Nonaqueous inkjet ink composition
By adding a specific proportion of carbon black and organic solvent to the non-aqueous inkjet ink, and using infrared drying technology, the problems of nozzle clogging and substrate deformation are solved, and non-aqueous spray with excellent spray stability and drying are achieved Ink printing ensures protection of resin substrates.
Patent Information
- Application Number
- CN202380035140.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-06-08
- Filing Date
- 2023-03-17
- Publication Date
- 2024-12-03
AI Technical Summary
The conventional non-aqueous inkjet composition for ink jet can easily cause the nozzle to be blocked after continuous ejection, and the drying property is unstable, and the substrate is easily deformed or wrinkled when heated and dried on the resin substrate, affecting the printing quality.
Non-aqueous inkjet ink composition containing 2.5 to 10.0 mass % carbon black, 80.0 mass % or more butyl acetate evaporation rate is 20 to 80, and resin, dried by infrared irradiation, and acrylic acid, Cellulose or vinyl chloride-vinyl acetate resins, and optimize the amount of carbon black and infrared irradiation intensity during inkjet printing.
The excellent effect of spray stability and dryness is achieved, and damage to the resin substrate is avoided, and the integrity of the substrate and the stability of the printing part are ensured during the printing process.
Smart Images

Figure SMS_1 
Figure SMS_2 
Figure SMS_3
Abstract
Description
Technical Field
[0001] The present invention relates to a non-aqueous inkjet ink composition having a printing surface as a printing surface on a substrate surface made of a resin or a surface of an arbitrary material. Background Art
[0002] As described in Patent Document 1, there is known a non-aqueous inkjet ink composition containing a pigment, a resin, a dispersant, and an organic solvent, wherein the substrate to be printed is a resin.
[0003] These non-aqueous inkjet ink compositions can be dried by rapidly evaporating the organic solvent immediately after printing, thereby enabling printing of a target image or the like.
[0004] However, such non-aqueous inkjet ink compositions have good drying properties, but when the ink is ejected continuously and then stopped, the nozzles may become clogged when the ink is ejected again, that is, the nozzles may not eject the non-aqueous inkjet ink composition. Therefore, it is necessary to clean the ink or replace it with a non-aqueous inkjet ink composition that dries slowly.
[0005] When operations such as cleaning are required, the productivity of the printed matter will be reduced. In addition, when a non-aqueous inkjet printing ink composition that dries slowly is used, when the printed matters are stacked, the ink composition of the lower printed part will be transferred to the back of the printed matter above it, and there is a risk of back printing.
[0006] It is known that there is a method of drying by heating immediately after printing an inkjet ink composition, wherein the inkjet ink composition is aqueous or contains water, and the method is to heat the water to evaporate it and print it. Such a printing method of heating and drying can be used in the case where a special paper is used as a printing substrate. When a resin is used as a printing substrate, even if printing is performed only on a part of the surface of the printing substrate, the heating and drying device is used to heat the entire surface of the printing substrate, so that thermal deformation or wrinkles may occur on at least a part of the printing substrate as the resin.
[0007] Furthermore, when drying by irradiation with infrared rays, a plurality of printed materials can be obtained quickly, so when continuous printing and drying are performed, the irradiation intensity of infrared rays needs to be increased. Therefore, even if the printed ink composition can be dried, the printed substrate is also heated at the same time, and because the heating temperature becomes too high, the printed substrate or the printed portion that has been formed may be deformed or wrinkled.
[0008] Furthermore, when a second printing is performed on the printed portion and / or non-printed portion of a printed substrate that has already been partially printed for the first time, if the second printing is accompanied by heat drying, the printed substrate or the printed portion of the first printing may sometimes be damaged by the heat, such as wrinkles or deformation.
[0009] Patent Literature Patent Document 1: Japanese Patent Application Publication No. 2018-59106 The problem to be solved by the present invention is to provide an inkjet ink composition and a printing method thereof, which have excellent ejection stability and drying properties even when printing is performed on a printed substrate whose printing surface is composed of a resin or the like, and further, even when the printed object is a resin substrate on which printing has already been performed on a portion, the printing can be performed under conditions where there is no thermal influence on the printed substrate or the already formed printed portion.
[0010] The present inventors have conducted intensive studies to solve the above-mentioned problems and, as a result, have found that the above-mentioned problems can be solved by using a specific composition as an organic solvent, thereby completing the present invention.
[0011] That is, the present invention is as follows.
[0012] 1. A non-aqueous inkjet ink composition for printing on a resin substrate, characterized in that: Contains 2.5 to 10.0 mass % of carbon black, Containing 80.0% by mass or more of an organic solvent having an evaporation rate of 20 to 80 when the evaporation rate of butyl acetate is 100, Contains resin, And it has drying properties based on infrared irradiation.
