process of removing the protective layer includes a wet etching process.
[0016] Optionally, it also includes: forming a control gate structure on the top surface and sidewall surface of the floating gate structure, the control gate structure spanning the floating gate structure; the control gate structure includes a gate dielectric layer and a control gate layer located on the gate dielectric layer.
[0017] Optionally, the method for forming the control gate structure includes: after forming a floating gate structure, removing an initial isolation structure on the side wall of the floating gate structure to expose the side wall surface and top surface of the floating gate structure, and forming an isolation structure located in an isolation groove; forming a gate dielectric layer on the side wall surface and top surface of the floating gate structure, and the top surface of the isolation structure; forming a control gate layer on the gate dielectric layer, wherein the control gate layer is parallel to a second direction, the second direction is parallel to the substrate surface, and the second direction is perpendicular to the first direction.
[0018] Compared with the prior art, the technical solution of the present invention has the following beneficial effects:
[0019] The technical solution of the present invention forms a protective layer on the surface of the initial isolation structure of the second groove, and then removes the buffer layer at the bottom of the second groove. Since the material of the protective layer is different from that of the buffer layer, when the buffer layer is removed, the protective layer can protect the side wall surface of the initial isolation structure from being damaged, so that the width loss of the initial isolation structure is small, and the width of the initial isolation structure can be accurately controlled, thereby accurately controlling the size and spacing of the floating gate structure, avoiding the problem of reliability degradation caused by too small spacing of the floating gate structure, and reducing process deviation.
[0020] Furthermore, after removing the protective layer, a floating gate structure is formed in the second groove. Since the width loss of the initial isolation structure is small, the width of the initial isolation structure can be adjusted again after removing the protective layer, and the size and spacing of the floating gate structure can be precisely controlled, and the process adjustability is strong.
[0021] Furthermore, before forming the initial isolation structure in the first groove and the isolation groove, part of the hard mask structure on the side wall of the first groove is removed, so that the width of the initial isolation structure formed subsequently on the substrate is larger. The size and spacing of the floating gate structure can be accurately controlled by adjusting the initial isolation structure, thereby avoiding the problem of reduced reliability due to too small spacing of the floating gate structure. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] Figure 1 is a schematic diagram of a semiconductor structure forming process in one embodiment;
[0023] Figures 2 to 12 Schematic diagram of a semiconductor structure forming process in an embodiment of the present invention. DETAILED DESCRIPTION
[0024] As described in the background art, the Nor Flash device manufactured by the existing process still has some potential problems or bottlenecks, which will now be analyzed and explained in conjunction with specific embodiments.
[0025] Figure 1 is a schematic diagram of a semiconductor structure forming process in one embodiment.
[0026] Please refer to Figure 1The semiconductor structure formation process includes: providing a substrate 100; forming a buffer layer 101 on the surface of the substrate 100; forming a hard mask structure 102 on the buffer layer 101, wherein the hard mask structure 102 has a plurality of first grooves arranged along a first direction X (not shown); etching the buffer layer 101 and the substrate 100 using the hard mask structure 102 as a mask to form an isolation groove (not shown) in the substrate 100 at the bottom of the first groove; and forming an initial isolation structure 103 in the first groove and in the isolation groove.
[0027] The semiconductor structure formation process also includes: removing the hard mask structure 102, forming a plurality of second grooves (not shown) between the initial isolation structures 102, wherein the second grooves expose the surface of the buffer layer 101; removing the buffer layer 101 at the bottom of the second grooves; after removing the buffer layer 101, forming a floating gate structure in the second grooves; after forming the floating gate structure, removing the initial isolation structure 103 in the first groove between the floating gate structures, and forming an isolation structure in the isolation groove; and forming a control gate structure in the first groove and on the floating gate structure.
