Flexible dry electrode and preparation method thereof
By constructing a flexible dry electrode with a layered structure on a titanium foil, and using DC electrodeposition and anodization reaction to form a nanoenzyme film, the problem of insufficient contact impedance and signal correlation of existing EEG signal acquisition electrodes is solved, and high efficiency is achieved , stable EEG signal acquisition and long-term monitoring.
Patent Information
- Application Number
- CN202411167582.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-23
- Publication Date
- 2024-12-06
AI Technical Summary
The existing EEG signal acquisition electrodes have high contact impedance, low signal correlation and insufficient signal stability, which limits the long-term reliability and quality of EEG monitoring.
Iridium nanoparticles were deposited on titanium foils by DC electrodeposition, anodizing reaction was carried out to form a titanium dioxide nanotube array, and a nanoenzyme film was formed on it to construct a flexible dry electrode with a layered structure to improve biocompatibility and electrocatalytic performance.
It realizes low contact impedance, stable and reliable EEG signal acquisition, reduces impedance with the scalp, is suitable for long-term EEG monitoring, and does not require conductive paste, which improves signal correlation and acquisition effect.
Smart Images

Figure CN119073999A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of flexible dry electrodes, and in particular relates to a flexible dry electrode and a preparation method thereof. Background Art
[0002] The brain is the center of the human body that controls various physiological and psychological activities and has a complex neural network. Its functions cover thinking, perception, movement and many other aspects. Bioelectric signals are the way neurons transmit information through electrochemical processes. Expanding brain functions means in-depth understanding and optimization of thinking, learning, memory and other aspects, and the exploration of bioelectric signals can promote the development of brain-computer interface technology and open up new possibilities for brain science and neural engineering. This research history can be traced back to the early 20th century and was first recorded by German neuroscientist Hans Baer in 1924. At first, electroencephalogram (EEG) was mainly used to study neurological diseases such as epilepsy, but with the advancement of technology, its application areas have gradually expanded to cognitive neuroscience, psychology, neural engineering and many other fields. Since then, EEG signals have attracted widespread attention.
[0003] Electroencephalography (EEG) is now the most widely used method in human brain research. It is used to capture the overall reflection of the electrophysiological activity of brain nerve cells on the cerebral cortex or scalp surface. This technology has been applied to the diagnosis and treatment of some brain diseases and has made important progress in the field of brain-computer interface (BCI) that has attracted much attention in recent years. In EEG monitoring, EEG electrodes play an important role.
[0004] Portable EEG devices have shown high application value in the judgment and monitoring of neurological diseases, neuroscience cognitive research, human fatigue detection, and brain-computer interface. However, in the environment of a non-shielded room, EEG signals usually face a variety of problems such as power frequency interference and motion artifacts, which may have a negative impact on the quality of EEG signals and the promotion of EEG applications. Therefore, one of the key factors to solve these problems is the optimization of EEG acquisition electrodes. The traditional electrode for EEG signal acquisition is Ag / AgCl electrode, also known as wet electrode. Its use requires the addition of gel-like conductive paste as an intermediate medium. Due to its complex operation process, poor comfort, and unsuitable for long-term measurement, the experiment is limited. Therefore, a new type of flexible nanomaterial EEG dry electrode is developed, which has the advantages of accurate and stable measurement results, convenience and speed, no need to use conductive paste, comfortable to wear, and suitable for daily long-term EEG monitoring. It has extremely important research significance for medical and brain-computer interface fields.
[0005] Compared with traditional electrodes, dry electrodes do not require the use of gel or conductive paste, which improves user comfort and makes long-term EEG signal acquisition more feasible. At the same time, dry electrodes are easier to wear and carry, which helps to realize the application of brain-computer interface technology in daily life. By adopting a more stable design, dry electrodes reduce the possibility of falling off, making the brain-computer interface system more reliable. This helps to promote the development of brain-computer interface technology and provide a positive driving force for the development of more advanced brain control applications (such as brain-controlled prostheses, brain-computer interactive games, etc.). Due to the comfort and stability of dry electrodes, they provide the possibility for long-term and long-term EEG monitoring, which is of great value for studying daily fluctuations in brain activity, long-term cognitive changes, etc.
