Switching device based on chalcogenide and storage device thereof
A sulfur compound-based switching device and storage device enable high-density and three-dimensional storage by utilizing instantaneous resistance transitions, addressing bandwidth and scalability issues in existing technologies with low power consumption and fast operation speed.
Patent Information
- Application Number
- CN202411035002.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-31
- Publication Date
- 2024-12-03
AI Technical Summary
Existing storage technologies face limitations in bandwidth, latency, and scalability, necessitating new solutions for high-density and three-dimensional storage that are compatible with CMOS processes and have low power consumption and fast operation speed, which self-switching memory (SSM) is regarded as an effective solution for CXL-based systems, and can be further miniaturized to meet the needs of high-density storage.
A switching device and storage device based on sulfur compounds, with a chemical formula (S x Se y Te 100-x-y ) 100-z M z, where M is Sb, Sn, Si, Ge, Bi, Pb, In, Ga, As, C, P, or N, and x, y, z satisfy specific ranges, featuring a lower and upper electrode layer with a sulfur compound material layer in between, capable of instantaneous resistance transitions under an external electric field.
The device achieves low power consumption, fast operation speed, and low leakage current, enabling high-density and three-dimensional storage with improved yield, performance consistency, and reliability, compatible with CMOS technology.
Smart Images

Figure CN119072219A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of micro-nano electronic technology, and in particular relates to a switching device based on a class of sulfur compounds and a storage device thereof. Background Art
[0002] The data throughput in the era of big data and artificial intelligence has increased dramatically, and the introduction of Compute Express Link (CXL) interconnection is needed to solve the limitations of information storage in terms of bandwidth, latency and scalability. CXL-based systems urgently need new storage technologies to fill the blank architecture between the computing system main memory dynamic random access memory (DRAM) and the system storage medium NAND flash memory in traditional high-performance computing systems. Among the many new memories, self-switching memory (SSM) is regarded as an effective solution for CXL storage technology due to its high density, fast operation speed, long life and low power consumption. Unlike traditional memories that require additional switching units, self-switching memory allows bidirectional threshold switches (OTS) to perform switching and storage operations at the same time. Since no additional switches are required, the aspect ratio of self-switching memory can be further miniaturized to meet the needs of high-density storage. It is a new storage device that is highly anticipated. Summary of the invention
[0003] The technical problem to be solved by the present invention is to provide a switching device and a storage device based on a class of sulfur compounds. The switching device and the storage device have extremely low power consumption, fast operation speed, low leakage current, and the preparation method is compatible with CMOS process, and can be used for the manufacture of high-density and three-dimensional massive storage.
[0004] The present invention provides a switching device based on a class of sulfur compounds, wherein the chemical formula of the sulfur compounds is (S x Se y Te 100-x-y ) 100-z M z , where M is one or more of Sb, Sn, Si, Ge, Bi, Pb, In, Ga, As, C, P, and N, and x, y, and z satisfy 0≤x≤100, 0≤y≤100, and 10≤z≤90.
[0005] Furthermore, the switch device comprises:
[0006] Lower electrode layer;
[0007] upper electrode layer;
[0008] Sulfur compound material layer: located between the lower electrode layer and the upper electrode layer.
[0009] Furthermore, the thickness of the sulfur-based compound material layer is 5 nm to 50 nm.
[0010] Furthermore, the material of the lower electrode layer includes one or more of C, Ta, TiN, TaC, TaN, Co, W, Pt, Au, Ti, Al, Ag, Cu, and Ni.
[0011] Furthermore, the material of the upper electrode layer is one or more of C, Ta, TiN, TaC, TaN, Co, W, Pt, Au, Ti, Al, Ag, Cu, and Ni.
[0012] Furthermore, the switch device realizes an instantaneous transition from a high-resistance state to a low-resistance state under the action of an external electric field, and realizes an instantaneous transition from a low-resistance state to a high-resistance state when the external electric field is removed.