[0028] In the process of removing the hard mask structure 102, a part of the side wall of the initial isolation structure 102 will also be removed; the process of removing the buffer layer 101 includes a wet etching process to avoid damage to the substrate surface caused by the dry etching process, and a part of the side wall of the initial isolation structure 102 will also be removed, which makes the width of the second groove formed in the first direction X larger. When the floating gate structure is formed in the second groove, the distance between the floating gate structures is too close, which will affect each other, thereby causing reading errors; the initial isolation structure 103 in the first groove between the floating gate structures is subsequently removed, and when the control gate structure is formed in the first groove and on the floating gate structure, due to the small width of the first groove, the quality of the control gate structure formed by the deposition process in the first groove is also poor, and voids are prone to occur, causing difficulty in erasing. In summary, the size of the floating gate structure cannot be accurately controlled, resulting in a too close distance between the floating gates, which leads to a problem of reduced reliability.
[0029] In order to solve the above problems, on the one hand, before forming the initial isolation structure 103 in the first groove and the isolation groove, part of the hard mask structure 102 on the sidewall of the first groove is removed to increase the width of the first groove in the first direction, thereby increasing the width of the initial isolation structure 103 in the first groove, that is, increasing the spacing between the floating gate structures subsequently formed in the second groove, and improving reliability. However, even if the hard mask structure 102 becomes smaller, there are boundary conditions, and the hard mask structure 102 cannot be made too thin, which will cause the pattern to be missing or unable to stand, and the width of the first groove in the first direction cannot be greatly increased.
[0030] On the other hand, when the buffer layer 101 is removed by a wet etching process, the concentration of the wet etching solution is reduced while ensuring that the buffer layer 101 is completely removed. However, reducing the concentration of the wet etching solution also has boundary conditions and needs to meet process requirements, and the width of the first groove in the first direction cannot be greatly increased.
[0031] In order to solve the above problems, the technical solution of the present invention provides a method for forming a semiconductor structure, by forming a protective layer on the surface of the initial isolation structure of the second groove, and then removing the buffer layer at the bottom of the second groove. Since the material of the protective layer is different from that of the buffer layer, when the buffer layer is removed, the protective layer can protect the side wall surface of the initial isolation structure from damage, so that the width loss of the initial isolation structure is small, and the width of the initial isolation structure can be accurately controlled, thereby accurately controlling the size and spacing of the floating gate structure, avoiding the problem of reliability degradation caused by too small spacing of the floating gate structure, and reducing process deviation.
[0032] In order to make the above-mentioned objects, features and beneficial effects of the present invention more obvious and easy to understand, specific embodiments of the present invention are described in detail below with reference to the accompanying drawings.
[0033] Figures 2 to 12 Schematic diagram of a semiconductor structure forming process in an embodiment of the present invention.
[0034] Please refer to Figure 2 and Figure 3 , Figure 2 for Figure 3 Schematic diagram of the cross-sectional structure along the section line AA1, Figure 3 for Figure 2 A top view of a substrate 200 is provided.
[0035] In this embodiment, the material of the substrate 200 is silicon.
[0036] In other embodiments, the substrate material includes silicon carbide, silicon germanium, a multinary semiconductor material composed of group III-V elements, silicon on insulator (SOI) or germanium on insulator (GOI). Among them, the multinary semiconductor material composed of group III-V elements includes InP, GaAs, GaP, InAs, InSb, InGaAs or InGaAsP.
[0037] Please continue to refer to Figure 2 and Figure 3 , a buffer layer 201 is formed on the surface of the substrate 200 .
[0038] The buffer layer 201 is used to protect the surface of the substrate 200 from being damaged.
[0039] The material of the buffer layer 201 includes a dielectric material, and the dielectric material includes one or more combinations of silicon oxide, silicon nitride, silicon carbide, silicon oxycarbide, silicon oxynitride, aluminum oxide, aluminum nitride, silicon carbide nitride, and silicon oxycarbide nitride.
[0040] In this embodiment, the material of the buffer layer 201 includes silicon oxide. The process of forming the buffer layer 201 includes a wet oxidation process.
[0041] Please continue to refer to Figure 2 and Figure 3 A hard mask structure 202 is formed on the buffer layer 201 , wherein the hard mask structure 202 has a plurality of first grooves 203 parallel to a first direction Y, wherein the first grooves 203 expose the surface of the buffer layer 201 , and the first direction Y is parallel to the surface of the substrate 200 .
