Itaconylated carboxymethyl chitosan derivative as well as preparation method and application thereof

CN119072498APending Publication Date: 2024-12-03IMEIK TECH DEV CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202480001978.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2023-03-30
Filing Date
2024-03-25
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

The existing methods of double-bond modification of carboxymethyl chitosan suffer from the sensitization and poor biocompatibility of methacrylic acid, the temperature sensitivity of hydroxybutyl chitosan, and the skin irritation of ammonium persulfate. problems, resulting in long reaction times, long purification times, and insufficient safety.

Method used

Use itaconic acid or itaconic anhydride as a modifier, and use an alkaline reagent to form an amide bond with carboxymethyl chitosan to perform a homogeneous reaction. Adjust the reaction temperature, time and pH value to increase the double bond rate.

Benefits of technology

It achieves efficient double bond modification under mild conditions, improves the double bond rate and safety of carboxymethyl chitosan, enhances its moisturizing performance and mechanical properties, and is suitable for beauty and medical applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119072498A_ABST
    Figure CN119072498A_ABST
Patent Text Reader

Abstract

The invention provides an itaconylated carboxymethyl chitosan derivative as well as a preparation method and application thereof. The itaconic acylated carboxymethyl chitosan derivative is obtained by grafting itaconic acid or itaconic anhydride and carboxymethyl chitosan, and on the premise of introducing an alkaline reagent, the itaconic acid or itaconic anhydride reacts with amino on the carboxymethyl chitosan to form an amido bond. The invention provides two preparation methods of itaconic acylated carboxymethyl chitosan derivatives, one method takes itaconic anhydride as a modifier, the itaconic anhydride is subjected to ring opening to form itaconic acid, and the itaconic acid is grafted on carboxymethyl chitosan to complete double-bond modification, and the other method takes itaconic acid as a modifier, an activator is added, and the itaconic acylated carboxymethyl chitosan derivatives are obtained. Itaconic acid is grafted on carboxymethyl chitosan through a condensation reaction to complete double-bond modification. The preparation method provided by the invention has the advantages of high grafting rate, simplicity, mild reaction conditions, no need of heating, short reaction time and simple post-treatment, and is suitable for amplification and industrial application.
Need to check novelty before this filing date? Find Prior Art

Description

An itaconylated carboxymethyl chitosan derivative and its preparation method and application Technical Field

[0001] The present invention belongs to the technical field of biomedical materials, and in particular relates to an itaconylated carboxymethyl chitosan derivative, a preparation method and an application thereof. Background Art

[0002] Carboxymethyl chitosan (CMC) is obtained by etherifying chitosan with chloroacetic acid, overcoming chitosan's poor water solubility. After the etherification reaction, -CH2COOH groups are attached to the chitosan. Depending on the site of substitution, carboxymethyl chitosan can be divided into N-carboxymethyl chitosan (N-CMC), O-carboxymethyl chitosan (O-CMC), N,O-carboxymethyl chitosan (N,O-CMC), and N,N-carboxymethyl chitosan (N,N-CMC). Carboxymethyl chitosan is a natural polysaccharide derivative with excellent properties such as good water solubility, antibacterial properties, enhanced permeability, adhesion, biocompatibility, and degradability. Carboxymethyl chitosan possesses two chemical groups, carboxyl and amino, which serve as reactive sites for binding to other molecules to modify the carboxymethyl chitosan.

[0003] Currently, existing methods for modifying carboxymethyl chitosan with double bonds primarily involve grafting carboxymethyl chitosan with methacrylic acid and its derivatives. This chemical modification introduces crosslinkable double bonds into the polymer chain, creating crosslinkable sites. However, acrylic acid, produced during the metabolism of methacrylic acid, is highly irritating and sensitizing, and is listed on the Class III carcinogen list. Furthermore, acrylic acid can only be obtained from petroleum-based feedstocks, resulting in poor biocompatibility.

[0004] Patent document CN112341552A discloses a preparation method of itaconic acid grafted onto hydroxybutyl chitosan. However, since hydroxybutyl chitosan is sensitive to temperature, it forms micelles when dissolved in water at low temperatures. When the temperature rises, the micelles aggregate to form a gel or precipitate, resulting in more hydrophobic groups in hydroxybutyl chitosan, which makes the water retention of hydroxybutyl chitosan poor. In addition, due to the large steric hindrance of hydroxybutyl chitosan, it is difficult to undergo condensation reaction with the conjugated double bonds in itaconic acid, resulting in a long reaction time for double bond modification of hydroxybutyl chitosan and a long subsequent purification time.

[0005] Patent document CN106832129A discloses a method for preparing itaconic acid homopolymer-grafted carboxymethyl chitosan nanoparticles. The method involves first grafting itaconic acid onto carboxymethyl chitosan in the form of a homopolymer to prepare the itaconic acid homopolymer-grafted carboxymethyl chitosan. The itaconic acid homopolymer-grafted carboxymethyl chitosan is then subjected to pH adjustment to allow the itaconic acid homopolymer-grafted carboxymethyl chitosan to undergo intramolecular and intermolecular self-crosslinking to prepare nanoparticles. However, ammonium persulfate is added to this method, which is irritating and corrosive to the skin and mucous membranes. Long-term skin contact may cause allergic dermatitis.

[0006] In order to solve the defects and problems of the above-mentioned prior art, the present application provides a method for double-bonding modification of carboxymethyl chitosan using itaconic acid or itaconic anhydride as a modifier. The method is simple, has a high double-bonding rate, and is highly safe.

[0007] Summary of the Invention

[0008] The present invention provides an itaconylated carboxymethyl chitosan derivative and a method for preparing the same. The present invention utilizes itaconic acid or itaconic anhydride as a modifier and, by adding an alkaline agent, grafts itaconic acid or itaconic acid obtained by ring-opening itaconic anhydride onto carboxymethyl chitosan to form an itaconylated carboxymethyl chitosan derivative, thereby achieving double-bonding modification. The preparation method of the present invention enables the grafting of itaconic acid or itaconic acid obtained by ring-opening itaconic anhydride onto carboxymethyl chitosan under relatively mild conditions through a homogeneous reaction, and by adjusting the reaction temperature, reaction time, pH value of the reaction system, and activating agent, thereby achieving double-bonding modification of the carboxymethyl chitosan and achieving a high double-bonding rate (grafting rate).

[0009] The technical solutions provided by the present invention are as follows:

[0010] In the first aspect of the present invention, an itaconic acid-modified carboxymethyl chitosan derivative is provided, which uses itaconic acid or itaconic anhydride as a modifier, and by introducing an alkaline reagent, the itaconic acid or itaconic anhydride forms an amide bond with the carboxymethyl chitosan for a grafting reaction to obtain the itaconic acid-modified carboxymethyl chitosan derivative, thereby completing the double bond modification.

[0011] Furthermore, the itaconylated carboxymethyl chitosan derivative has the following structure:

[0012] Wherein, n is a positive integer (its value is affected by factors such as the molecular weight and double bond rate of carboxymethyl chitosan).

[0013] In order to ensure that the amino group of the polysaccharide has sufficient reactivity, the carboxymethyl chitosan used in the present invention includes but is not limited to N-carboxymethyl chitosan, O-carboxymethyl chitosan, N,O-carboxymethyl chitosan and N,N-carboxymethyl chitosan, preferably O-carboxymethyl chitosan, and more preferably 6-O-carboxymethyl chitosan.