[0006] Although flexible dry electrodes have shown advantages such as comfort and ease of use in many applications, existing technologies still have some problems, such as high contact impedance and low signal correlation. In addition, the signal stability and long-term reliability of these electrodes are often problems. Summary of the invention
[0007] In view of the deficiencies in the prior art, an object of the present invention is to provide a flexible dry electrode.
[0008] Another object of the present invention is to provide a method for preparing a flexible dry electrode, which uses a direct current electrodeposition method to deposit iridium nanoparticles as a first iridium nanolayer on a titanium foil (flexible substrate), keep the temperature, obtain a first iridium-plated titanium foil, and then perform an anodization reaction to prepare a titanium dioxide nanotube array on the first iridium-plated titanium foil, keep the temperature, and then deposit iridium nanoparticles as a second iridium nanolayer to obtain a second iridium-plated titanium foil. Finally, the second iridium-plated titanium foil is placed in a nanozyme solution to form a nanozyme film on the second iridium-plated titanium foil to obtain a flexible dry electrode with improved biocompatibility and electrocatalysis.
[0009] The purpose of the present invention is achieved through the following technical solutions.
[0010] A flexible dry electrode has a layered structure, which is composed of a nanozyme film, a second iridium nanolayer, a titanium dioxide nanotube array, a first iridium nanolayer and a flexible substrate from top to bottom. The nanozyme film includes amino graphene quantum dots loaded with copper single atoms.
[0011] In the above technical solution, the flexible substrate is a titanium foil.
[0012] A method for preparing a flexible dry electrode comprises the following steps:
[0013] Step 1, connecting the titanium foil to the negative electrode of a direct current power supply, connecting the first platinum sheet to the positive electrode of the direct current power supply, placing the titanium foil and the first platinum sheet in a first electrodeposition solution, starting the direct current power supply so that the titanium foil serves as a working electrode and the first platinum sheet serves as a counter electrode, reacting for 50 to 60 minutes at room temperature and stirring the first electrodeposition solution, so that iridium nanoparticles are electrodeposited on the titanium foil as a first iridium nanolayer, and washing to obtain a first iridium-plated titanium foil precursor, wherein the first electrodeposition solution comprises: iridium trichloride, potassium oxalate and water;
[0014] In step 1, the concentration of iridium trichloride in the first electrodeposition solution is 0.64-0.96 mmol / L, and the concentration of potassium oxalate in the first electrodeposition solution is 6.4-9.6 mmol / L.
[0015] In step 1, the pH of the first electrodeposition solution is 10.2-10.5.
[0016] In the above technical solution, a potassium carbonate aqueous solution is used to adjust the pH of the first electrodeposition solution, and the concentration of potassium carbonate in the potassium carbonate aqueous solution is 5 to 5.2 mmol / L.
[0017] In step 1, the stirring speed is 120-150 r / min.
[0018] In step 1, the output voltage of the DC power supply is 0.8-1.0V, and the current of the DC power supply is 0.1-0.12A.
[0019] Step 2, placing the first iridium-plated titanium foil precursor in a muffle furnace, keeping the temperature at 500-600° C. for 30-40 minutes, and cooling to room temperature to obtain a first iridium-plated titanium foil;
[0020] In step 2, the temperature is raised to 500-600° C. at a rate of 4-5° C. / min.