[0013] The present invention also provides a method for preparing a switching device based on a class of sulfur compounds, comprising the following steps:
[0014] S1: forming a lower electrode layer;
[0015] S2: forming a sulfur compound material layer on the lower electrode layer, wherein the sulfur compound has a chemical formula of (S x Se y Te 100-x-y ) 100-z M z , where M is one or more of Sb, Sn, Si, Ge, Bi, Pb, In, Ga, As, C, P, and N, and x, y, and z satisfy 0≤x≤100, 0≤y≤100, and 10≤z≤90;
[0016] S3: forming an upper electrode layer on the chalcogenide compound material layer;
[0017] S4: forming a lead-out electrode on the upper electrode layer.
[0018] Furthermore, the method of forming the sulfide compound material layer on the lower electrode layer includes: sputtering, chemical vapor deposition, atomic layer deposition or electron beam evaporation.
[0019] The present invention also provides a storage device, comprising a storage unit, wherein the storage unit comprises the switching device.
[0020] Furthermore, the turn-on current is greater than or equal to 10 -7 A, the switching ratio is greater than or equal to 2, the threshold voltage is less than or equal to 10V, the maximum number of cycles is greater than or equal to 100 times, and the threshold voltage window is greater than or equal to 0.2V after the polarity of the applied voltage is changed.
[0021] Beneficial Effects
[0022] The switch device of the present invention can realize instantaneous conversion from high resistance state to low resistance state when the voltage reaches the threshold voltage under the action of an external electric field; when the external energy is removed, it can immediately change from low resistance state to high resistance state. At the same time, for the switch device prepared based on the sulfur-based compound provided by the present invention, after the direction of the applied voltage is changed, the threshold voltage required for the first opening will be significantly higher than the threshold voltage required for subsequent opening. By changing the direction of the voltage, pulses with unchanged direction and size can read high resistance state and low resistance state information respectively, and a new storage device can be prepared using this principle. The switch device and storage device prepared based on this type of sulfur-based compound have extremely low power consumption, fast operation speed, and low leakage current, and the preparation method of the switch unit and storage device of the present invention is compatible with the CMOS process. The reduction of material leakage current helps the processing technology of the memory to continue to shrink with the CMOS technology node, which is beneficial to the processing of the device, while improving the yield rate, performance consistency and reliability of the storage array, greatly helping the manufacture of high-density and three-dimensional massive storage. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1 A schematic diagram of an IV characteristic curve of a sulfur-based compound storage device provided in Example 1;
[0024] Figure 2 The fatigue characteristic diagram of the sulfur compound storage device provided in Example 1;
[0025] Figure 3 A schematic diagram of an IV characteristic curve of a sulfur-based compound storage device provided in Example 2;
[0026] Figure 4 This is a fatigue characteristic diagram of the sulfur-based compound storage device provided in Example 2. DETAILED DESCRIPTION
[0027] The present invention will be further described below in conjunction with specific embodiments. It should be understood that these embodiments are only used to illustrate the present invention and are not intended to limit the scope of the present invention. In addition, it should be understood that after reading the content taught by the present invention, those skilled in the art can make various changes or modifications to the present invention, and these equivalent forms fall within the scope limited by the appended claims of the application equally.
[0028] The following is a description of a class of sulfur compounds provided by the present invention, wherein the general chemical formula of the sulfur compounds is (S x Se y Te 100-x-y ) 100-z M z, wherein M is one or more of Sb, Sn, Si, Ge, Bi, Pb, In, Ga, As, C, P, and N, and x, y, and z satisfy 0≤x≤100, 0≤y≤100, and 10≤z≤90;
[0029] In an embodiment, the sulfur-based compound may be a bidirectional threshold switch type switch material.
[0030] In the embodiment, the sulfur-based compound can realize an instantaneous transition from a high resistance state to a low resistance state under the action of an external electric field, and realize an instantaneous transition from a low resistance state to a high resistance state when the external electric field is removed.
[0031] In an embodiment, the on / off current ratio of the sulfur-based compound may be greater than or equal to 2.
[0032] Preferably, the on / off current ratio of the sulfur-based compound may be greater than or equal to 3.
[0033] Preferably, the on / off current ratio of the sulfur-based compound may be greater than or equal to 2 and less than or equal to 10.
[0034] Preferably, the on / off current ratio of the sulfur-based compound may be greater than or equal to 3 and less than or equal to 9.