[0042] In this embodiment, the material of the hard mask structure 202 includes silicon nitride.
[0043] In this embodiment, the material of the hard mask structure 202 is different from that of the buffer layer 201 , so that the buffer layer 201 can better protect the substrate surface during the process of forming the hard mask structure 202 .
[0044] Please refer to Figure 4 , Figure 4 For Figure 3 Based on the schematic diagram, the buffer layer 201 and the substrate 200 are etched using the hard mask structure 202 as a mask to form an isolation groove 204 in the substrate 200 at the bottom of the first groove 203.
[0045] The isolation groove 204 is used to form an isolation structure in the isolation groove 204. The process of etching the substrate 200 includes a dry etching process.
[0046] Please refer to Figure 5 , removing part of the hard mask structure 202 on the sidewall of the first groove 203 .
[0047] After removing part of the hard mask structure 202 on the sidewall of the first groove 203 , the width of the first groove 203 in the second direction X is greater than the width of the isolation groove 204 in the second direction X. The second direction X is parallel to the surface of the substrate 200 and perpendicular to the first direction Y.
[0048] In this embodiment, the process of removing a portion of the hard mask structure 202 on the sidewall of the first groove 203 includes a wet etching process.
[0049] Part of the hard mask structure 202 on the side wall of the first groove 203 is removed, and the width of the first groove 203 in the second direction X is greater than the width of the isolation groove 204 in the second direction X, so that the width of the initial isolation structure subsequently formed in the first groove 203 on the substrate 200 is larger, and the size and spacing of the floating gate structure can be accurately controlled by adjusting the initial isolation structure, thereby avoiding the problem of reduced reliability due to too small spacing of the floating gate structure.
[0050] Please refer to Figure 6 , an initial isolation structure 206 is formed in the first groove 203 and the isolation groove 204 .
[0051] The material of the initial isolation structure 206 includes a dielectric material, and the dielectric material includes one or more combinations of silicon oxide, silicon nitride, silicon carbide, silicon oxycarbide, silicon oxynitride, aluminum oxide, aluminum nitride, silicon carbide nitride, and silicon carbide nitride.
[0052] In this embodiment, the material of the initial isolation structure 206 includes silicon oxide.
[0053] Please refer to Figure 7 After the initial isolation structure 206 is formed, the hard mask structure 202 is removed, and a plurality of second grooves 207 are formed between the initial isolation structures 206 , wherein the second grooves 207 expose the surface of the buffer layer 201 .
[0054] Please refer to Figure 8 A protection layer 208 is formed on the surface of the initial isolation structure 206 at the sidewall of the second groove 207 . The material of the protection layer 208 is different from that of the buffer layer 201 .
[0055] The material of the protection layer 208 includes a dielectric material, and the dielectric material includes one or more combinations of silicon oxide, silicon nitride, silicon carbide, silicon oxycarbide, silicon oxynitride, aluminum oxide, aluminum nitride, silicon carbide nitride, and silicon oxycarbide nitride.
[0056] In this embodiment, the material of the protection layer 208 includes silicon nitride.
[0057] The formation process of the protective layer 208 includes: forming a protective material layer (not shown) on the side wall surface and bottom surface of the second groove 207 and the surface of the initial isolation structure 206; etching back the protective material layer until the surface of the buffer layer 201 is exposed, and forming a protective layer 208 on the surface of the initial isolation structure 206 on the side wall of the second groove 207.
[0058] Please refer to Fig. 9 After forming the protection layer 208 , the buffer layer 201 at the bottom of the second groove 207 is removed.
[0059] In the process of removing the buffer layer 201 at the bottom of the second groove 207 , the etching rate of the buffer layer 201 is greater than the etching rate of the protection layer 208 .
[0060] In this embodiment, the process of removing the buffer layer 201 at the bottom of the second groove 207 includes a wet etching process, and the wet etching process will not cause damage to the surface of the substrate 200 .