[0013] 2. The non-aqueous inkjet ink composition according to item 1, which is used for printing on a printing layer provided on a resin substrate.
[0014] 3. The non-aqueous inkjet ink composition according to 1 or 2, wherein the resin contained in the non-aqueous inkjet ink composition comprises at least one selected from the group consisting of acrylic resins, cellulose resins, and vinyl chloride-vinyl acetate resins.
[0015] 4. The non-aqueous inkjet ink composition according to any one of 1 to 3, comprising 80.0% by mass or more of an organic solvent having an evaporation rate of 30 to 60 when the evaporation rate of butyl acetate is 100.
[0016] 5. A printing method based on a non-aqueous inkjet ink composition, characterized in that: Contains 2.5 to 10.0 mass % of carbon black, Containing 80.0% by mass or more of an organic solvent having an evaporation rate of 20 to 80 when the evaporation rate of butyl acetate is 100, A non-aqueous inkjet ink composition containing a resin, Inkjet printing is performed on a printed substrate made of resin and / or a printed portion pre-formed on the surface of the printed substrate. Drying is carried out by infrared irradiation.
[0017] The non-aqueous inkjet ink composition of the present invention contains an acrylic resin, a pigment, a pigment dispersant, and a specific composition as an organic solvent.
[0018] Therefore, as a heat-drying ink composition for printing on a resin substrate, it has excellent drying properties and good ejection stability from the nozzle of an inkjet printer. Furthermore, it can achieve the effect of printing under conditions that will not damage the resin substrate or the already formed printed part. DETAILED DESCRIPTION
[0019] (Carbon Black) As the carbon black in the present invention, the carbon black used for ink can be used. It is difficult to fully heat and dry the non-aqueous inkjet ink composition when only solvent blacks such as Lactam Black, Perylene Black, Solvent Black 29, various dispersed blacks, direct blacks, acid blacks, etc. are contained. Among the black color materials that can absorb infrared rays, especially near infrared rays and generate heat, carbon black is required.
[0020] Carbon black can be used in one kind or in a mixture of two or more kinds, and its usage amount is 2.5 mass % or more and 10 mass % or less relative to the total amount of the non-aqueous inkjet ink composition. More preferably, it is 3.0 mass % or more. In addition, it is preferably 9.0 mass % or less, more preferably 8.5 mass % or less, more preferably 8.0 mass % or less, and most preferably 5.0 mass % or less. When it is less than 2.5 mass %, in order to dry the printed non-aqueous inkjet ink composition, it is necessary to excessively increase the energy of the irradiated infrared rays, and the temperature of the resin substrate as the printed substrate rises too high, and wrinkles or skews are generated on the surface of the resin substrate, or it is deformed and the possibility of causing damage is high. In order to prevent the occurrence of this damage, when the energy of the irradiated infrared rays is weakened, the drying property of the ink composition is reduced. On the other hand, when it is more than 10.0 mass %, the viscosity rises, and the ejection stability of the non-aqueous inkjet ink composition is reduced. In addition, even if higher energy infrared rays are irradiated, further improvement of drying property cannot be expected.
[0021] (Color materials other than carbon black) As color materials other than carbon black contained in the non-aqueous inkjet ink composition of the present invention, known inorganic and organic pigments or dyes, non-carbon black black color materials, etc. that have been used in conventional non-aqueous inkjet ink compositions may be used without impairing the effects brought about by the present invention.
[0022] Specific examples of the inorganic pigment include titanium oxide, zinc white, zinc oxide, lithopone, iron oxide, aluminum oxide, silicon dioxide, kaolinite, montmorillonite, talc, barium sulfate, calcium carbonate, silica, alumina, cadmium red, red iron oxide, molybdenum red, chrome vermilion, molybdenum orange, chrome yellow, lead chrome yellow, cadmium yellow, yellow iron oxide, titanium yellow, chromium oxide, chrome green, cobalt green, titanium cobalt green, cobalt chrome green, ultramarine, ultramarine blue, Prussian blue, cobalt blue, azure blue, manganese violet, cobalt violet, and mica.
[0023] Specific examples of organic pigments include azo pigments, azomethine pigments, polyazo pigments, phthalocyanine pigments, quinacridone pigments, anthraquinone pigments, indigo pigments, thioindigo pigments, quinophthalone pigments, benzimidazolone pigments, isoindoline pigments, and isoindolinone pigments. Specific examples of organic pigments represented by color index include Pigment Black 7, Pigment Blue 15, 15:1, 15:3, 15:4, 15:6, 60, Pigment Green 7, 36, Pigment Red 9, 48, 49, 52, 53, 57, 97, 122, 149, 168, 177, 178, 179, 206, 207, 209, 242, 254, 255, Pigment Violet 19, 23, 29, 30, 37, 4 0, 50, Pigment Yellow 12, 13, 14, 17, 20, 24, 74, 83, 86, 93, 94, 95, 109, 110, 117, 120, 125, 128, 137, 138, 139, 147, 148, 150, 151, 154, 155, 166, 168, 180, 185, Pigment Orange 36, 43, 51, 55, 59, 61, 71, 74, etc.