[0035] In an embodiment, the thickness of the sulfur-based compound is 5 nm to 50 nm.
[0036] In an embodiment, the sulfur-based compound can be synthesized by methods including but not limited to sputtering, chemical vapor deposition, atomic layer deposition or electron beam evaporation.
[0037] In the embodiment, the sulfur-based compound can be synthesized by a single target co-sputtering method or an alloy target sputtering method.
[0038] In one embodiment, the chalcogenide compound material can be synthesized from a Bi2Se3 target and a GeSe target by co-sputtering.
[0039] Thus, the present invention provides (S x Se y Te 100-x-y ) 100-z M z Sulfur-based compound materials can overcome the disadvantage that PCM storage cells require additional series switching units, and can exhibit excellent comprehensive performance by adjusting the content of the doping element M.
[0040] The switch unit provided by the present invention is introduced below, and the switch unit includes:
[0041] Lower electrode layer;
[0042] upper electrode layer;
[0043] Sulfur-based compound material layer: located between the lower electrode layer and the upper electrode layer, and includes the sulfur-based compound material mentioned above.
[0044] In the embodiment, preferably, the thickness of the sulfide compound material layer may be 5 nm to 50 nm.
[0045] In the embodiment, preferably, the thickness of the upper electrode layer may be 5 nm to 50 nm.
[0046] In the embodiment, preferably, the thickness of the lower electrode layer may be 5 nm to 50 nm.
[0047] In an embodiment, the material of the upper electrode layer may be one or more of C, Ta, TiN, TaC, TaN, Co, W, Pt, Au, Ti, Al, Ag, Cu and Ni.
[0048] In an embodiment, the material of the lower electrode layer may be one or more of C, Ta, TiN, TaC, TaN, Co, W, Pt, Au, Ti, Al, Ag, Cu and Ni.
[0049] In the embodiment, the turn-on current I on Can be greater than or equal to 10 -7 A; the threshold voltage V of the switch unit th can be less than or equal to 10V; the leakage current I of the switch unit off ≤10 -7 A; The maximum number of cycles of the switch unit can be greater than or equal to 10 4 times; the switching ratio of the switching unit may be greater than or equal to 2.
[0050] Preferably, the turn-on current I of the switch unit on ≥10 -6 A; leakage current I of the switch unit off ≤10 -7 A; the threshold voltage V of the switch unit th ≤5V; the maximum number of cycles of the switching unit can be greater than or equal to 10 5 times; the switching ratio of the switching unit may be greater than or equal to 3.
[0051] Preferably, the turn-on current I of the switch unit on ≥10 -3 A, the switching ratio of the switch unit may be greater than or equal to 5, and the leakage current I off ≤10 -9 A.
[0052] Preferably, the threshold voltage V thIt can be 1V, 2V, 3V, 4V, 5V, 6V, 7V, 8V or 9V.
[0053] Preferably, the switching ratio of the switching unit may be greater than or equal to 3 and less than or equal to 9.
[0054] Preferably, the selectable number of the switch units can be 4, 5, 6, 7 or 8.
[0055] The following describes a method for preparing a switch unit based on a sulfur compound provided by the present invention, comprising the following steps:
[0056] S1: forming the lower electrode layer;
[0057] S2: forming the sulfur compound material layer on the lower electrode layer, wherein the sulfur compound has the general chemical formula (S x Se y Te 100-x-y ) 100-z M z , where M is one or more of Sb, Sn, Si, Ge, Bi, Pb, In, Ga, As, C, P, and N, and x, y, and z satisfy 0≤x≤100, 0≤y≤100, and 10≤z≤90;
[0058] S3: forming the upper electrode layer on the material layer;
[0059] S4: forming the lead-out electrode on the upper electrode layer.
[0060] In the embodiment, the shapes of the switch unit and the storage device include but are not limited to a columnar structure or a strip structure having a lower electrode layer / sulfur compound material layer / upper electrode layer. The present invention does not limit the shapes of the switch unit and the storage device.
[0061] In an embodiment, the material of the lower electrode layer may be one or more of C, Ta, TiN, TaC, TaN, Co, W, Pt, Au, Ti, Al, Ag, Cu and Ni; the material of the upper electrode layer may be one or more of C, Ta, TiN, TaC, TaN, Co, W, Pt, Au, Ti, Al, Ag, Cu and Ni.