[0014] Furthermore, the molecular weight of the carboxymethyl chitosan can be arbitrary, for example, 1000-30000 Da (such as 1000, 2000, 3000, 4000, 5000, 6000, 7000, 8000, 9000, 10000, 12000, 14000, 16000, 18000, 20000, 22000, 24000, 26000, 28000, 30000 Da).

[0015] Furthermore, the dynamic viscosity of the carboxymethyl chitosan can be arbitrary, for example, 30-60 mPa·s (e.g., 30, 32, 34, 36, 38, 40, 42, 44, 46, 48, 50, 52, 54, 56, 58, 60 mPa·s).

[0016] Furthermore, the alkaline agent is selected from sodium hydroxide, potassium hydroxide, calcium hydroxide or barium hydroxide; preferably, the alkaline agent is sodium hydroxide.

[0017] Furthermore, the double bond rate (i.e., grafting rate) of the carboxymethyl chitosan is 70-100% (such as 70%, 72%, 75%, 78%, 80%, 82%, 85%, 88%, 90%, 91%, 92%, 93%, 94%, 95%, 96%, 97%, 98%, 99%, 100%); preferably, the double bond rate of the carboxymethyl chitosan is 90%-100%.

[0018] Furthermore, the itaconylated carboxymethyl chitosan derivative can be prepared by the methods described in the second and third aspects of the present invention.

[0019] The second aspect of the present invention provides a method for preparing an itaconic acid modified carboxymethyl chitosan derivative using itaconic anhydride as a modifier, comprising the following steps: under the protection of an inert gas, using a double-drop method, itaconic anhydride and an alkaline reagent are simultaneously added dropwise to a carboxymethyl chitosan solution, the pH value of the reaction system is adjusted to 6.5-9.0, and the reaction is stirred to obtain an itaconic acid modified carboxymethyl chitosan derivative.

[0020] In one embodiment of the present invention, the reaction process of the preparation method is shown in FIG1 .

[0021] Furthermore, the inert gas is nitrogen or helium.

[0022] Furthermore, the carboxymethyl chitosan is selected from N-carboxymethyl chitosan, O-carboxymethyl chitosan or N,O-carboxymethyl chitosan, preferably O-carboxymethyl chitosan, more preferably 6-O-carboxymethyl chitosan.

[0023] Furthermore, the solvent of the carboxymethyl chitosan is water; preferably deoxygenated water, wherein the deoxygenation method includes but is not limited to boiling and passing an inert gas (such as nitrogen). In order to ensure that itaconic anhydride does not open and deteriorate during the dropwise addition, the contact with oxygen during the dissolution of the carboxymethyl chitosan should be minimized.

[0024] Furthermore, the concentration of the carboxymethyl chitosan solution is 1-20 mg / ml (such as 1, 1.5, 2, 2.5, 3, 3.5, 4, 4.5, 5, 5.5, 6, 6.5, 7, 7.5, 8, 8.5, 9, 9.5, 10, 10.5, 11, 11.5, 12, 12.5, 13, 13.5, 14, 14.5, 15, 15.5, 16, 16.5, 17, 17.5, 18, 18.5, 19, 19.5, 20 mg / ml); preferably 5-20 mg / ml.

[0025] Those skilled in the art will appreciate that carboxymethyl chitosan of various molecular weights can be used in the present invention. For example, the molecular weight of the carboxymethyl chitosan is 1000-30000 Da (e.g., 1000, 2000, 3000, 4000, 5000, 6000, 7000, 8000, 9000, 10000, 12000, 14000, 16000, 18000, 20000, 22000, 24000, 26000, 28000, 30000 Da).

[0026] Furthermore, the dynamic viscosity of the carboxymethyl chitosan can be arbitrary, for example, 30-60 mPa·s (e.g., 30, 32, 34, 36, 38, 40, 42, 44, 46, 48, 50, 52, 54, 56, 58, 60 mPa·s).

[0027] Furthermore, the solvent of itaconic anhydride is selected from one or more of acetone, tetrahydrofuran, dioxane, and acetonitrile; preferably acetone.

[0028] Furthermore, the amount of itaconic anhydride added is 2-6 times (such as 2, 2.5, 3, 3.5, 4, 4.5, 5, 5.5, 6 times) the molar equivalent of the amino group in the carboxymethyl chitosan repeating unit; preferably 4 times.

[0029] Furthermore, the solvent of the alkaline reagent is water; preferably deoxygenated water, wherein the deoxygenation method includes but is not limited to boiling and passing an inert gas (such as nitrogen). To ensure that itaconic anhydride does not undergo ring opening and deterioration during the dropwise addition, the contact with oxygen during the dissolution of NaOH should be minimized.

[0030] Furthermore, the alkaline agent is selected from sodium hydroxide, potassium hydroxide, calcium hydroxide or barium hydroxide; preferably, the alkaline agent is sodium hydroxide.

[0031] Furthermore, the concentration of the alkaline reagent solution is 2-5 mol / L (such as 2, 3, 4, 5 mol / L).

[0032] Furthermore, in the double-drop method, in order to control the reaction process, the molar amount of the alkaline reagent hydroxide added per unit time is 1.5-2.5 times (e.g., 1.5, 1.8, 2, 2.2, 2.5 times) the molar amount of itaconic anhydride.

[0033] In the present invention, the alkaline reagent acts as an amino group activator in the system to activate the amino group, prevent the amino group from being protonated under relatively alkaline conditions, and ensure the reaction activity during the grafting of the amino group and itaconic anhydride. In addition, by adding the alkaline reagent, the pH value of the reaction system is adjusted to avoid precipitation of carboxymethyl chitosan dissolved in water when the pH value is too low, thereby further improving the reaction efficiency.

[0034] The present invention improves the double-bonding grafting efficiency by adjusting the timing of adding the alkaline reagent. Specifically, itaconic anhydride and the alkaline reagent are added dropwise at the same time by a double-drop method, and the addition amount of the two per unit time is controlled by the dropping speed, so that itaconic anhydride can be ring-opened and grafted with amino groups after being dropped into water. The alkaline reagent added dropwise can neutralize the pH reduction of the system caused by the ring opening of itaconic anhydride to avoid the precipitation of carboxymethyl chitosan; and can prevent the amino group from being protonated and activate the amino group during the dropping process, thereby ensuring the stability and activity of the system during the reaction to the greatest extent and improving the double-bonding grafting efficiency. If the alkaline reagent is added too early compared to itaconic anhydride, it is easy to cause the carboxyl group to undergo a neutralization reaction with the base after the ring opening of itaconic anhydride, thereby reducing the grafting efficiency; if the alkaline reagent is added too late, it is easy to cause the carboxymethyl chitosan to precipitate during the reaction, and the amino group activity is low, resulting in grafting difficulties.

[0035] Furthermore, the pH value of the reaction system is specifically 6.5, 6.8, 7.0, 7.2, 7.5, 7.8, 8.0, 8.2, 8.5, 8.8, 9.0; preferably 6.5-8.5, more preferably 7.5.

[0036] Furthermore, the reaction time is 3-12 h (such as 3, 4, 5, 6, 7, 8, 9, 10, 11, 12 h); preferably 4-5 h; more preferably 4 h.