[0024] Furthermore, metallic pigments may be contained.
[0025] Specific examples of the dye include various known dyes such as anionic dyes, cationic dyes, nonionic dyes, and zwitterionic dyes.
[0026] (resin) The non-aqueous inkjet ink composition of the present invention contains a resin. The resin that can be contained needs to be sufficiently soluble in the solvent of the present invention and can form a film after printing. The non-aqueous inkjet ink composition of the present invention forms a film on the printed part by heating and drying, and is not an ink composition containing a resin that forms a resin film by reacting reactive components when heated.
[0027] As the resin that can be used, at least one selected from acrylic resins, cellulose resins, vinyl chloride-vinyl acetate resins and the like is preferably used.
[0028] The content of the resin relative to the total amount of the non-aqueous inkjet ink composition is preferably 1.0% by mass or more, more preferably 3.0% by mass or more, and further preferably 5.0% by mass or more. In addition, it is preferably 20.0% by mass or less, more preferably 15.0% by mass or less, and further preferably 12.0% by mass or less. When it is less than 1.0% by mass, the fixation with the substrate is insufficient and it is possible that it becomes difficult to form a printed layer, and when it exceeds 20.0% by mass, it is possible that it becomes difficult to print in a state with excellent ejection stability.
[0029] (Acrylic resin) Examples of the acrylic resin that may be contained in the non-aqueous inkjet ink composition of the present invention include polymers composed of (meth)acrylates soluble in organic solvents and copolymers thereof. Examples of such (meth)acrylates include alkyl (meth)acrylates such as ethyl (meth)acrylate, propyl (meth)acrylate, or butyl (meth)acrylate; and hydroxyalkyl (meth)acrylates such as hydroxymethyl (meth)acrylate, hydroxyethyl (meth)acrylate, hydroxypropyl (meth)acrylate, hydroxybutyl (meth)acrylate, and hydroxypentyl (meth)acrylate.
[0030] As an example, DIANAL series of Mitsubishi Rayon Corporation includes BR-60 (Tg: 75°C), BR-64 (Tg: 55°C), BR-75 (Tg: 90°C), BR-77 (Tg: 80°C), BR-83 (Tg: 105°C), BR-87 (Tg: 105°C), BR-88 (Tg: 105°C), BR-90 (Tg: 65°C), BR-93 (Tg: 50°C), BR-95 (Tg: 80°C), BR-105 (Tg: 50°C), BR-106 (Tg: 50°C), BR-107 (Tg: 50°C), BR-108 (Tg: 90°C), BR-113 (Tg: 75°C), BR-115 (Tg: 50°C) and BR-116 (Tg: 50°C).
[0031] (Cellulose resin) Examples of the cellulose resin that may be contained in the non-aqueous inkjet ink composition of the present invention include nitrocellulose (nitro-substituted products), lower acyl-substituted products such as cellulose acetate, cellulose acetate propionate, and cellulose acetate butyrate, and lower alkyl-substituted products such as methyl cellulose and ethyl cellulose.
[0032] (Vinyl chloride-vinyl acetate resin) The vinyl chloride-vinyl acetate resin that can be used in the present invention is a vinyl chloride-vinyl acetate copolymer containing vinyl chloride and vinyl acetate as essential components. In addition, a copolymer obtained by copolymerization by adding other radical polymerizable monomers as needed can also be used. In this case, the ester bond of the part derived from vinyl acetate is saponified, and a compound containing an amino group is used as another radical polymerizable monomer, or a hydrocarbon compound containing an amino group is subjected to a dehydrochlorination reaction in the part derived from vinyl chloride to introduce an amino group, for example, a vinyl chloride-vinyl acetate-vinyl alcohol copolymer containing an amino group.
[0033] As such a vinyl chloride-vinyl acetate-based resin, a copolymer of a vinyl chloride monomer and a vinyl acetate monomer, which has been conventionally used in an ink composition, can be used.
[0034] Specific examples include SOLBIN C, SOLBIN CL, SOLBIN CH, SOLBIN CN, SOLBIN C5R, SOLBIN A, SOLBIN AL, SOLBIN TA2, SOLBIN TA3, SOLBIN TAO, SOLBIN TA5R, SOLBIN M, SOLBIN ME, SOLBIN MFK (all from Nissin Chemical Industries, Ltd.), VINNOL E15 / 48A, VINNOL E22 / 48A, VINNOL E14 / 45, VINNOL H14 / 36, VINNOL H40 / 55, VINNOL E15 / 45M (all from WACKER), and the like.