[0062] In the embodiment, preferably, the thickness of the sulfide compound material layer may be 5 nm to 50 nm.
[0063] Preferably, the thickness of the sulfide compound material layer may be 10 nm, 15 nm, 20 nm, 25 nm, 30 nm, 35 nm, 40 nm or 45 nm, etc.
[0064] In the embodiment, preferably, the diameter of the lower electrode layer may be 5 to 200 nm.
[0065] In the embodiment, preferably, the diameter of the upper electrode layer may be 5 to 200 nm.
[0066] In an embodiment, the deposition of a sulfur-based compound material layer thin film on the surface of the lower electrode layer may include but is not limited to: deposition of a sulfur-based compound material layer thin film on the surface of the lower electrode layer by sputtering, chemical vapor deposition, atomic layer deposition or electron beam evaporation.
[0067] Preferably, the sputtering method may be a magnetron sputtering method.
[0068] In an embodiment, depositing the sulfide compound material layer thin film on the surface of the lower electrode layer may include: depositing the sulfide compound material layer thin film on the surface of the lower electrode layer using a single target co-sputtering method or an alloy target sputtering method.
[0069] In one embodiment, a Bi2Se3 target material or a GeSe target material may be used to deposit the chalcogenide compound material layer thin film by a single target co-sputtering method.
[0070] In another embodiment, an In target material and a GeSe target material may be used to deposit the chalcogenide compound material layer thin film by a single-target co-sputtering method.
[0071] In an embodiment, the preparation method of the upper electrode layer and the lower electrode layer may include but is not limited to physical vapor deposition, chemical vapor deposition, electron beam evaporation and molecular beam epitaxy.
[0072] Furthermore, the methods that can be used to form the upper electrode layer on the upper surface of the sulfur-based compound material layer include but are not limited to sputtering, evaporation, chemical vapor deposition (CVD), plasma enhanced chemical vapor deposition (PECVD), low pressure chemical vapor deposition (LPCVD), metal compound vapor deposition (MOCVD), molecular beam epitaxy (MBE), atomic vapor deposition (AVD) or atomic layer deposition (ALD), etc.
[0073] Furthermore, methods that may be used to form the lower electrode layer on the substrate include, but are not limited to, sputtering, evaporation, CVD, PECVD, LPCVD, MOCVD, MBE, AVD or ALD.
[0074] The present invention also provides a storage device, comprising a storage unit, wherein the storage unit comprises the switching device.
[0075] Example 1
[0076] This embodiment provides a method for preparing a switch unit and a storage device based on a type of sulfur-based compound, comprising the following steps:
[0077] S1: forming the lower electrode layer. The lower electrode layer can be prepared by any one of sputtering, evaporation, chemical vapor deposition (CVD), plasma enhanced chemical vapor deposition (PECVD), low pressure chemical vapor deposition (LPCVD), metal compound vapor deposition (MOCVD), molecular beam epitaxy (MBE), atomic vapor deposition (AVD) or atomic layer deposition (ALD). In this embodiment, magnetron sputtering is preferably used to prepare the lower electrode layer. The material of the lower electrode layer may include any one of W, Pt, Au, Ti, Al, Ag, Cu and Ni, or an alloy material composed of any two or more of the above single metal materials W, Pt, Au, Ti, Al, Ag, Cu and Ni, or a nitride or oxide containing one of the above single metal materials W, Pt, Au, Ti, Al, Ag, Cu and Ni. In this embodiment, the material of the lower electrode layer is preferably TiN. The diameter of the electrode of the TiN lower electrode layer made by magnetron sputtering is one of 60nm, 120nm, 150nm, and 200nm, and the height is 200nm.