[0037] Furthermore, the reaction temperature is 10-30°C (e.g., 10, 11, 12, 13, 14, 15, 16, 17, 18, 19, 20, 21, 22, 23, 24, 25, 26, 27, 28, 29, 30°C).

[0038] Furthermore, the preparation method further comprises a post-processing step, and the post-processing step comprises washing and drying.

[0039] Furthermore, the washing agent used is selected from one or more of 75% ethanol, 80% ethanol or 100% ethanol. The purpose of washing is to remove residual itaconic acid as much as possible, and the washing is carried out under stirring conditions.

[0040] Furthermore, the drying is carried out under vacuum conditions.

[0041] Furthermore, the drying temperature is 20-30° C. (e.g., 20, 21, 22, 23, 24, 25, 26, 27, 28, 29, 30° C.), preferably 30° C. The drying temperature should not be too high to prevent the grafted double bonds from being destroyed by high temperature.

[0042] Furthermore, the drying time is 18-28 hours (such as 18, 19, 20, 21, 22, 23, 24, 25, 26, 27, 28 hours); preferably 24-28 hours.

[0043] The third aspect of the present invention provides a method for preparing an itaconic acid-modified carboxymethyl chitosan derivative using itaconic acid as a modifier, comprising the following steps: adding an alkaline reagent to itaconic acid to adjust the pH value of the itaconic acid solution to 7.0-8.0, then adding the alkaline reagent to the carboxymethyl chitosan solution, and then adding an activator and a co-activator, stirring the reaction, and obtaining the itaconic acid-modified carboxymethyl chitosan derivative.

[0044] In one embodiment of the present invention, the reaction process of the preparation method is shown in FIG2 .

[0045] Furthermore, the carboxymethyl chitosan is selected from N-carboxymethyl chitosan, O-carboxymethyl chitosan or N,O-carboxymethyl chitosan, preferably O-carboxymethyl chitosan, more preferably 6-O-carboxymethyl chitosan.

[0046] Furthermore, the solvent of the carboxymethyl chitosan is water.

[0047] Furthermore, the concentration of the carboxymethyl chitosan solution is 1-10 mg / mL (such as 1, 1.5, 2, 2.5, 3, 3.5, 4, 4.5, 5, 5.5, 6, 6.5, 7, 7.5, 8, 8.5, 9, 9.5, 10 mg / ml); preferably 5-10 mg / mL.

[0048] Those skilled in the art will appreciate that carboxymethyl chitosan of various molecular weights can be used in the present invention. For example, the molecular weight of the carboxymethyl chitosan is 1000-30000 Da (e.g., 1000, 2000, 3000, 4000, 5000, 6000, 7000, 8000, 9000, 10000, 12000, 14000, 16000, 18000, 20000, 22000, 24000, 26000, 28000, 30000 Da).

[0049] Furthermore, the dynamic viscosity of the carboxymethyl chitosan can be arbitrary, for example, 30-60 mPa·s (e.g., 30, 32, 34, 36, 38, 40, 42, 44, 46, 48, 50, 52, 54, 56, 58, 60 mPa·s).

[0050] Furthermore, the solvent of the itaconic acid is water.

[0051] Furthermore, the amount of itaconic acid added is 5-30 times (e.g., 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 16, 17, 18, 19, 20, 21, 22, 23, 24, 25, 26, 27, 28, 29, 30 times) the molar equivalent of the amino group in the carboxymethyl chitosan repeating unit; preferably 10-20 times; more preferably 20 times. By controlling the amount of itaconic acid added, the self-crosslinking reaction of the carboxyl group in itaconic acid can be reduced, thereby improving the double-bond grafting modification efficiency.

[0052] Furthermore, the solvent of the alkaline reagent is water.

[0053] Furthermore, the alkaline agent is selected from sodium hydroxide, potassium hydroxide, calcium hydroxide or barium hydroxide; preferably, the alkaline agent is sodium hydroxide.

[0054] Furthermore, the concentration of the alkaline reagent solution is 3-8 mol / L (such as 3, 4, 5, 6, 7, 8 mol / L); preferably 5 mol / L.

[0055] Furthermore, the alkaline reagent adjusts the pH value of the itaconic acid solution to 7.0-8.0 (such as 7.0, 7.1, 7.2, 7.3, 7.4, 7.5, 7.6, 7.7, 7.8, 7.9, 8.0); preferably 7.5.

[0056] The present invention improves the double bond grafting efficiency by adjusting the timing of adding an alkaline reagent. Specifically, the pH value of an itaconic acid solution is adjusted to 7.0-8.0 using an alkaline reagent to form a buffer salt system of itaconic acid and sodium itaconate, which is then added to a carboxymethyl chitosan solution. The formed buffer salt system can, on the one hand, make the reaction conditions mild and avoid the occurrence of excessive acidity in the system. While COOH in itaconic acid continuously reacts with EDC, COOH generated by hydrolysis of sodium itaconate also reacts with EDC, thereby improving the activation efficiency of the carboxyl group activated by EDC. On the other hand, the reaction is carried out under weakly alkaline conditions, avoiding the precipitation of carboxymethyl chitosan, while activating the amino groups on the carboxymethyl chitosan and improving the modification efficiency.

[0057] Furthermore, the activator is a water-soluble carbodiimide, preferably one or more selected from 1-ethyl-3-(dimethylaminopropyl)carbodiimide (EDC), 1-(3-dimethylaminopropyl)-3-ethyl-carbodiimide, 1-cyclohexyl-3-(2-morpholinoethyl)carbodiimide, and 1,3-bis[di(methoxymethyl)methyl]carbodiimide; more preferably 1-ethyl-3-(dimethylaminopropyl)carbodiimide.

[0058] Furthermore, the co-activator is selected from one or more of N-hydroxysuccinimide (NHS), sulfonated N-hydroxysuccinimide, tert-butanol, and 1-hydroxybenzotriazole; preferably N-hydroxysuccinimide.

[0059] Furthermore, the amount of the activator added is 2-20 times (such as 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 16, 17, 18, 19, 20 times) the molar equivalent of the amino group in the carboxymethyl chitosan repeating unit; preferably 4-10 times; more preferably 8 times.

[0060] Furthermore, the amount of the co-activator is the same as that of the activator.

[0061] Furthermore, the reaction time is 4-20 h (such as 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 16, 17, 18, 19, 20 h); preferably 6-8 h; more preferably 6 h.

[0062] Furthermore, the reaction temperature is 10-30°C (e.g., 10, 11, 12, 13, 14, 15, 16, 17, 18, 19, 20, 21, 22, 23, 24, 25, 26, 27, 28, 29, 30°C).

[0063] Furthermore, the preparation method further comprises a post-processing step, and the post-processing step comprises washing and drying.

[0064] Furthermore, the washing agent used is selected from one or more of 75% ethanol, 80% ethanol or 100% ethanol. The purpose of washing is to remove residual itaconic acid as much as possible, and the washing is carried out under stirring conditions.

[0065] Furthermore, the drying is carried out under vacuum conditions.

[0066] Furthermore, the drying temperature is 20-30°C (such as 20, 21, 22, 23, 24, 25, 26, 27, 28, 29, 30°C); preferably 30°C.