[0035] As the vinyl chloride-vinyl acetate-based resin, it is preferable to use a vinyl chloride-vinyl acetate-based resin of 85% vinyl chloride-15% vinyl acetate.
[0036] In the case of a vinyl chloride-vinyl acetate copolymer having a hydroxyl group obtained by saponifying a part of the acetate portion, the film properties or the dissolved state of the resin are determined by the ratio of the structural unit based on the reaction site of vinyl chloride (the following formula 1), the structural unit based on the reaction site of vinyl acetate (the following formula 2), and the structural unit based on the saponification of the reaction site of vinyl acetate (the following formula 3) in the molecule.
[0037] That is, the structural unit based on the reaction site of vinyl chloride imparts toughness or hardness to the resin film, the structural unit based on the reaction site of vinyl acetate imparts adhesion or flexibility, and the structural unit based on the saponification of the reaction site of vinyl acetate imparts good solubility in organic solvents of the ink in consideration of the environment.
[0038] Formula 1 -CH2-CHCl- Formula 2 -CH2-CH(OCOCH3)- Formula 3 -CH2-CH(OH)- (Vinyl chloride-vinyl acetate-vinyl alcohol resin containing amino groups) The amino group-containing vinyl chloride-vinyl acetate-vinyl alcohol resin that can be used in the present invention is composed of vinyl chloride units, vinyl acetate units, vinyl alcohol units, and units containing amino groups. In addition, the so-called vinyl chloride units and vinyl acetate units refer to units composed of ethylene chains generated by the cleavage of unsaturated double bonds and residues obtained by removing the unsaturated double bonds of the monomers bonded thereto, which are occupied in the copolymer after the reaction of vinyl chloride and vinyl acetate. That is, the vinyl chloride unit is a unit represented by [-CH2-CHCl-], and the vinyl acetate unit is a unit represented by [-CH2-CH(OCOCH3)-]. In addition, the so-called vinyl alcohol unit is a unit composed of an ethylene chain after the ester bond of the vinyl acetate unit is hydrolyzed by saponification reaction and a hydroxyl group bonded thereto, and is represented by [-CH2-CH(OH)-]. Furthermore, the amino group-containing unit refers to a unit consisting of an ethylene chain generated by cleavage of a free radical polymerizable unsaturated double bond and a residue obtained by removing the unsaturated double bond of a monomer bonded thereto when an amino group-containing compound is used as another free radical polymerizable monomer, and is represented by [-CH2-CHX-] (X is a residue obtained by removing the unsaturated double bond of the monomer, and contains an amino group). On the other hand, when an amino group-containing hydrocarbon compound is introduced into a vinyl chloride unit by a dehydrogenation reaction, a unit obtained by replacing the chlorine of the vinyl chloride unit with a residue obtained by removing one hydrogen from the amino group-containing hydrocarbon compound is represented by [-CH2-CHY-] (Y is a residue obtained by removing one hydrogen from the amino group-containing hydrocarbon compound).
[0039] As a method for preparing the amino group-containing vinyl chloride-vinyl acetate-vinyl alcohol copolymer, for example, it can be obtained by the following method: a copolymer of vinyl chloride, vinyl acetate and an amino group-containing monomer having an ethylenically unsaturated double bond is obtained, and the copolymer is saponified to convert a part of the vinyl acetate unit into a vinyl alcohol unit to obtain an amino group-containing unit. Examples of the amino group-containing ethylenically unsaturated double bond monomer include general formula (1): [Chemistry 1]
[0040] (Where R 1 is a hydrogen atom or a methyl group, R2 and R3 are independently a monovalent hydrocarbon group, and m is an integer of 1 to 6. ) is a dialkylaminoalkyl (meth)acrylate represented by. In the above general formula (1), as the formula: (CH2) m Examples of the alkylene group represented by R2 and R3 include methylene, ethylene, trimethylene, propylene, tetramethylene, and butylene. Examples of the monovalent hydrocarbon group represented by R2 and R3 include alkyl groups having 1 to 4 carbon atoms, such as methyl, ethyl, propyl, isopropyl, and butyl. Specific examples of the amino group-containing ethylenically unsaturated double bond monomer represented by the general formula (1) include dimethylaminoethyl (meth)acrylate, diethylaminoethyl (meth)acrylate, dimethylaminopropyl (meth)acrylate, and diethylaminopropyl (meth)acrylate. As the amino group-containing ethylenically unsaturated double bond monomer, in addition to the monomer represented by the general formula (1), dimethylaminopropyl acrylamide, dimethylacrylamide, and acrylamide can also be used.
