Efficient cleaning roller and preparation method thereof

Through physical nesting and chemical bonding of polyvinyl formaldehyde-cellulose composite sponge with the stainless steel central axis, combined with silane coupling agent, the problems of insufficient water absorption capacity and environmental pollution of the existing cleaning roller are solved, and efficient and long-lasting Cleaning effect.

CN119073850APending Publication Date: 2024-12-06FULOMEI (SUZHOU) ULTRACLEAN TECHNOLOGY CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411508011.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-28
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

The existing cleaning drum has limited water absorption capacity and weak water retention capacity. It requires frequent squeeze and reabsorbing during use. It may contain chemical adhesives that are not friendly to the environment, affecting air quality and cleaning effect.

Method used

The polyvinyl formaldehyde-cellulose composite sponge is used to connect to the stainless steel central axis through physical nesting and chemical bonding. The silane coupling agent is used to enhance the water absorption and water retention ability of the sponge and reduce the use of glue.

Benefits of technology

It improves water absorption and water retention ability, reduces frequent water absorption operations, enhances cleaning efficiency and effect, and avoids environmental pollution and wipe marks.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119073850A_ABST
    Figure CN119073850A_ABST
Patent Text Reader

Abstract

The invention discloses an efficient cleaning roller and a preparation method thereof.The efficient cleaning roller comprises a center shaft, the center shaft is made of stainless steel, and a spiral groove is formed in the outer surface of the center shaft; the sponge layer is connected with the central shaft in a physical nesting and chemical bonding mode, and chemical bonding is achieved through a reaction between a solution containing a silane coupling agent and hydroxyl in sponge, and the solution is coated in the spiral groove of the central shaft in advance. According to the cleaning roller, the polyvinyl formal-cellulose composite sponge is adopted, cellulose in the composite sponge has a large number of hydrophilic groups, the water absorption capacity of the composite sponge can reach 10-12 times of the mass of the composite sponge, and the water absorption capacity is greatly improved. Meanwhile, the porous structure of the inner layer cellulose can store a large amount of water, and the polyvinyl formal of the outer layer can slow down evaporation of the water, so that the water retention capacity is improved. In the cleaning process, frequent water absorption operation is not needed, and the good cleaning effect can be continuously kept.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of cleaning equipment, in particular to a high-efficiency cleaning roller and a preparation method thereof. Background Art

[0002] Cleaning is an indispensable part of daily life and industrial production. As a common cleaning tool, cleaning roller is widely used in various scenarios such as floor cleaning and glass cleaning. It can effectively absorb dust, stains and liquids, etc., and improve cleaning efficiency and quality.

[0003] Through the study of relevant search cases, it is found that the existing cleaning rollers mainly have the following types and structures. A common cleaning roller is made of sponge alone, which is usually an ordinary polyurethane sponge. It has a simple structure and relatively low cost. However, this traditional cleaning roller has many problems.

[0004] Ordinary polyurethane sponges have limited water absorption capacity, and their water absorption capacity can only reach 3-5 times their own weight. During the cleaning process, especially for large-area water stains, they need to be squeezed and re-absorbed frequently, which greatly reduces the cleaning efficiency. Moreover, their water retention capacity is also weak, and water is easily lost quickly during use, resulting in a short-lasting cleaning effect.

[0005] In the manufacturing process of some cleaning rollers, a large amount of chemical adhesives are used to fix the sponge or connect the sponge to other parts. These adhesives may contain volatile organic compounds (VOCs), which will be released into the environment during use and have a negative impact on indoor air quality. In addition, some sponges may use some environmentally unfriendly raw materials or additives during the production process.

[0006] When ordinary sponges are dry and come into contact with cleaning liquids (such as water or cleaning solutions), their wetting rate is slow. This means that at the beginning of cleaning, the sponge cannot absorb the liquid quickly, thus affecting the timeliness and effectiveness of cleaning. For example, when cleaning a glass surface, if the sponge cannot soak quickly, it will be difficult to quickly dissolve and absorb the stains on the glass surface, and may leave wiping marks. Summary of the invention

[0007] The object of the present invention is to provide a high-efficiency cleaning roller and a preparation method thereof to solve the problems raised in the above background technology.