[0078] S2: Using magnetron sputtering, select Bi2Se3 target material and GeSe target material for co-sputtering, and deposit a 20nm thick sulfur compound material layer film on the lower electrode layer. The chemical formula of the sulfur compound material is Ge 30 Bi 10 Se 60 ;
[0079] S3: forming the upper electrode layer on the sulfur compound material layer. On the sulfur compound material layer, the upper electrode layer can be prepared by any one of sputtering, evaporation, chemical vapor deposition, plasma enhanced chemical vapor deposition, low pressure chemical vapor deposition, metal compound vapor deposition (MOCVD), molecular beam epitaxy, atomic vapor deposition or atomic layer deposition. The material of the upper electrode layer may, for example, include any one of the single metal materials W, Pt, Au, Ti, Al, Ag, Cu and Ni, or an alloy material composed of any two or more of the above single metal materials W, Pt, Au, Ti, Al, Ag, Cu and Ni, or a nitride or oxide containing one of the above single metal materials W, Pt, Au, Ti, Al, Ag, Cu and Ni.
[0080] S4: preparing a lead-out electrode on the upper electrode layer, for example, the lead-out electrode can be prepared by any one of sputtering, evaporation, chemical vapor deposition, plasma enhanced chemical vapor deposition, low pressure chemical vapor deposition, metal compound vapor deposition, molecular beam epitaxy, atomic vapor deposition or atomic layer deposition. In this way, the upper and lower electrode layers can be integrated with other components in the storage device such as storage cells, drive circuits and peripheral circuits through the lead-out electrode, thereby preparing a complete storage device, and the processing method used is a conventional semiconductor process.
[0081] As an example, the material of the lead-out electrode may include any one of the single metal materials W, Pt, Au, Ti, Al, Ag, Cu and Ni, or an alloy material composed of any two or more of the above single metal materials W, Pt, Au, Ti, Al, Ag, Cu and Ni, or a nitride or oxide containing one of the above single metal materials W, Pt, Au, Ti, Al, Ag, Cu and Ni.
[0082] In this embodiment, preferably, the lead-out electrode is prepared by magnetron sputtering, the material is Al, and the film thickness of the prepared lead-out electrode is 200 nm.
[0083] The voltage-current curve of the storage device obtained by electrical testing is as follows: Figure 1 As shown by Figure 1 It can be seen that after the polarity of the operating voltage of the storage device in this embodiment is changed, when the voltage applied to the storage device is less than about 2V, the storage device is in a high-resistance state; when the voltage applied to the storage device exceeds the high-state threshold voltage (about 3V), the storage device is instantly turned on and becomes a low-resistance state, and the current passing through the storage device increases sharply to 10 -3 A: When the voltage applied to the storage device is removed, the storage device returns to the high impedance state instantly, and the current passing through the storage device decreases sharply. Figure 2 It can be seen that the storage device can be stably cycled for more than 10 times.
[0084] It should be noted that the chalcogenide compound material layer can be formed by, but is not limited to, magnetron sputtering.
[0085] It should be noted that the thickness of the sulfur-based compound material layer can be set according to actual needs. Preferably, the thickness of the material layer can be 5 nm to 50 nm. More preferably, in this embodiment, the thickness of the material layer is 20 nm.
[0086] It should be noted that the upper electrode material may include but is not limited to one or more of C, Ta, TiN, TaC, TaN, Co, W, Pt, Au, Ti, Al, Ag, Cu and Ni. The lower electrode material may include but is not limited to one or more of C, Ta, TiN, TaC, TaN, Co, W, Pt, Au, Ti, Al, Ag, Cu and Ni.
[0087] In this embodiment, the turn-on current I on ≥10 -4 A, the switching ratio of the storage device is greater than or equal to 3, and the leakage current I off ≤10 -7 A, the voltage window ΔV of the storage device th ≤0.5V, the device can stably cycle more than 10 times.
[0088] Example 2
[0089] This embodiment provides a method for preparing a switch unit and a storage device based on a type of sulfur-based compound, comprising the following steps:
[0090] S1: forming the lower electrode layer. The lower electrode layer can be prepared by any one of sputtering, evaporation, chemical vapor deposition (CVD), plasma enhanced chemical vapor deposition (PECVD), low pressure chemical vapor deposition (LPCVD), metal compound vapor deposition (MOCVD), molecular beam epitaxy (MBE), atomic vapor deposition (AVD) or atomic layer deposition (ALD). In this embodiment, magnetron sputtering is preferably used to prepare the lower electrode layer. The material of the lower electrode layer may include any one of W, Pt, Au, Ti, Al, Ag, Cu and Ni, or an alloy material composed of any two or more of the above single metal materials W, Pt, Au, Ti, Al, Ag, Cu and Ni, or a nitride or oxide containing one of the above single metal materials W, Pt, Au, Ti, Al, Ag, Cu and Ni. In this embodiment, the material of the lower electrode layer is preferably TiN. The diameter of the electrode of the TiN lower electrode layer made by magnetron sputtering is one of 60nm, 120nm, 150nm, and 200nm, and the height is 200nm.