[0067] Furthermore, the drying time is 18-28 hours (such as 18, 19, 20, 21, 22, 23, 24, 25, 26, 27, 28 hours); preferably 24-28 hours.

[0068] The fourth aspect of the present invention provides a method for detecting the grafting rate (double bond rate) of an itaconylated carboxymethyl chitosan derivative, the method comprising the following steps: dissolving the itaconylated carboxymethyl chitosan derivative in a deuterated reagent, and detecting the grafting rate by hydrogen nuclear magnetic resonance spectroscopy. The grafting rate is calculated as follows: Grafting rate m (%) = S 双键对应氢积分面积 / S 羧甲基壳聚糖糖环所含氢积分面积 ×100%

[0069] (Here S 羧甲基壳聚糖糖环所含氢积分面积 The number "11" refers to the total number of hydrogen atoms contained in each repeating unit of carboxymethyl chitosan after itaconic acid is grafted onto the repeating unit.

[0070] Furthermore, the deuterated reagent is deuterated water.

[0071] Furthermore, the concentration of the itaconylated carboxymethyl chitosan derivative solution is 10 mg / mL.

[0072] Furthermore, the number of nuclear magnetic resonance scans in the hydrogen nuclear magnetic resonance spectroscopy is 16-64 times.

[0073] The fifth aspect of the present invention provides the use of the itaconylated carboxymethyl chitosan derivative described in the first aspect or the itaconylated carboxymethyl chitosan derivative prepared by the preparation method described in the second aspect or the third aspect.

[0074] Furthermore, the application is the use of itaconylated carboxymethyl chitosan derivatives in the preparation of soft tissue fillers (such as gels), medicines, and tissue engineering materials.

[0075] Specifically, the soft tissue filler can be used to eliminate wrinkles (such as wrinkles around the eyes, forehead wrinkles, glabellar wrinkles, perioral wrinkles, nasolabial folds, tear grooves, nasolabial folds, neck wrinkles, hand wrinkles, stretch marks, etc.), anti-aging, scar and trauma repair, etc.

[0076] Specifically, the drug uses itaconylated carboxymethyl chitosan derivatives as carriers to achieve the purposes of sustained release, controlled release, targeted drug delivery, etc.

[0077] Specifically, the tissue engineering material can be a bone tissue engineering material, a cartilage tissue engineering material, a corneal tissue engineering material, a cardiovascular tissue engineering material, a liver tissue engineering material, etc.

[0078] The present invention has the following beneficial effects:

[0079] 1. The present invention uses itaconic anhydride or itaconic acid as a modifier to double-bond modified carboxymethyl chitosan. By introducing an alkaline reagent and adjusting the timing of its addition, the double-bonding grafting efficiency is improved, so that the final double-bonding rate of the carboxymethyl chitosan is 70-100%. After modification, a large number of hydrophilic carboxyl groups are introduced, so that the moisturizing performance of the double-bonded carboxymethyl chitosan gel material is significantly better than that of the unmodified carboxymethyl chitosan material.

[0080] 2. When itaconic anhydride is used as a modifier, the present invention simultaneously drips itaconic anhydride and an alkaline reagent by using a double-drop method, and controls the amount of both added per unit time by the dripping speed, so that the itaconic anhydride undergoes ring opening and grafting with the amino group after being dripped into water. The alkaline reagent added thereto neutralizes the pH drop caused by the ring opening of itaconic anhydride, so that the pH of the system is 6.5-9.0, thereby avoiding the precipitation of carboxymethyl chitosan. In addition, the protonation of the amino group can be prevented during the dripping process, the amino group can be activated, the stability and activity of the system during the reaction process can be guaranteed to the greatest extent, and the double-bond grafting efficiency can be improved.

[0081] 3. When itaconic acid is used as a modifier in the present invention, an alkaline reagent is first introduced into itaconic acid to adjust the pH of the solution to 7.0-8.0 to form a buffer salt system of itaconic acid and sodium itaconate, which is then added to the carboxymethyl chitosan solution. The formed buffer salt system can, on the one hand, make the reaction conditions mild and avoid the occurrence of excessive acidity in the system. While the COOH in itaconic acid continuously reacts with EDC, the COOH generated by the hydrolysis of sodium itaconate also reacts with EDC, thereby improving the activation efficiency of the carboxyl group activated by EDC. On the other hand, the reaction is carried out under weakly alkaline conditions to avoid the precipitation of carboxymethyl chitosan and simultaneously activate the amino groups on the carboxymethyl chitosan, thereby improving the modification efficiency.

[0082] 4. The present invention provides an itaconylated carboxymethyl chitosan derivative and a method for its preparation. This preparation method does not require heating, allowing the modification reaction to proceed under relatively mild conditions. It also exhibits a high grafting rate, positively impacting subsequent applications. For example, it exhibits high reaction efficiency when initiating free radical reactions. The introduced hydrophilic carboxyl groups further enhance the moisturizing, mechanical, and thermal stability of the double-bonded carboxymethyl chitosan gel. This method has potential research value and broad application prospects in cosmetic moisturizing and in vivo applications. BRIEF DESCRIPTION OF THE DRAWINGS

[0083] FIG1 is a schematic diagram showing the grafting reaction of itaconic anhydride and carboxymethyl chitosan.

[0084] FIG2 is a schematic diagram showing the grafting reaction of itaconic acid and carboxymethyl chitosan.

[0085] FIG3 shows the itaconylated carboxymethyl chitosan derivative of Example 1. 1 H NMR spectrum.

[0086] FIG4 shows the itaconylated carboxymethyl chitosan derivative of Example 4. 1 H NMR spectrum.

[0087] Figure 5 shows the carboxymethyl chitosan 1 H NMR spectrum.

[0088] FIG6 is a comparison diagram showing the itaconylated carboxymethyl chitosan derivative of Example 6 ( FIG6A ) and the itaconylated carboxymethyl chitosan derivative of Comparative Example 3 ( FIG6B ). DETAILED DESCRIPTION

[0089] Unless otherwise defined, all scientific and technical terms used in the present invention have the same meanings as commonly understood by one of ordinary skill in the art to which the present invention relates.

[0090] The disclosures of various publications, patents, and published patent specifications cited herein are incorporated by reference in their entirety.

[0091] The embodiments of the present invention will be described in detail below with reference to the examples, but it will be understood by those skilled in the art that the following examples are merely illustrative of the present invention and should not be construed as limiting the scope of the invention. Where specific conditions are not specified in the examples, the methods were performed according to conventional conditions or the conditions recommended by the manufacturer. Where the manufacturers of the reagents or instruments are not specified, they are all commercially available conventional products.