[0008] To achieve the above object, the present invention provides the following technical solutions:

[0009] A high-efficiency cleaning roller, comprising

[0010] A central shaft, the central shaft is made of stainless steel and has a spiral groove on its outer surface;

[0011] The sponge layer is connected to the central axis by physical nesting and chemical bonding. The chemical bonding is achieved by reacting a solution containing a silane coupling agent pre-coated in the spiral groove of the central axis with hydroxyl groups in the sponge.

[0012] In the present invention, the spiral groove has a depth of 1-3 mm, a width of 2-5 mm, and a spacing between adjacent spirals of 5-10 mm.

[0013] In the present invention, the sponge layer is a polyvinyl formal-cellulose composite sponge, and the sponge layer includes an outer layer and an inner layer. The outer layer is polyvinyl formal with a thickness of 0.5-5 mm, and the inner layer is cellulose with a thickness of 1-8 mm.

[0014] In the present invention, the silane coupling agent is γ-aminopropyltriethoxysilane, and the solution containing the silane coupling agent is an ethanol solution with a mass fraction of 5%-10%.

[0015] In the present invention, the water absorption capacity of the composite sponge is 10-12 times of its own weight, the cellulose is used to store a large amount of water, and the polyvinyl formal is used to slow down the evaporation of water to improve the water retention capacity.

[0016] In the present invention, the polyvinyl formal is a polyvinyl formal with low formaldehyde content, which is prepared by reacting polyvinyl alcohol with a polymerization degree of 1500-2000 and an alcoholysis degree of 90 mol%-95 mol% with formaldehyde under acidic conditions, the reaction temperature is 50-60°C, and the reaction time is 2-3 hours.

[0017] In the present invention, the cellulose has a regular pore structure, and the surface of the polyvinyl formal has a micro-nano structure.

[0018] A method for preparing a high-efficiency cleaning roller includes the steps of preparing raw materials:

[0019] Step S101, preparation of polyvinyl formal raw material: selecting polyvinyl alcohol with a degree of polymerization of 1500-2000 and a degree of alcoholysis of 90 mol%-95 mol%, reacting with formaldehyde under acidic conditions, controlling the reaction temperature to 50-60°C, and the reaction time to 2-3 hours, to obtain polyvinyl formal with low formaldehyde content;

[0020] Step S102, preparation of cellulose raw material: using pretreated cellulose fibers, wherein the pretreatment process includes soaking in a sodium hydroxide solution for 1-2 hours, then washing with clean water, and drying for later use;

[0021] Step S103, preparation of a silane coupling agent solution: selecting γ-aminopropyltriethoxysilane and preparing it into an ethanol solution with a mass fraction of 5%-10%.

[0022] The present invention also includes the steps of preparing the sponge layer:

[0023] Step S201, firstly, dispersing the pretreated cellulose fibers in water to form a cellulose suspension with a mass fraction of 10%-20%, adding sodium carboxymethyl cellulose as a thickener, wherein the amount of the sodium carboxymethyl cellulose is 1%-3% of the mass of the cellulose, and stirring evenly;

[0024] Step S202, dissolving polyvinyl formal with low formaldehyde content in water to form a solution with a mass fraction of 20%-30%, then mixing the polyvinyl formal solution with the cellulose suspension in a volume ratio of 1:1-1:2, adding sodium dodecyl sulfate as a surfactant, the amount of which is 0.5%-1% of the mass of the mixed solution, and sodium bicarbonate as a foaming agent, the amount of which is 1%-2% of the mass of the mixed solution, and stirring at a high speed to foam;

[0025] Step S203, pouring the foamed mixed solution into a mold, and curing it at 60-80° C. for 2-3 hours to obtain a composite sponge.

[0026] The present invention further includes the step of assembling a cleaning roller:

[0027] Step S301, uniformly coating the silane coupling agent solution prepared in step S103 in the spiral groove of the central axis and drying it;

[0028] Step S302, sleeve the composite sponge prepared in step S203 on the central axis, and keep it at a pressure of 0.1-0.3 MPa for 1-2 hours to allow the silane coupling agent to fully react with the hydroxyl groups in the sponge, thereby completing the assembly of the cleaning roller.