[0041] As another method for producing the above-mentioned vinyl chloride-vinyl acetate-vinyl alcohol copolymer containing amino groups, a method in which a part of the vinyl acetate units is converted into vinyl alcohol units by a saponification / amine modification method in the presence of an amine compound, and a part of the chlorine atoms of the vinyl chloride units are reacted with the amine compound to introduce the amino groups into the side chains to produce units containing amino groups can be cited. As the above-mentioned amine compounds, aliphatic amines, alicyclic amines, aromatic amines, etc. can be cited. Specifically, ethylamine, propylamine, butylamine, cyclohexylamine, ethanolamine, naphthylamine, aniline, o-toluidine, diethylamine, dibutylamine, diisobutylamine, dioctylamine, diethanolamine, N-methylaniline, trimethylamine, triethylamine, tributylamine, triisobutylamine, N-methyldiphenylamine, triethanolamine, etc. can be cited.
[0042] Furthermore, from the perspective of ink ejection stability or adhesion to a recording medium, an amino group-containing vinyl chloride-vinyl acetate-vinyl alcohol copolymer in which the proportion of vinyl alcohol units in the copolymer is 4.0 to 7.0% by mass can be preferably used. When the proportion of vinyl alcohol units in the copolymer is less than 4.0% by mass, adhesion tends to decrease, while when it exceeds 7.0% by mass, ejection stability tends to decrease.
[0043] In the amino group-containing vinyl chloride-vinyl acetate-vinyl alcohol copolymer, the amino group-containing vinyl chloride unit and the vinyl acetate unit are preferably contained in a mass ratio of amino group-containing vinyl chloride unit / vinyl acetate unit=80 / 20 to 99 / 1.
[0044] Furthermore, the content of the amino group-containing unit of the amino group-containing vinyl chloride-vinyl acetate-vinyl alcohol copolymer is preferably 0.1 to 5.0% by mass in the copolymer. When the proportion of the amino group-containing unit is less than 0.1% by mass, the ejection stability tends to decrease.
[0045] The amino group-containing vinyl chloride-vinyl acetate-vinyl alcohol copolymer preferably has a number average molecular weight in the range of 10,000 to 50,000. If the number average molecular weight exceeds the above range, the viscosity increases and it tends to be difficult to eject from the nozzle.
[0046] Examples of commercially available products of the amino group-containing vinyl chloride-vinyl acetate-vinyl alcohol copolymer include SOLBIN TAO and SOLBIN TAOL (both from Nissin Chemical Industry Co., Ltd.).
[0047] In addition, within the range not impairing the effects brought about by the present invention, resins other than the above-mentioned acrylic resins, cellulose resins or vinyl chloride-vinyl acetate resins, such as vinyl chloride resins, vinyl chloride-acrylic resins, ethylene-vinyl acetate resins, styrene-acrylic resins, styrene-maleic acid resins, rosin resins, rosin ester resins, petroleum resins, coumarone-indene resins, terpene phenolic resins, phenolic resins, polyurethane resins, melamine resins, urea resins, epoxy resins, xylene resins, alkyd resins, aliphatic hydrocarbon resins, butyral resins, maleic acid resins, fumaric acid resins, etc. may also be used in combination.
[0048] Furthermore, especially when a resin other than vinyl chloride-vinyl acetate resin is used in combination, it is preferred to mix 1.0 to 15.0 parts by mass of the resin other than vinyl chloride-vinyl acetate resin with respect to 100 parts by mass of acrylic resin or vinyl chloride-vinyl acetate resin, and it is more preferred to mix 2.0 to 12.0 parts by mass, and it is further preferred to mix 3.0 to 10.0 parts by mass.
[0049] In addition, a cycloolefin resin may or may not be contained. In addition, the present invention has drying properties due to irradiation with specific energy rays, and does not contain a polymerizable monomer in the ink composition.
[0050] (Pigment dispersant) As the pigment dispersant that may be contained in the non-aqueous inkjet ink composition of the present invention, an ionic or nonionic surfactant or an anionic, cationic or nonionic polymer compound may be used.
[0051] Among them, preferred are polymer compounds, for example, carbodiimide compounds described in Japanese Patent Application Publication No. 2004-083872, International Publication No. 2003 / 076527, and International Publication No. 2004 / 000950, AJISPER PB821 and 822 (both from Ajinomoto Fine Chemicals Co., Ltd.) (acid value and amine value are both 10 to 20 mgKOH / g), SOLSPERSE 56000, SOLSPERSE 32000, and SOLSPERSE 39000 (all from Lubrizol), and DISPERBYK series (from BYK Chemical Co., Ltd.) as copolymers containing basic functional groups. These pigment dispersants can be used alone or in combination of two or more.