[0092] Example 1: Double-bonding of carboxymethyl chitosan with itaconic anhydride at pH 6.5 to obtain double-bonded carboxymethyl chitosan A1

[0093] Weigh 1.0g of carboxymethyl chitosan and add 50ml of deoxygenated purified water. Dissolve completely under mechanical stirring at 350 rpm for approximately 40 minutes, until the carboxymethyl chitosan is completely dissolved. Weigh 0.014 mol of itaconic anhydride (3 times the molar equivalent of the amino groups in the carboxymethyl chitosan repeating unit) and dissolve it in 10ml of acetone. Using a 3M sodium hydroxide solution, add the prepared itaconic anhydride solution and sodium hydroxide solution simultaneously to the carboxymethyl chitosan solution using a double-drop method. Both additions are performed under nitrogen. The itaconic anhydride acetone solution is added at a faster rate than the sodium hydroxide solution, ensuring that the molar amount of sodium hydroxide added per unit time is 1.5 times the molar amount of itaconic anhydride. After the itaconic anhydride is added, continue adding sodium hydroxide dropwise under nitrogen until the reaction system reaches a pH of 6.5. The reaction is then stirred magnetically at 400 rpm at room temperature under nitrogen for 4 hours. After the reaction, the solution was purified and dried to obtain itaconic acid-modified carboxymethyl chitosan, completing the double-bond modification. This double-bonded carboxymethyl chitosan was designated A1. A1 was characterized by H NMR spectroscopy. The H NMR spectrum, shown in Figure 3, shows peaks at 5.4 ppm and 5.9 ppm corresponding to the itaconic acid double bond. The presence of double bond peaks indicates successful grafting of itaconic acid onto the carboxymethyl chitosan, completing the double-bond modification. The integration of both double bond peaks was averaged, yielding a double-bond rate of 90%.

[0094] Example 2: Double-bonding of carboxymethyl chitosan with itaconic anhydride at pH = 7.5 to obtain double-bonded carboxymethyl chitosan A2

[0095] Weigh 1.0g of carboxymethyl chitosan and add 100ml of deoxygenated purified water. Dissolve completely under mechanical stirring at 350 rpm for approximately 40 minutes, until the carboxymethyl chitosan is completely dissolved. Weigh 0.018 mol of itaconic anhydride (4 times the molar equivalent of the amino groups in the carboxymethyl chitosan repeating unit) and dissolve it in 10ml of acetone. Using a 4M sodium hydroxide solution, add the prepared itaconic anhydride solution and sodium hydroxide solution simultaneously to the carboxymethyl chitosan solution using a double-drop method. Both additions are performed under nitrogen. The itaconic anhydride acetone solution is added at a faster rate than the sodium hydroxide solution, ensuring that the molar amount of sodium hydroxide added per unit time is twice the molar amount of itaconic anhydride. After the itaconic anhydride is added, continue adding sodium hydroxide dropwise under nitrogen until the reaction system reaches a pH of 7.5. The reaction is then allowed to proceed under nitrogen at room temperature for 4 hours with magnetic stirring at 400 rpm. After the reaction, the solution was purified and dried to obtain itaconylated carboxymethyl chitosan, completing the double-bond modification. This double-bonded carboxymethyl chitosan was designated A2. A2 was characterized by H NMR spectroscopy, integrating both double-bond peaks and calculating the average value. The double-bond ratio was 94%.

[0096] Example 3: Double-bonding of carboxymethyl chitosan with itaconic anhydride at pH = 8.5 to obtain double-bonded carboxymethyl chitosan A3

[0097] Weigh 1.0g of carboxymethyl chitosan and add 200ml of deoxygenated purified water. Dissolve completely under mechanical stirring at 350 rpm for approximately 40 minutes, until the carboxymethyl chitosan is completely dissolved. Weigh 0.023 mol of itaconic anhydride (5 times the molar equivalent of the amino groups in the carboxymethyl chitosan repeating unit) and dissolve it in 10ml of acetone. Using a 5M sodium hydroxide solution, add the prepared itaconic anhydride solution and sodium hydroxide solution simultaneously to the carboxymethyl chitosan solution using a double-drop method. Both additions are performed under nitrogen. The itaconic anhydride acetone solution is added at a faster rate than the sodium hydroxide solution, ensuring that the molar amount of sodium hydroxide added per unit time is 2.5 times the molar amount of itaconic anhydride. After the addition is complete, sodium hydroxide is added dropwise under nitrogen until the pH of the reaction system reaches 8.5. The reaction is then allowed to react at room temperature under nitrogen for 4 hours with magnetic stirring at 400 rpm. After the reaction, the solution was purified and dried to obtain itaconylated carboxymethyl chitosan, completing the double-bond modification. This double-bonded carboxymethyl chitosan was designated A3. A3 was characterized by H NMR spectroscopy, integrating both double-bond peaks and calculating the average value, revealing a double-bonding rate of 85%.

[0098] Example 4: Condensation of double-bonded carboxymethyl chitosan under 5 times equivalent itaconic acid to obtain double-bonded carboxymethyl chitosan B1

[0099] Weigh 0.5g carboxymethyl chitosan solution and dissolve it in 500ml water to obtain carboxymethyl chitosan solution. Weigh 5 times the molar equivalent of amino group in carboxymethyl chitosan repeating unit (0.012mol) itaconic acid and add it in 50ml water, then add 5M sodium hydroxide and dissolve gradually. After completely dissolving, adjust the solution pH to 7. Finally, after itaconic acid solution is diluted to 100ml, add itaconic acid solution. After fully stirring and evenly mixing, add EDC / NHS (0.005mol) of 2 times the molar equivalent of amino group in carboxymethyl chitosan repeating unit, mechanical stirring reaction is 6 hours at room temperature. After the reaction, the solution purification process in the system is carried out, and after drying, itaconic acidized carboxymethyl chitosan is obtained, and double bond modification is completed. This double bonded carboxymethyl chitosan is named after B1. NMR characterization of B1 revealed that the NMR spectrum of the condensed double-bonded carboxymethyl chitosan was consistent with that of the double-bonded carboxymethyl chitosan obtained by ring-opening grafting with itaconic anhydride, as shown in Figure 4. The peaks at 5.9 ppm and 5.4 ppm are attributed to the double bonds after itaconic acid grafting. Based on the H NMR spectrum, the double-bonding rate was calculated to be 70%.

[0100] Example 5: Condensation of double-bonded carboxymethyl chitosan under 10 times equivalent itaconic acid to obtain double-bonded carboxymethyl chitosan B2

[0101] Weigh 0.5g carboxymethyl chitosan solution and dissolve it in 100ml water to obtain carboxymethyl chitosan solution. Weigh 10 times the molar equivalent of the amino group in the carboxymethyl chitosan repeating unit (0.023mol) itaconic acid and add it to 50ml water, then add 5M sodium hydroxide and dissolve gradually. After complete dissolution, adjust the solution pH to 7.5. Finally, dilute the itaconic acid solution to 100ml and add it to the carboxymethyl chitosan solution. After sufficient stirring and mixing, add 4 times the molar equivalent of the amino group in the carboxymethyl chitosan repeating unit (0.01mol) EDC / NHS, and mechanically stir the reaction at room temperature for 6 hours. After the reaction, the solution in the system is purified and dried to obtain itaconic acid-modified carboxymethyl chitosan, complete double bond modification, and the double bonded carboxymethyl chitosan is named B2. According to the nuclear magnetic resonance hydrogen spectrum, the double bond rate is calculated to be 92%.