[0029] Compared with the prior art, the present invention has the following beneficial effects:

[0030] 1. The cleaning roller of the present invention adopts a polyvinyl formal-cellulose composite sponge. The cellulose in the composite sponge has a large number of hydrophilic groups, and its water absorption capacity can reach 10-12 times of its own weight, which greatly improves the water absorption capacity. At the same time, the porous structure of the inner layer of cellulose can store a large amount of water, and the polyvinyl formal of the outer layer can slow down the evaporation of water, thereby improving the water retention capacity. During the cleaning process, there is no need for frequent water absorption operations, and a good cleaning effect can be maintained continuously;

[0031] 2. The sponge layer of the present invention is connected to the central axis by physical nesting and chemical bonding. A layer of solution containing a silane coupling agent is pre-coated in the spiral groove of the central axis. When the sponge layer is sleeved on the central axis, the silane coupling agent reacts with the hydroxyl group in the sponge to form a chemical bond, thereby avoiding the use of glue and reducing pollution to the environment.

[0032] 3. The inner cellulose layer of the composite sponge of the present invention has a rich porous structure, and the outer polyvinyl formal layer has been specially treated, and the surface has a micro-nano structure, which can greatly improve the infiltration rate of the sponge. When the cleaning roller contacts the cleaning liquid, it can start to absorb water instantly. Whether it is cleaning the ground or glass, it can quickly dissolve and absorb stains, improve the timeliness and effect of cleaning, and avoid leaving wiping marks. BRIEF DESCRIPTION OF THE DRAWINGS

[0033] Figure 1 This is a schematic diagram of the central axis structure of a high-efficiency cleaning roller of the present invention;

[0034] Figure 2 This is a schematic diagram of the sponge layer structure of a high-efficiency cleaning roller of the present invention;

[0035] Figure 3 A schematic diagram of a raw material preparation process of a method for preparing a high-efficiency cleaning roller according to the present invention;

[0036] Figure 4 It is a schematic diagram of the sponge layer preparation process of a method for preparing a high-efficiency cleaning roller of the present invention;

[0037] Figure 5 The present invention is a schematic diagram of a cleaning roller assembly process of a method for preparing a high-efficiency cleaning roller.

[0038] In the figure: 1, central axis; 2, sponge layer; 3, spiral groove; 4, outer layer; 5, inner layer. DETAILED DESCRIPTION

[0039] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0040] See also Figure 1-2 , the present invention provides a technical solution:

[0041] A high-efficiency cleaning roller comprises a central shaft 1, which is made of stainless steel and has a spiral groove 3 on its outer surface; a sponge layer 2, which is connected to the central shaft 1 by physical nesting and chemical bonding, wherein the chemical bonding is achieved by reacting a solution containing a silane coupling agent pre-coated in the spiral groove 3 of the central shaft 1 with a hydroxyl group in the sponge. The spiral groove 3 has a depth of 1-3 mm, a width of 2-5 mm, and a spacing of 5-10 mm between adjacent spirals. The sponge layer 2 is a polyvinyl formal-cellulose composite sponge, and comprises an outer layer 4 and an inner layer 5, wherein the outer layer 4 is polyvinyl formal with a thickness of 0.5-5 mm, and the inner layer 5 is cellulose with a thickness of 1-8 mm. The silane coupling agent is γ-aminopropyltriethoxysilane, and the solution containing the silane coupling agent is an ethanol solution with a mass fraction of 5%-10%. The composite sponge absorbs 10-12 times its own weight, the cellulose is used to store a large amount of water, and the polyvinyl formal is used to slow down water evaporation to improve water retention capacity. The polyvinyl formal is a polyvinyl formal with low formaldehyde content, which is prepared by reacting polyvinyl alcohol with a polymerization degree of 1500-2000 and a degree of alcoholysis of 90mol%-95mol% with formaldehyde under acidic conditions, the reaction temperature is 50-60°C, and the reaction time is 2-3 hours. The cellulose has a regular pore structure, and the surface of the polyvinyl formal has a micro-nano structure.