[0052] Among them, a copolymer containing a basic functional group having an amine value of 10.0 to 40.0 mgKOH / g is preferred.
[0053] The pigment dispersant may be appropriately selected and used depending on the type of the pigment and the type of the organic solvent used.
[0054] (Organic solvents) The organic solvent having an evaporation rate of 20 to 80 when the evaporation rate of butyl acetate is 100 in the present invention is obtained by the measurement method described in ASTM D3539-87, which is the evaporation time of n-butyl acetate and the evaporation time of the test solvent measured under the same conditions at 25° C. in dry air, and the evaporation rate value obtained by the following formula.
[0055] {(Time required for 90% by mass of n-butyl acetate to evaporate) / (Time required for 90% by mass of the test solvent to evaporate)}×100 The organic solvent having an evaporation rate of 20 to 80 when the evaporation rate of butyl acetate is 100 may be contained in the non-aqueous inkjet ink composition in an amount of 80.0% by mass or more. Further, it is preferably 82.0% by mass or more, and more preferably 84.0% by mass or more. In addition, it is preferably 93.0% by mass or less, and more preferably 90.0% by mass or less. When it is less than 80.0% by mass, it is necessary to further increase the heating temperature or extend the heating time in the drying process, which may deteriorate the printing layer of the lower layer.
[0056] The evaporation rate of each organic solvent contained in the non-aqueous inkjet ink composition of the present invention is preferably 75 or less, more preferably 70 or less, and even more preferably 50 or less, when the evaporation rate of butyl acetate is 100. In addition, it is preferably 25 or more, and more preferably 30 or more. Among them, the non-aqueous inkjet ink composition of the present invention preferably contains a solvent having an evaporation rate of 25 or more when the evaporation rate of butyl acetate is 100, and preferably contains only a solvent having an evaporation rate of 25 or more when the evaporation rate of butyl acetate is 100.
[0057] Preferred organic solvents include propylene glycol monomethyl ether acetate (evaporation rate 44), ethyl lactate (evaporation rate 22), propylene glycol monomethyl ether (evaporation rate 71), xylene (evaporation rate 68), tripropylamine (evaporation rate 20), mesitylene (evaporation rate 22), dibutyl ether (evaporation rate 43), nonane (evaporation rate 39), isobutyl alcohol (evaporation rate 64), 1-butanol (evaporation rate 47), ethylene glycol monomethyl ether (evaporation rate 53), ethylene glycol monoethyl ether (evaporation rate 38), 1-ethoxy-2-propanol (evaporation rate 34), and propylene glycol monopropyl ether (evaporation rate 22).
[0058] As long as the effects of the present invention are not impaired, other known organic solvents having an evaporation rate of less than 20 or exceeding 80 may or may not be used in combination.
[0059] Furthermore, alkylene glycol dialkyl ethers such as diethylene glycol diethyl ether, ethylene glycol monobenzyl ether or ethylene glycol monophenyl ether, 3-methoxybutanol, ethylene glycol monobutyl ether acetate, and ethylene glycol diacetate may or may not be contained.
[0060] (Other ingredients) Furthermore, various additives such as surfactants, plasticizers, surface conditioners, ultraviolet light blocking agents, light stabilizers, and antioxidants may be used in the non-aqueous inkjet ink composition of the present invention as necessary.
[0061] (Manufacture of non-aqueous inkjet ink composition) Next, a method for producing the non-aqueous inkjet ink composition of the present invention using these materials will be described.
[0062] The non-aqueous inkjet ink composition of the present invention can be obtained by, for example, dispersing and mixing using a disperser such as a wet circulation mill, a bead mill, a ball mill, a sand mill, an attritor, a roll mill, a DCP mill, a stirrer, a Henschel mixer, a colloid mill, an ultrasonic homogenizer, a high-pressure homogenizer (Micro fluidizer, Nanomizer, Ultimizer, Genus PY, DeBEE2000, etc.), or a Pearl Mill, and adjusting the viscosity of the non-aqueous inkjet ink composition to 2.0 to 10.0 mPa·s.
[0063] The total organic solvent content in the non-aqueous inkjet ink composition of the present invention is the amount obtained by deducting the total amount of the resin, pigment, pigment dispersant, and other additives used as required from the total amount of the ink composition, but is preferably appropriately changed so that the ink viscosity is within the above range.
[0064] The non-aqueous inkjet ink composition of the present invention thus obtained can be printed by a known inkjet printer. As its printing substrate, it can be a substrate on which a printed layer is formed in advance. In addition, it can also be a substrate on which a printed layer is not formed in advance. Among these, it can be used in the case where the substrate or the pre-formed printed layer is easily softened and shrunk by heating.