[0091] S2: Using magnetron sputtering, select In target material and GeSe target material for co-sputtering, and deposit a 20nm thick sulfur compound material layer film on the lower electrode layer. The chemical formula of the sulfur compound material is In 30 Ge 10 Se 60 ;
[0092] S3: forming the upper electrode layer on the sulfur compound material layer. On the sulfur compound material layer, the upper electrode layer can be prepared by any one of sputtering, evaporation, chemical vapor deposition, plasma enhanced chemical vapor deposition, low pressure chemical vapor deposition, metal compound vapor deposition (MOCVD), molecular beam epitaxy, atomic vapor deposition or atomic layer deposition. The material of the upper electrode layer may, for example, include any one of the single metal materials W, Pt, Au, Ti, Al, Ag, Cu and Ni, or an alloy material composed of any two or more of the above single metal materials W, Pt, Au, Ti, Al, Ag, Cu and Ni, or a nitride or oxide containing one of the above single metal materials W, Pt, Au, Ti, Al, Ag, Cu and Ni.
[0093] S4: preparing a lead-out electrode on the upper electrode layer, for example, the lead-out electrode can be prepared by any one of sputtering, evaporation, chemical vapor deposition, plasma enhanced chemical vapor deposition, low pressure chemical vapor deposition, metal compound vapor deposition, molecular beam epitaxy, atomic vapor deposition or atomic layer deposition. In this way, the upper and lower electrode layers can be integrated with other components in the storage device such as storage cells, drive circuits and peripheral circuits through the lead-out electrode, thereby preparing a complete storage device, and the processing method used is a conventional semiconductor process.
[0094] As an example, the material of the lead-out electrode may include any one of the single metal materials W, Pt, Au, Ti, Al, Ag, Cu and Ni, or an alloy material composed of any two or more of the above single metal materials W, Pt, Au, Ti, Al, Ag, Cu and Ni, or a nitride or oxide containing one of the above single metal materials W, Pt, Au, Ti, Al, Ag, Cu and Ni.
[0095] In this embodiment, preferably, the lead-out electrode 5 is prepared by magnetron sputtering, the material is Al, and the film thickness of the prepared lead-out electrode is 200 nm.
[0096] The voltage-current curve of the storage device obtained by electrical testing is as follows: Figure 3 As shown by Figure 3 It can be seen that after the polarity of the operating voltage of the storage device in this embodiment is changed, when the voltage applied to the storage device is less than about 1.5V, the storage device is in a high-resistance state; when the voltage applied to the storage device exceeds the high-state threshold voltage (about 2V), the storage device is instantly turned on and becomes a low-resistance state, and the current passing through the storage device increases sharply to 10 -3A: When the voltage applied to the storage device is removed, the storage device returns to the high impedance state instantly, and the current passing through the storage device decreases sharply. Figure 4 It can be seen that the storage device can be stably cycled for more than 10 times.
[0097] It should be noted that the chalcogenide compound material layer can be formed by, but is not limited to, magnetron sputtering.
[0098] It should be noted that the thickness of the sulfur-based compound material layer can be set according to actual needs. Preferably, the thickness of the material layer can be 5 nm to 50 nm. More preferably, in this embodiment, the thickness of the material layer is 20 nm.
[0099] It should be noted that the upper electrode material may include but is not limited to one or more of C, Ta, TiN, TaC, TaN, Co, W, Pt, Au, Ti, Al, Ag, Cu and Ni. The lower electrode material may include but is not limited to one or more of C, Ta, TiN, TaC, TaN, Co, W, Pt, Au, Ti, Al, Ag, Cu and Ni.