[0042] In this embodiment, the cleaning roller of the present invention adopts a polyvinyl formal-cellulose composite sponge. The cellulose in the composite sponge has a large number of hydrophilic groups, and its water absorption capacity can reach 10-12 times of its own mass, which greatly improves the water absorption capacity. At the same time, the porous structure of the cellulose in the inner layer 5 can store a large amount of water, and the polyvinyl formal in the outer layer 4 can slow down the evaporation of water, thereby improving the water retention capacity. During the cleaning process, there is no need for frequent water absorption operations, and a good cleaning effect can be continuously maintained.

[0043] Specifically, the sponge layer 2 is connected to the central axis 1 by physical nesting and chemical bonding. A layer of solution containing a silane coupling agent is pre-coated in the spiral groove 3 of the central axis 1. When the sponge layer 2 is put on the central axis 1, the silane coupling agent will react with the hydroxyl group in the sponge to form a chemical bond, thereby avoiding the use of glue and reducing pollution to the environment.

[0044] like Figure 3-5 As shown, a method for preparing a high-efficiency cleaning roller includes the steps of preparing raw materials:

[0045] Step S101, preparation of polyvinyl formal raw material: selecting polyvinyl alcohol with a degree of polymerization of 1500-2000 and a degree of alcoholysis of 90 mol%-95 mol%, reacting with formaldehyde under acidic conditions, controlling the reaction temperature to 50-60°C, and the reaction time to 2-3 hours, to obtain polyvinyl formal with low formaldehyde content;

[0046] Step S102, preparation of cellulose raw material: using pretreated cellulose fibers, wherein the pretreatment process includes soaking in a sodium hydroxide solution for 1-2 hours, then washing with clean water, and drying for later use;

[0047] Step S103, preparation of a silane coupling agent solution: selecting γ-aminopropyltriethoxysilane and preparing it into an ethanol solution with a mass fraction of 5%-10%.

[0048] The sponge layer preparation steps are also included:

[0049] Step S201, firstly, dispersing the pretreated cellulose fibers in water to form a cellulose suspension with a mass fraction of 10%-20%, adding sodium carboxymethyl cellulose as a thickener, wherein the amount of the sodium carboxymethyl cellulose is 1%-3% of the mass of the cellulose, and stirring evenly;

[0050] Step S202, dissolving polyvinyl formal with low formaldehyde content in water to form a solution with a mass fraction of 20%-30%, then mixing the polyvinyl formal solution with the cellulose suspension in a volume ratio of 1:1-1:2, adding sodium dodecyl sulfate as a surfactant, the amount of which is 0.5%-1% of the mass of the mixed solution, and sodium bicarbonate as a foaming agent, the amount of which is 1%-2% of the mass of the mixed solution, and stirring at a high speed to foam;

[0051] Step S203, pouring the foamed mixed solution into a mold, and curing it at 60-80° C. for 2-3 hours to obtain a composite sponge.

[0052] Further comprising the steps of cleaning the roller assembly:

[0053] Step S301, uniformly coating the silane coupling agent solution prepared in step S103 in the spiral groove 3 of the central axis 1, and drying;

[0054] Step S302, sleeve the composite sponge prepared in step S203 on the central shaft 1, and keep it at a pressure of 0.1-0.3 MPa for 1-2 hours to allow the silane coupling agent to fully react with the hydroxyl groups in the sponge, thereby completing the assembly of the cleaning roller.

[0055] In this embodiment, in the preparation process of the cleaning roller of the present invention, a polyvinyl alcohol formal raw material with low formaldehyde content is used, and by optimizing the reaction conditions, the free formaldehyde content in the final product is lower than the national standard. In addition, the cellulose in the inner layer 5 of the composite sponge has a rich pore structure, and the polyvinyl alcohol formal in the outer layer 4 is specially treated, and the surface has a micro-nano structure, which can greatly improve the infiltration rate of the sponge. When the cleaning roller contacts the cleaning liquid, it can start to absorb water instantly. Whether it is cleaning the ground or the surface of glass, it can quickly dissolve and absorb the stains, improve the timeliness and effect of cleaning, and avoid leaving wiping marks.

[0056] It should be noted that, in this article, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variants thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device.

[0057] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. A high-efficiency cleaning roller, characterized by: include A central shaft, the central shaft is made of stainless steel and has a spiral groove on its outer surface; The sponge layer is connected to the central axis by physical nesting and chemical bonding. The chemical bonding is achieved by reacting a solution containing a silane coupling agent pre-coated in the spiral groove of the central axis with hydroxyl groups in the sponge.