[0102] Example 6: Condensation of double-bonded carboxymethyl chitosan under 20 times equivalent itaconic acid to obtain double-bonded carboxymethyl chitosan B3

[0103] Weigh 0.5g carboxymethyl chitosan solution and dissolve it in 100ml water to obtain carboxymethyl chitosan solution. Weigh 20 times the molar equivalent of the amino group in the carboxymethyl chitosan repeating unit (0.046mol) itaconic acid and add it to 50ml water, then add 5M sodium hydroxide and dissolve gradually. After complete dissolution, adjust the solution pH to 7.5. Finally, dilute the itaconic acid solution to 100ml and add it to the carboxymethyl chitosan solution. After sufficient stirring and mixing, add 8 times the molar equivalent of the amino group in the carboxymethyl chitosan repeating unit (0.02mol) EDC / NHS, and mechanically stir the reaction at room temperature for 6 hours. After the reaction, the solution in the system is purified and dried to obtain itaconic acid-modified carboxymethyl chitosan, complete double-bonding modification, and the double-bonding carboxymethyl chitosan is named B3. According to the hydrogen nuclear magnetic resonance spectrum, the double-bonding rate calculated is 94%.

[0104] Example 7: Condensation of double-bonded carboxymethyl chitosan under 30 times equivalent itaconic acid to obtain double-bonded carboxymethyl chitosan B4

[0105] Weigh 0.5g carboxymethyl chitosan solution and dissolve it in 50ml water to obtain carboxymethyl chitosan solution. Weigh 30 times (0.069mol) itaconic acid of the molar equivalent of amino group in carboxymethyl chitosan repeating unit and add it to 50ml water, then add 5M sodium hydroxide and dissolve gradually. After complete dissolution, adjust the solution pH to 8. Finally, after the itaconic acid solution is diluted to 100ml, add it to the carboxymethyl chitosan solution. After fully stirring and mixing, add (0.03mol) EDC / NHS of the molar equivalent of amino group in carboxymethyl chitosan repeating unit, and mechanically stir the reaction for 6 hours at room temperature. After the reaction, the solution in the system is purified and dried to obtain itaconic acid-modified carboxymethyl chitosan, complete double bond modification, and the double bond carboxymethyl chitosan is named B4. According to the hydrogen nuclear magnetic resonance spectrum, the double bond rate calculated is 75%.

[0106] Comparative Example 1: Carboxymethyl chitosan was dissolved in acetic acid solution and itaconic anhydride was double-bonded and grafted onto carboxymethyl chitosan

[0107] Weigh 1.0g of carboxymethyl chitosan and add 100ml of 3% acetic acid solution. Dissolve the mixture under mechanical stirring at 350 rpm for approximately 40 minutes until the carboxymethyl chitosan dissolves. Weigh 0.018 mol of itaconic anhydride (4 times the molar equivalent of the amino groups in the carboxymethyl chitosan repeating unit) and dissolve itaconic anhydride in 10ml of acetone. All additions were performed under nitrogen. The itaconic anhydride acetone solution was added in 10ml drops. After addition, the mixture was stirred magnetically at 400 rpm at room temperature under nitrogen for 4 hours. After the reaction, the solution was purified and dried to obtain itaconylated carboxymethyl chitosan in an acetic acid environment, completing the double-bond modification. This double-bonded carboxymethyl chitosan was designated C1. Proton nuclear magnetic resonance (HNMR) spectroscopy was performed, and the average value of the two double-bond peaks was integrated, revealing a double-bonding rate of 54%.

[0108] Comparative Example 2: Double bond grafting of itaconic anhydride onto carboxymethyl chitosan under alkaline conditions

[0109] Weigh 1.0g of carboxymethyl chitosan and add 100ml of deoxygenated purified water. Dissolve completely under mechanical stirring at a speed of 350r / min. Stir for about 40min until the carboxymethyl chitosan is completely dissolved. Use 4M sodium hydroxide solution and add it to the carboxymethyl chitosan solution, stirring thoroughly to adjust the pH to 7.5. Weigh 4 times the equivalent of carboxymethyl chitosan (0.018mol) of itaconic anhydride and dissolve itaconic anhydride in 10ml of acetone. The acetone solution of itaconic anhydride is added dropwise to the reaction system under nitrogen protection. After the addition is complete, the reaction is stirred magnetically at room temperature for 4h under nitrogen protection. The magnetic stirring speed is 400r / min. After the reaction, the solution in the system is purified and dried to obtain itaconic acid-modified carboxymethyl chitosan, completing the double bond modification. This double-bonded carboxymethyl chitosan is named C2. The H NMR spectrum was characterized, and the two double bond peaks were integrated and the average value was calculated. The double bond rate was 60%.

[0110] Comparative Example 3: Double-bonded carboxymethyl chitosan was condensed under the conditions of 1 equivalent of itaconic acid to obtain double-bonded carboxymethyl chitosan

[0111] 0.5g of carboxymethyl chitosan solution was weighed and dissolved in 100ml of water to obtain a carboxymethyl chitosan solution. 1 times (0.002mol) of itaconic acid, the molar equivalent of the amino group in the carboxymethyl chitosan repeating unit, was weighed and added to 50ml of water. 5M sodium hydroxide was then added to gradually dissolve the solution. After complete dissolution, the pH of the solution was adjusted to 7.5. Finally, the itaconic acid solution was diluted to 100ml and added to the carboxymethyl chitosan solution. After sufficient stirring and mixing, 8 times (0.02mol) of EDC / NHS, the molar equivalent of the amino group in the carboxymethyl chitosan repeating unit, was added. The mixture was mechanically stirred and reacted for 6 hours at room temperature to obtain itaconic acid-modified carboxymethyl chitosan, completing the double bond modification. The double bond-modified carboxymethyl chitosan was named C3. After the reaction, C3 was a turbid suspension (as shown in Figure 6B), indicating that the dicarboxyl groups in itaconic acid were involved in the amide condensation reaction, forming a microgel that caused turbidity. The solution of double-bond modified carboxymethyl chitosan B3 prepared according to the process in Example 6 (as shown in FIG6A ) is a transparent and uniform clear solution, indicating that itaconic acid is successfully grafted onto the carboxymethyl chitosan and no dicarboxyl amide condensation reaction occurs.

[0112] Comparative Example 4: Condensation of double-bonded carboxymethyl chitosan under alkaline conditions to obtain double-bonded carboxymethyl chitosan C4

[0113] Weigh 0.5g of carboxymethyl chitosan solution and dissolve it in 100ml of water to obtain a carboxymethyl chitosan solution. Use 5M sodium hydroxide to adjust the solution pH to 7.5. Weigh 20 times the molar equivalent of the amino group in the carboxymethyl chitosan repeating unit (0.046mol) of itaconic acid and add it to 100ml of water. After complete dissolution, add it to the carboxymethyl chitosan solution. After thorough stirring and mixing, add 8 times the molar equivalent of the amino group in the carboxymethyl chitosan repeating unit (0.02mol) of EDC / NHS and react at room temperature with mechanical stirring for 6 hours. After the reaction, the solution in the system is purified and dried to obtain itaconylated carboxymethyl chitosan, completing the double bond modification. The condensed double bonded carboxymethyl chitosan is named C4. It is characterized by hydrogen nuclear magnetic resonance spectrum. The two double bond peaks are integrated and averaged, and the double bond rate is 58%.

[0114] Example 8: Preparation of heated self-crosslinking gel of double bond modified carboxymethyl chitosan

[0115] Heat-induced self-crosslinking gels were prepared using the double-bonded carboxymethyl chitosans obtained in Examples 1-7 and Comparative Examples 1, 2, and 4, respectively. 0.1 g each of double-bonded carboxymethyl chitosans A1, A2, A3, B1, B2, B3, B4, C1, C2, and C4 were dissolved in water to form a 20 mg / ml solution. The solution was heated to 60° C. and maintained for 5 h to obtain the corresponding crosslinked gels, designated A1′, A2′, A3′, B1′, B2′, B3′, B4′, C1′, C2′, and C4′, respectively.