[0100] In this embodiment, the turn-on current I on ≥10 -4 A, the switching ratio of the storage device is greater than or equal to 3, and the leakage current I off ≤10 -7 A, the voltage window ΔV of the storage device th ≤0.5V, the device can stably cycle more than 10 times.
[0101] In summary, the sulfur compounds applied to the storage device in the present invention are brand-new components. The switching device prepared based on the sulfur compounds provided by the present invention can realize instantaneous conversion from high-resistance state to low-resistance state when the voltage reaches the threshold voltage under the action of an external electric field; when the external energy is removed, it can immediately change from the low-resistance state to the high-resistance state. At the same time, for the switching device prepared based on the sulfur compounds provided by the present invention, after the direction of the applied voltage is changed, the threshold voltage required for the first opening will be significantly higher than the threshold voltage required for subsequent openings. By changing the direction of the voltage, pulses with unchanged direction and size can read high-resistance state and low-resistance state information respectively, and a brand-new storage device can be prepared using this principle. The switching devices and storage devices prepared based on this type of sulfur compounds have extremely low power consumption, fast operating speed, low leakage current, and high integration density, and can be used for the manufacture of high-density and three-dimensional massive storage devices.
[0102] The above description has fully disclosed the specific embodiments of the present invention. It should be pointed out that any changes made by those skilled in the art to the specific embodiments of the present invention do not deviate from the scope of the claims of the present invention. Accordingly, the scope of the claims of the present invention is not limited to the above specific embodiments.
Claims
1. A switching device based on a class of sulfur compounds, characterized in that: The general chemical formula of the sulfur compound is (S x Se y Te 100-x-y ) 100-z M z , where M is one or more of Sb, Sn, Si, Ge, Bi, Pb, In, Ga, As, C, P, and N, and x, y, and z satisfy 0≤x≤100, 0≤y≤100, and 10≤z≤90.
2. The switch device according to claim 1, characterized in that: The switch device comprises: Lower electrode layer; upper electrode layer; Sulfur compound material layer: located between the lower electrode layer and the upper electrode layer.
3. The switch device according to claim 2, characterized in that: The thickness of the sulfur compound material layer is 5nm to 50nm.
4. The switch device according to claim 2, characterized in that: The material of the lower electrode layer includes one or more of C, Ta, TiN, TaC, TaN, Co, W, Pt, Au, Ti, Al, Ag, Cu, and Ni.
5. The switch device according to claim 2, characterized in that: The material of the upper electrode layer is one or more of C, Ta, TiN, TaC, TaN, Co, W, Pt, Au, Ti, Al, Ag, Cu, and Ni.
6. The switch device according to claim 1, characterized in that: The switch device realizes instantaneous transition from a high resistance state to a low resistance state under the action of an external electric field, and realizes instantaneous transition from a low resistance state to a high resistance state when the external electric field is removed.
7. A method for preparing a switching device based on a class of sulfur compounds, comprising the following steps: S1: forming a lower electrode layer; S2: forming a sulfur compound material layer on the lower electrode layer, wherein the sulfur compound has a chemical formula of (S x Se y Te 100-x-y ) 100-z M z , where M is one or more of Sb, Sn, Si, Ge, Bi, Pb, In, Ga, As, C, P, and N, and x, y, and z satisfy 0≤x≤100, 0≤y≤100, and 10≤z≤90; S3: forming an upper electrode layer on the chalcogenide compound material layer; S4: forming a lead-out electrode on the upper electrode layer.
8. The preparation method according to claim 6, characterized in that: The method of forming the sulfide compound material layer on the lower electrode layer includes: sputtering, chemical vapor deposition, atomic layer deposition or electron beam evaporation.
9. A storage device, characterized in that: A memory cell is included, the memory cell comprising the switching device according to claim 1.
10. A switching device according to claim 1 or a storage device according to claim 8, characterized in that: Opening current is greater than or equal to 10 -7 A, the switching ratio is greater than or equal to 2, the threshold voltage is less than or equal to 10V, the maximum number of cycles is greater than or equal to 100 times, and the threshold voltage window is greater than or equal to 0.2V after the polarity of the applied voltage is changed.