2. The high-efficiency cleaning roller according to claim 1, characterized in that: The spiral groove has a depth of 1-3 mm, a width of 2-5 mm, and a spacing between adjacent spirals of 5-10 mm.

3. The high-efficiency cleaning roller according to claim 1, characterized in that: The sponge layer is a polyvinyl formal-cellulose composite sponge, and comprises an outer layer and an inner layer. The outer layer is polyvinyl formal with a thickness of 0.5-5 mm, and the inner layer is cellulose with a thickness of 1-8 mm.

4. The high-efficiency cleaning roller according to claim 1, characterized in that: The silane coupling agent is gamma-aminopropyltriethoxysilane, and the solution containing the silane coupling agent is an ethanol solution with a mass fraction of 5%-10%.

5. The high-efficiency cleaning roller according to claim 3, characterized in that: The water absorption capacity of the composite sponge is 10-12 times of its own weight. The cellulose is used to store a large amount of water, and the polyvinyl formal is used to slow down water evaporation to improve water retention capacity.

6. The high-efficiency cleaning roller according to claim 3, characterized in that: The polyvinyl formal is a polyvinyl formal with low formaldehyde content, which is prepared by reacting polyvinyl alcohol with a polymerization degree of 1500-2000 and an alcoholysis degree of 90 mol%-95 mol% with formaldehyde under acidic conditions, the reaction temperature is 50-60°C, and the reaction time is 2-3 hours.

7. The high-efficiency cleaning roller according to claim 3, characterized in that: The cellulose has a regular pore structure, and the surface of the polyvinyl formal has a micro-nano structure.

8. The method for preparing a high-efficiency cleaning roller according to claim 1, characterized in that: Including raw material preparation steps: Step S101, preparation of polyvinyl formal raw material: selecting polyvinyl alcohol with a degree of polymerization of 1500-2000 and a degree of alcoholysis of 90 mol%-95 mol%, reacting it with formaldehyde under acidic conditions, controlling the reaction temperature to 50-60°C, and the reaction time to 2-3 hours to obtain polyvinyl formal with low formaldehyde content; Step S102, preparation of cellulose raw material: using pretreated cellulose fibers, wherein the pretreatment process includes soaking in a sodium hydroxide solution for 1-2 hours, then washing with clean water, and drying for later use; Step S103, preparation of a silane coupling agent solution: selecting γ-aminopropyltriethoxysilane and preparing it into an ethanol solution with a mass fraction of 5%-10%.

9. The method for preparing a high-efficiency cleaning roller according to claim 8, characterized in that: Also included are the steps for preparing the sponge layer: Step S201: first, pretreated cellulose fibers are dispersed in water to form a cellulose suspension with a mass fraction of 10% to 20%, sodium carboxymethyl cellulose is added as a thickener, and the amount of sodium carboxymethyl cellulose is 1% to 3% of the mass of the cellulose, and the mixture is stirred evenly; Step S202: dissolving polyvinyl formal with a low formaldehyde content in water to form a solution with a mass fraction of 20%-30%, then mixing the polyvinyl formal solution with a cellulose suspension in a volume ratio of 1:1-1:2, adding sodium lauryl sulfate as a surfactant in an amount of 0.5%-1% by mass of the mixed solution, and sodium bicarbonate as a foaming agent in an amount of 1%-2% by mass of the mixed solution, and stirring at high speed to foam; Step S203 , pouring the foamed mixed liquid into a mold, and curing it at 60-80° C. for 2-3 hours to obtain a composite sponge.

10. The method for preparing a high-efficiency cleaning roller according to claim 9, characterized in that: Further includes cleaning roller assembly steps: Step S301, uniformly coating the silane coupling agent solution prepared in step S103 in the spiral groove of the central axis and drying it; Step S302 , sleeve the composite sponge prepared in step S203 on the central shaft and maintain the pressure at 0.1-0.3 MPa for 1-2 hours to allow the silane coupling agent to fully react with the hydroxyl groups in the sponge, thereby completing the assembly of the cleaning roller.

Citation Information

Cited By

  • Suction nozzle assembly of sanitation vehicle and sanitation vehicle

    CN119465844A