[0061] In this embodiment, the wet etching process includes an etchant containing hydrofluoric acid. Due to the protective effect of the protective layer 208 on the initial isolation structure 206, there is no need to worry about the damage of the hydrofluoric acid to the initial isolation structure 206. The concentration of the hydrofluoric acid can be adjusted to the maximum within the process allowable range, which can improve production efficiency.
[0062] The protective layer 208 can protect the side wall surface of the initial isolation structure 206 from being damaged, so that the width loss of the initial isolation structure 206 is small, and the width of the initial isolation structure 206 can be accurately controlled, thereby accurately controlling the size and spacing of the subsequently formed floating gate structure, avoiding the problem of reduced reliability due to too small spacing of the floating gate structure, and reducing process deviation.
[0063] Next, after removing the buffer layer 201, a floating gate structure is formed in the second groove 207, and the floating gate structure exposes the top surface of the initial isolation structure 206. The formation process of the floating gate structure can be found in Fig.10 and Fig.11 .
[0064] The floating gate structure includes: a tunneling oxide layer 210 located on the bottom surface of the second groove 207 , and a floating gate layer 209 located on the tunneling oxide layer.
[0065] Please refer to Fig.10 After removing the buffer layer 201 at the bottom of the second groove 207 , the protection layer 208 is removed.
[0066] In this embodiment, the process of removing the protection layer 208 includes a wet etching process.
[0067] Please refer to Fig.11 After removing the protective layer 208, a tunneling oxide material layer (not shown) and a floating gate material layer (not shown) located on the tunneling oxide material layer are formed in the second groove 207; the floating gate material layer and the tunneling oxide material layer are planarized until the top surface of the initial isolation structure 206 is exposed, and a tunneling oxide layer 210 and a floating gate layer 209 located on the tunneling oxide layer 210 are formed in the second groove 207.
[0068] In this embodiment, the material of the tunneling oxide layer 210 includes silicon oxide; and the material of the floating gate layer 209 includes polysilicon.
[0069] After removing the protection layer 208, a floating gate structure is formed in the second groove 207. Since the width loss of the initial isolation structure 206 is small, the width of the initial isolation structure 206 can be adjusted again after removing the protection layer 208, and the size and spacing of the floating gate structure can be precisely controlled, and the process adjustability is strong.
[0070] Please refer to Fig.12 A control gate structure is formed on the top surface and sidewall surface of the floating gate structure, and the control gate structure spans the floating gate structure.
[0071] The control gate structure includes a gate dielectric layer 212 and a control gate layer 213 located on the gate dielectric layer 212 .
[0072] The method for forming the control gate structure includes: after forming the floating gate structure, removing the initial isolation structure 206 on the side wall of the floating gate structure to expose the side wall surface and the top surface of the floating gate structure, and forming an isolation structure 211 located in the isolation groove; forming a gate dielectric layer 212 on the side wall surface and the top surface of the floating gate structure, and the top surface of the isolation structure; forming a control gate layer 213 on the gate dielectric layer 212, and the control gate layer 213 is parallel to the second direction X.
[0073] In this embodiment, when the initial isolation structure 206 on the sidewall of the floating gate structure is removed, the tunneling oxide layer 210 on the sidewall of the floating gate structure is also removed.
[0074] In this embodiment, the material of the gate dielectric layer 212 includes silicon oxide, silicon nitride or aluminum oxide; the material of the control gate layer 213 includes polysilicon.
[0075] Although the present invention is disclosed as above, the present invention is not limited thereto. Any person skilled in the art can make various changes and modifications without departing from the spirit and scope of the present invention. Therefore, the protection scope of the present invention shall be subject to the scope defined by the claims.