[0065] (use) The non-aqueous inkjet ink composition of the present invention can be used for known applications using a resin substrate as a printed surface. In addition, it can be used for applications using the surface of a printing portion formed in advance on a substrate surface composed of any material as a printed surface.
[0066] (Printing method) Using the non-aqueous inkjet ink composition of the present invention, after printing by the known inkjet printer shown above, infrared rays can be quickly irradiated for drying and curing. The printed substrate at this time can be any of resin, paper and metal. However, it can also be a material that is prone to wrinkling or deformation due to excessive heating of the printed substrate, preferably a resin substrate, wherein a thermoplastic resin substrate is more preferably used. When using a resin substrate, known resins such as polyolefin resins, polyvinyl chloride resins, polyvinyl alcohol resins, acrylic resins, polyester resins, and polyamide resins can be used. Since the irradiated infrared rays are absorbed by the carbon black contained in the non-aqueous inkjet ink composition of the present invention, the energy of the irradiated infrared rays can be effectively used for heating. If it is a color material other than carbon black, the energy of the irradiated infrared rays needs to be quite high, so that the possibility of excessive temperature rise of the resin substrate as the printed substrate increases.
[0067] At this time, infrared rays having a peak at 0.90 to 1.25 μm can be used as infrared rays. In this range, the wavelength is more preferably 1.00 μm or more, further preferably 1.05 μm or more, more preferably 1.20 μm or less, further preferably 1.15 μm or less.
[0068] The infrared irradiation time is preferably such that the printed non-aqueous inkjet ink composition is dried and cured, and the drying speed is not too slow relative to the printing speed based on the inkjet printer. In order to make the irradiation time in such a range dry and cure, the output power of the infrared ray is preferably above 2.0 kW.
[0069] In addition, it is preferred that the infrared light source is arranged at a distance as close as possible to the surface of the printed non-aqueous inkjet ink composition, and the distance is about 1.0 to 15.0 mm, and within this range, it can be 2.0 mm or more, 3.0 mm or more, 12.0 mm or less, or 10.0 mm or less.
[0070] If the intensity of the irradiated infrared light is too high, the temperature of the surface of the printed substrate may become too high when the printed substrate is a resin, which may cause damage such as wrinkles, distortion, and warping on the printed substrate surface.
[0071] Example The present invention is further described in detail with reference to the following examples, but the present invention is not limited to these examples. In addition, unless otherwise specified, "%" means "mass %" and "part" means "mass part".
[0072] The materials used in the following examples and comparative examples are as follows. All components other than the organic solvent are solid content.
[0073] The unit of the numerical values in the columns of each component and total in the table is "mass %".
[0074] <Carbon black> Bk7: Carbon black MA7 (Mitsubishi Chemical Corporation) <Black dye> Solvent Black 29: Orasol Black RLI (BASF) <Pigment dispersant> SOLSPERSE 32000 (Lubrizol) <Resin> DIANAL BR-83: Acrylic resin (Mitsubishi Rayon Co., Ltd.) SOLBIN TAO: Vinyl chloride-vinyl acetate-vinyl alcohol copolymer containing amino groups (Nissin Chemical Industry Co., Ltd.) (Examples 1 to 5, Comparative Examples 1 to 5, Reference Examples 1 to 4) <Production of non-aqueous inkjet ink composition> According to the formulation ratios in Tables 1 and 2 (the formulation ratio of each material is in mass %), each material was stirred and mixed to obtain a non-aqueous inkjet ink composition of each Example, each Comparative Example, and each Reference Example.
[0075] <Printing method> The non-aqueous inkjet ink composition of each example, each comparative example and each reference example was loaded into a commercially available inkjet printer and solid printed on a stretched polypropylene film (trade name P-2161, thickness 25 μm, Toyobo Co., Ltd.) in a high-speed printing mode. The printed portion was irradiated with infrared light having a peak at 1.10 μm and an output power of 2.3 to 7.5 kW for 0.1 second from a distance of 10 mm to dry and cure the printed matter of each example, each comparative example and each reference example.
[0076] The following characteristics were measured and evaluated for these printed products. In addition, evaluation of substrate damage was conducted in two ways: when printing was performed without printed data and when printing was performed with printed data already available.
[0077] <Discharge stability> A commercially available inkjet printer was used to perform solid printing in a high-speed printing mode using the ink composition of each Example, each Comparative Example, and each Reference Example. After the printing was left for 1 minute without ejection, the number of nozzle clogging when ejection was repeated was measured.