[0116] Test Example 1: Gel Moisturizing Performance Test

[0117] The gels obtained in Example 8 were dried at 40°C to constant weight. 0.5 g of carboxymethyl chitosan and each gel were weighed, and 10% of the weight of each gel was added to purified water. The gels were placed in a desiccator filled with dry silica gel and placed in a 25°C constant temperature box. The weight change of each gel after 7 days was recorded. The weight of the gel after 7 days was weighed. n Compared with the gel weight 7 days ago o , calculated according to the formula, moisturizing rate % = 100H n / H o The moisturizing rate of the obtained gel is shown in Table 1.

[0118] Table 1 Gel moisturizing performance test results

[0119] As shown in Table 1, the moisturizing properties of the double-bonded carboxymethyl chitosan gels are further improved compared to those of the un-double-bonded grafted carboxymethyl chitosan. This is because, after double-bonding, the carboxyl groups from itaconic anhydride or itaconic acid are introduced into the carboxymethyl chitosan. The increase in hydrophilic carboxyl groups improves the water retention of the double-bonded product. However, gel C1' in Comparative Example 1 dissolves under acidic conditions, where carboxymethyl chitosan easily precipitates. Furthermore, the amino group reactivity is low, resulting in a low double-bonding grafting rate and poor moisturizing properties. Compared with Example 2, Comparative Example 2 is different from Example 2 in that sodium hydroxide is first added to the carboxymethyl chitosan solution and then itaconic anhydride is added dropwise under alkaline conditions. Although the amino groups on the carboxymethyl chitosan can be protected from protonation under alkaline conditions, the carboxyl groups exposed after the ring opening of itaconic anhydride in the aqueous solution are easily neutralized by sodium hydroxide, which affects the activity of itaconic anhydride, resulting in a decrease in the double bond grafting rate and limited improvement in moisturizing performance. In Example 2, sodium hydroxide and itaconic anhydride are added dropwise to the carboxymethyl chitosan at the same time by a double-drop method, which can avoid the precipitation of raw materials and improve the activity of the amino group. Therefore, the double bond grafting efficiency is high, and its moisturizing performance (92.1%) is much higher than that of the gel (50.3%) and the unmodified carboxymethyl chitosan material (42.5%) in Comparative Example 2. In Comparative Example 4, since sodium hydroxide is directly added to the carboxymethyl chitosan solution, compared with the system in Example 6 in which sodium hydroxide is first added to the itaconic acid solution to form a buffer salt, the problem of local overacidity is easily generated when itaconic acid is subsequently added in Comparative Example 4, thereby causing the precipitation of carboxymethyl chitosan and affecting the activity of the amino group. Ultimately, the double bond grafting effect is poor, and its moisturizing property (49.6%) is also significantly lower than the moisturizing property (92.7%) of the gel in Example 6.

[0120] Test Example 2: Determination of gel rheological properties

[0121] The self-crosslinking gels A1', A2', A3', B1', B2', B3', B4', C1', C2', and C4' prepared in Example 8 were tested using a rotational rheometer before and after sterilization. The sterilization conditions were: sterilization at 121°C for 15 minutes; the rotational rheometer test parameters were: sample 2ml, operating gap: 1000mm, loading gap: 45000m, operating temperature: 37°C, deformation: 1%, frequency: 0.9Hz, and operating time: 60s. The rheological data of each gel are shown in Table 2; the calculation method for the loss rate of G' (elastic modulus) is as follows:

[0122] G' loss rate = (G' before sterilization - G' after sterilization) / G' before sterilization;

[0123] Table 2 Determination results of gel rheological properties

[0124] The loss rate of elastic modulus before and after sterilization represents the thermal stability of the gel to a certain extent. In this experimental example, the double-bonded carboxymethyl chitosan obtained by the two double-bond grafting methods of itaconic anhydride or itaconic acid has only one conformation (comparing the nuclear magnetic resonance spectrum of carboxymethyl chitosan Figure 5 with the nuclear magnetic resonance spectrum of the two grafted modified double-bonded carboxymethyl chitosan Figures 3 and 4, it can be seen that the double-bonded products obtained after modification have only two peaks, at 5.9ppm and 5.4ppm respectively). This is mainly due to the fact that after the ring opening of itaconic anhydride, the steric hindrance between the double bond and the carboxyl group close to the double bond is large, so the carboxyl group cannot complete the acylation grafting reaction with the amino group, and only the carboxyl group far away from the double bond is available for grafting; when itaconic acid is selected for modification, there is also a large steric hindrance between the double bond and the carboxyl group close to the double bond, and only the carboxyl group far away from the double bond is available for grafting.

[0125] In addition, after high-temperature sterilization, some glycosidic bonds on the carboxymethyl chitosan will be broken, resulting in a decrease in the elastic modulus after sterilization. However, based on the similarity of the chemical structure, there is no significant difference in the loss of elastic modulus between the gels corresponding to the products obtained by the two modification methods, and the loss rate is within 17%, indicating that the double-bonded carboxymethyl chitosan can improve the thermal stability of the gel; and from Table 2, it can be seen that regardless of which modification method is used in the examples, when conducting a vertical comparison, the higher the double-bonding rate, the higher the elastic modulus of the gel prepared. This may be due to the higher grafting rate, which gives the gel more cross-linking grafting sites during cross-linking, forming a more stable network structure, thereby providing higher mechanical strength.

[0126] For the gels prepared in Comparative Examples 1, 2, and 4, the elastic modulus before sterilization is low, and after high-temperature sterilization, the loss rate of the elastic modulus is also very high, which is 49.35%, 53.23%, and 50.17%, respectively. This may be because the double bond grafting rate is low in the double bond reaction, and the low grafting rate can provide fewer cross-linking sites, resulting in a loose network structure formed by cross-linking. Therefore, the final gel has a low modulus and poor thermal stability, and the loss rate of the elastic modulus after sterilization is high.