Claims
1. A method for forming a semiconductor structure, characterized in that: include: providing a substrate; forming a buffer layer on a surface of the substrate; forming a hard mask structure on the buffer layer, wherein the hard mask structure has a plurality of first grooves parallel to a first direction, wherein the first grooves expose a surface of the buffer layer, and the first direction is parallel to a surface of the substrate; Etching the buffer layer and the substrate using the hard mask structure as a mask to form an isolation groove in the substrate at the bottom of the first groove; forming an initial isolation structure in the first groove and in the isolation groove; After forming the initial isolation structure, removing the hard mask structure, forming a plurality of second grooves between the initial isolation structures, wherein the second grooves expose the surface of the buffer layer; forming a protection layer on the surface of the initial isolation structure on the sidewall of the second groove, wherein the material of the protection layer is different from the material of the buffer layer; After forming the protective layer, removing the buffer layer at the bottom of the second groove; After removing the buffer layer, a floating gate structure is formed in the second groove, wherein the floating gate structure exposes the top surface of the initial isolation structure.
2. The method for forming a semiconductor structure according to claim 1, wherein: The width of the first groove in the second direction is greater than the width of the isolation structure at the bottom of the first groove in the second direction. The second direction is parallel to the substrate surface and perpendicular to the first direction.
3. The method for forming a semiconductor structure according to claim 2, wherein: Before forming the initial isolation structure in the first groove and the isolation groove, the method further includes: removing a portion of the hard mask structure on the sidewall of the first groove.
4. The method for forming a semiconductor structure according to claim 3, wherein: The process of removing a portion of the hard mask structure on the sidewall of the first groove includes a wet etching process.
5. The method for forming a semiconductor structure according to claim 1, wherein: In the process of removing the buffer layer at the bottom of the second groove, an etching rate of the buffer layer is greater than an etching rate of the protection layer.
6. The method for forming a semiconductor structure according to claim 5, wherein: The process of removing the buffer layer at the bottom of the second groove includes a wet etching process.
7. The method for forming a semiconductor structure according to claim 5, wherein: The material of the buffer layer includes a dielectric material, and the dielectric material includes a combination of one or more of silicon oxide, silicon nitride, silicon carbide, silicon oxycarbide, silicon nitride oxide, aluminum oxide, aluminum nitride, silicon carbide nitride and silicon oxycarbon nitride; the material of the protective layer includes a dielectric material, and the dielectric material includes a combination of one or more of silicon oxide, silicon nitride, silicon carbide, silicon oxycarbide, silicon nitride oxide, aluminum oxide, aluminum nitride, silicon carbide nitride and silicon oxycarbon nitride.
8. The method for forming a semiconductor structure according to claim 7, wherein: The material of the buffer layer includes silicon oxide; the material of the protection layer includes silicon nitride.
9. The method for forming a semiconductor structure according to claim 1, wherein: The floating gate structure includes: a tunneling oxide layer located on the bottom surface of the second groove, and a floating gate layer located on the tunneling oxide layer.
10. The method for forming a semiconductor structure according to claim 9, wherein: The method for forming a floating gate structure in the second groove comprises: removing the protective layer after removing the buffer layer at the bottom of the second groove; forming a tunneling oxide material layer and a floating gate material layer located on the tunneling oxide material layer in the second groove after removing the protective layer; planarizing the floating gate material layer and the tunneling oxide material layer until the top surface of the initial isolation structure is exposed, and forming a tunneling oxide layer and a floating gate layer located on the tunneling oxide layer in the second groove.
11. The method for forming a semiconductor structure according to claim 10, wherein: The process of removing the protection layer includes a wet etching process.
12. The method for forming a semiconductor structure according to claim 1, wherein: Also includes: A control gate structure is formed on the top surface and sidewall surface of the floating gate structure, and the control gate structure spans the floating gate structure; the control gate structure includes a gate dielectric layer and a control gate layer located on the gate dielectric layer.
13. The method for forming a semiconductor structure according to claim 12, wherein: The method for forming a control gate structure comprises: after forming a floating gate structure, removing an initial isolation structure on a side wall of the floating gate structure to expose the side wall surface and the top surface of the floating gate structure and to form an isolation structure located in an isolation groove; forming a gate dielectric layer on the side wall surface and the top surface of the floating gate structure and the top surface of the isolation structure; forming a control gate layer on the gate dielectric layer, wherein the control gate layer is parallel to a second direction, the second direction is parallel to a substrate surface, and the second direction is perpendicular to the first direction.