[0078] ○: All nozzles spray ×: One or more nozzles are clogged <Drying properties> The printed matter produced by the above method is rubbed in one direction with a cotton swab vertically raised and pressed, and the determination is made by observing whether ink is attached to the cotton swab.
[0079] ○: No ink adhesion ×: Ink adheres <Damage to substrate (no data on completed printing)> The evaluation piece prepared by the above method was judged by visually observing the change in the appearance.
[0080] ○: No change ×: Visible changes such as opening, wrinkles, and surface distortion <Damage to the substrate (with data after printing)> On the front half of the moving direction of an A4-sized substrate film (trade name P-2161, thickness 25 μm, Toyobo Co., Ltd.), a solid image was formed by gravure printing using a front-side gravure ink (Superior Ink ink, Sakata Ink Co., Ltd.) under the following conditions. Then, on the remaining half of the area, the non-aqueous inkjet ink composition of each example, comparative example, and reference example was printed under the above conditions and dried, and the appearance changes of the prepared evaluation pieces were visually observed for judgment.
[0081] ○: No change ×: Visible changes such as opening, wrinkles, and surface distortion (Gravure printing conditions) Base film: stretched polypropylene film (trade name P-2161, thickness 25 μm, Toyobo Co., Ltd.) Printing machine: Gravure printing correction machine Printing ink brush plate: Helio 175 lines / inch (pattern: solid printing plate) Printing speed: 80m / min Drying conditions: 80℃ [Table 1]
[0082] [Table 2]
[0083] According to each embodiment, the non-aqueous inkjet ink composition has excellent ejection stability and drying properties, and can exhibit an excellent effect of not damaging the substrate. In particular, when printing on a substrate with printed data that already has a printed layer formed of a black ink composition containing carbon black, the effect of being able to print without changing the appearance of the printed portion of the printed data is exhibited.
[0084] However, according to Comparative Example 1 in which the concentration of carbon black was low, the drying property was poor, and according to Comparative Example 2 in which the concentration of carbon black was high, the ejection stability was poor. Furthermore, according to Comparative Examples 3 and 4 in which the organic solvent of the present invention was not used, the drying property or ejection stability was poor. Moreover, according to Comparative Example 5 in which a black color material other than carbon black was used, the drying property was poor.
[0085] In addition, regarding Comparative Examples 1 and 3, which were poor in drying properties, when infrared ray irradiation was continued until the drying was completed, wrinkles and the like were generated on the printed base film due to heat.
[0086] Furthermore, in Reference Examples 1 to 4, which used the same substrate film as in the embodiment but used non-black pigments, the drying properties were poor in Reference Examples 1 to 4, in which the infrared irradiation intensity was changed respectively. In addition, in Reference Examples 3 and 4, in which the infrared irradiation intensity was high, even if the infrared irradiation intensity was not increased to a level that could fully dry, the substrate was greatly damaged, and wrinkles were formed on the substrate surface.
Claims
1. A non-aqueous inkjet ink composition for printing on a resin substrate, characterized in that: Contains 2.5 to 10.0 mass % of carbon black, Containing 80.0% by mass or more of an organic solvent having an evaporation rate of 20 to 80 when the evaporation rate of butyl acetate is 100, Contains resin, And it has drying properties based on infrared irradiation.
2. The non-aqueous inkjet ink composition according to claim 1, characterized in that: Used to print on a printing layer provided on a resin substrate.
3. The non-aqueous inkjet ink composition according to claim 1 or 2, characterized in that: The resin contained in the non-aqueous inkjet ink composition includes at least one selected from the group consisting of acrylic resins, cellulose resins, and vinyl chloride-vinyl acetate resins.
4. The non-aqueous inkjet ink composition according to claim 1 or 2, characterized in that: The organic solvent having an evaporation rate of 30 to 60 when the evaporation rate of butyl acetate is 100 is contained in an amount of 80.0% by mass or more.
5. A printing method based on a non-aqueous inkjet ink composition, characterized in that: use: Contains 2.5 to 10.0 mass % of carbon black, Containing 80.0% by mass or more of an organic solvent having an evaporation rate of 20 to 80 when the evaporation rate of butyl acetate is 100, A non-aqueous inkjet ink composition containing a resin, Inkjet printing is performed on a printed substrate made of resin and / or a printed portion pre-formed on the surface of the printed substrate. Drying is carried out by infrared irradiation.
Citation Information
Patent Citations
Processed organic pigment, use of the same, and compound for processing pigment
JP2004083872A
Non-aqueous inkjet ink
JP2018059106A
Treated pigment, use thereof, and compound for treating pigment
WO2003076527A1
Treated pigment, use thereof, and compound for pigment treatment
WO2004000950A1
Cited By
Weak solvent ink for ink-jet printer and preparation method of weak solvent ink
CN120137455A