[0127] Test Example 3: Lysozyme degradation rate test in vitro

[0128] Lysozyme was diluted to a solution of 0.5 mg / ml using phosphate buffer and stored at 4°C. 2 ml each of the self-crosslinked gels A1', A2', A3', B1', B2', B3', B4', C1', C2', and C4' prepared in Example 8 were taken, placed at 4°C for 2 hours, and then 1 ml of lysozyme solution (concentration of 0.5 mg / ml) was added and quickly stirred evenly. The mixture was then placed on a rheometer for degradation testing. The rheometer test parameters were: 40 mm diameter aluminum flat plate fixture, 2 ml sample, operating gap: 1000 μm, test mode: Flow Peak Hold, test time: 7200 s, and the Peltier plate temperature of the rheometer must be equilibrated to 4°C before loading. During the test, the shear viscosity at 0 min, 15 min, 30 min, and 120 min was recorded. The shear viscosity at 0 min was η0, and the shear viscosity measured at different times was η1. The degradation rate (%) = (η0-η1) / η0×100. The in vitro degradation results are shown in Table 3:

[0129] Table 3 Degradation results of double-bonded carboxymethyl chitosan gel after cross-linking

[0130] It can be seen from the data in the table that during the gel degradation process, the degradation rate of the gel prepared by self-crosslinking the double-bonded grafted carboxymethyl chitosan A1, A2, A3, B1, B2, B3, and B4 prepared in Examples 1-7 is much lower than that of the gel prepared by self-crosslinking the carboxymethyl chitosan C1, C2, and C4 with lower grafting rates in Comparative Examples 1-2 and 4. The degradation of the two groups of gels showed a significant difference in degradation rate 15 minutes after the test. The self-crosslinked gels C1', C2', and C4' prepared by comparative examples 1-2 and 4 degraded quickly, with degradation rates all above 20%. The degradation rates of the gels A1', A2', A3', B1', B2', B3', and B4' prepared by self-crosslinking in examples 1-7 were all within 15%, and as the double bonding rate increased, the degradation rate decreased. As can be seen from the table, when the double bonding rate was above 90%, the degradation rates of gels A1', A2', B2', and B3' were all below 9% at 15 minutes. The same degradation trend can also be observed at 30 minutes and 120 minutes. When the double-bonding rate is 90%, the degradation rate at 120 minutes is about 60%, while when the double-bonding rate is below 60%, the degradation rate at 120 minutes is above 80%. This is mainly because the double-bonding grafting modification can provide cross-linking sites for carboxymethyl chitosan self-crosslinking. The higher the double-bonding grafting rate, the more cross-linking sites the carboxymethyl chitosan has during cross-linking, and thus the higher the cross-linking efficiency, making the gel have a more stable and dense mechanical structure, further improving the stability and effectively preventing the rapid degradation of the carboxymethyl chitosan gel. In addition, lysozyme mainly acts on the β-1,4 glycosidic bond connecting the carboxymethyl chitosan backbone, causing the carboxymethyl chitosan backbone in the gel to be degraded into fragments, destroying the mechanical strength of the gel and causing degradation. The stable mechanical structure can effectively protect the β-1,4 glycosidic bonds in carboxymethyl chitosan from being degraded by lysozyme, resulting in a low degradation rate for gels prepared from carboxymethyl chitosan with a high double-bonding grafting rate. However, when the double-bonding rate is low, the prepared gel structure is loose, making it difficult to effectively protect the β-1,4 glycosidic bonds connecting the carboxymethyl chitosan backbone. Lysozyme degrades the β-1,4 glycosidic bonds more quickly, resulting in a higher overall degradation rate. Therefore, gels prepared from carboxymethyl chitosan with a high double-bonding rate have higher stability and a lower degradation rate, which is beneficial for subsequent clinical applications.

[0131] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the above embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the above embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.

Claims

1. An itaconylated carboxymethyl chitosan derivative, It is characterized in that Itaconic acid or itaconic anhydride is used as a modifier, and an alkaline reagent is introduced to form an amide bond between itaconic acid or itaconic anhydride and carboxymethyl chitosan for grafting reaction to obtain itaconic acid-modified carboxymethyl chitosan derivatives, thereby completing double bond modification.

2. The itaconylated carboxymethyl chitosan derivative according to claim 1, It is characterized in that The carboxymethyl chitosan is selected from N-carboxymethyl chitosan, O-carboxymethyl chitosan or N,O-carboxymethyl chitosan, preferably O-carboxymethyl chitosan, more preferably 6-O-carboxymethyl chitosan; the alkaline agent is selected from sodium hydroxide, potassium hydroxide, calcium hydroxide or barium hydroxide.

3. A method for preparing an itaconic acid-modified carboxymethyl chitosan derivative using itaconic anhydride as a modifier, It is characterized in that The preparation method comprises the following steps: under the protection of inert gas, using a double drop method, simultaneously adding an itaconic anhydride solution and an alkaline reagent solution to a carboxymethyl chitosan solution, the pH value of the reaction system is 6.5-9.0, stirring the reaction, and obtaining an itaconic acid-acylated carboxymethyl chitosan derivative.

4. The preparation method according to claim 3, It is characterized in that The solvent of the carboxymethyl chitosan is water; preferably, the solvent of the carboxymethyl chitosan is deoxygenated water; Preferably, the concentration of the carboxymethyl chitosan solution is 1-20 mg / ml; more preferably, the concentration of the carboxymethyl chitosan solution is 5-20 mg / ml.

5. The preparation method according to claim 3, It is characterized in that The amount of itaconic anhydride added is 2-6 times the molar equivalent of the amino group in the carboxymethyl chitosan repeating unit; Preferably, the reaction time is 3-12 hours; preferably, the reaction temperature is 10-30°C.

6. The preparation method according to claim 3, It is characterized in that In the double-drop method, the molar amount of the alkaline reagent hydroxide added per unit time is 1.5-2.5 times the molar amount of itaconic anhydride; the alkaline reagent is selected from sodium hydroxide, potassium hydroxide, calcium hydroxide or barium hydroxide.

7. A method for preparing an itaconic acid-modified carboxymethyl chitosan derivative, It is characterized in that The preparation method comprises the following steps: adding an alkaline agent to itaconic acid to adjust the pH value of the itaconic acid solution to 7.0-8.0, then adding it to a carboxymethyl chitosan solution, then adding an activator and an auxiliary activator, stirring and reacting, and obtaining an itaconic acid-modified carboxymethyl chitosan derivative.

8. The preparation method according to claim 7, It is characterized in that The solvent of the carboxymethyl chitosan is water; Preferably, the concentration of the carboxymethyl chitosan solution is 1-10 mg / mL; more preferably, the concentration of the carboxymethyl chitosan solution is 5-10 mg / mL; Preferably, the amount of itaconic acid added is 5-30 times, more preferably 10-20 times, the molar equivalent of the amino group in the carboxymethyl chitosan repeating unit; Preferably, the reaction time is 4-20h; preferably, the reaction temperature is 10-30°C; Preferably, the alkaline agent is selected from sodium hydroxide, potassium hydroxide, calcium hydroxide or barium hydroxide.

9. The preparation method according to claim 7, It is characterized in that The activator is a water-soluble carbodiimide, preferably selected from 1-ethyl-3-(dimethylaminopropyl)carbodiimide, 1-(3-dimethylaminopropyl)-3-ethyl-carbodiimide, 1-cyclohexyl-3-(2-morpholinoethyl)carbodiimide, 1,3-bis[bis(methoxymethyl)methyl]carbodiimide; preferably, the activator is 1-ethyl-3-(dimethylaminopropyl)carbodiimide; Preferably, the amount of the activator added is 2-20 times, more preferably 4-10 times, the molar equivalent of the amino group in the carboxymethyl chitosan repeating unit; Preferably, the co-activator is selected from one or more of N-hydroxysuccinimide, sulfonated N-hydroxysuccinimide, tert-butyl alcohol, and 1-hydroxybenzotriazole; more preferably, the co-activator is N-hydroxysuccinimide; Preferably, the amount of the co-activator is the same as the amount of the activator.

10. Use of the itaconylated carboxymethyl chitosan derivative according to claim 1 or the itaconylated carboxymethyl chitosan derivative prepared by the method according to any one of claims 2 to 9 in the preparation of soft tissue fillers, drugs and tissue engineering materials.