[0021] Step 3, connecting the first iridium-coated titanium foil to the positive electrode of a direct current power supply, connecting the second platinum sheet to the negative electrode of the direct current power supply, immersing the first iridium-coated titanium foil and the second platinum sheet in a first reaction solution at room temperature, starting the direct current power supply so that the first iridium-coated titanium foil serves as a working electrode and the second platinum sheet serves as a counter electrode, reacting for 60 to 90 minutes under stirring the first reaction solution, so that an anodic oxidation reaction occurs on the first iridium-coated titanium foil to obtain a vertical titanium dioxide nanotube array, and washing to obtain a first iridium-coated titanium foil precursor after anodization;
[0022] In step 3, the first reaction liquid is a mixture of glycerol, water and ammonium fluoride, and the ratio of the volume fraction of the glycerol, the volume fraction of the water in step 3 and the mass fraction of ammonium fluoride is 35:5:0.45, the unit of the volume fraction is mL, and the unit of the mass fraction is g.
[0023] In step 3, the output voltage of the DC power supply is 15-15.5V, and the current of the DC power supply is 110-115mA.
[0024] In step 3, the stirring speed is 600-700 r / min.
[0025] Step 4, placing the anodized first iridium-plated titanium foil precursor in a muffle furnace, keeping the temperature at 500-600° C. for 150-200 min, and cooling to room temperature to obtain an anodized first iridium-plated titanium foil;
[0026] In step 4, the temperature is raised to 500-600° C. at a rate of 5-7° C. / min.
[0027] Step 5, connecting the first iridium-plated titanium foil after anodization to the negative electrode of a direct current power supply, connecting the third platinum sheet to the positive electrode of the direct current power supply, placing the first iridium-plated titanium foil after anodization and the third platinum sheet in a second electrodeposition solution, starting the direct current power supply, so that the first iridium-plated titanium foil is used as a working electrode and the third platinum sheet is used as a counter electrode, reacting for 80 to 90 minutes at room temperature and stirring the second electrodeposition solution, so that iridium nanoparticles are electrodeposited on the first iridium-plated titanium foil after anodization as a second iridium nanolayer, washing, and obtaining a second iridium-plated titanium foil, wherein the second electrodeposition solution comprises: iridium trichloride, potassium oxalate and water;
[0028] In step 5, the concentration of iridium trichloride in the second electrodeposition solution is 0.64-0.96 mmol / L, and the concentration of potassium oxalate in the second electrodeposition solution is 6.4-9.6 mmol / L.
[0029] In step 5, the pH of the second electrodeposition solution is 10.2-10.5.
[0030] In the above technical solution, a potassium carbonate aqueous solution is used to adjust the pH of the second electrodeposition solution, and the concentration of potassium carbonate in the potassium carbonate aqueous solution is 5 to 5.2 mmol / L.
[0031] In step 5, the second electrodeposition solution is the same as the first electrodeposition solution.
[0032] In step 5, the output voltage of the DC power supply is 15-15.5V, and the current of the DC power supply is 150-160mA.
[0033] In step 5, the stirring speed is 250-300 r / min.
[0034] Step 6, under light-proof conditions, immerse the second iridium-coated titanium foil in an acidic nanozyme solution for 48 to 72 hours, form a nanozyme film on the second iridium-coated titanium foil, take it out, and dry it to obtain a flexible dry electrode, wherein the nanozyme solution includes: high-copper-loaded single-atom nanozyme (high-copper-loaded single-atom nanozyme is amino-modified graphene quantum dots loaded with copper single atoms), and the concentration of high-copper-loaded single-atom nanozyme in the nanozyme solution is 7 to 10 mmol / L.
[0035] In step 6, the pH value of the nanozyme solution is 5.4-5.6.
[0036] In step 6, the method for preparing the high-copper-loaded single-atom nanozyme comprises the following steps:
[0037] S1, mixing an aqueous solution of aminated graphene quantum dots with a concentration of 0.8 to 1.5 mg / mL and an aqueous solution of a Cu source with a concentration of 4 to 7 mg / mL until uniform, ultrasonicating at room temperature for 15 to 20 min, and freeze-drying to obtain a first powder, wherein the ratio of the mass fraction of the aminated graphene quantum dots to the molar fraction of Cu in the Cu source is 30:(0.01 to 0.05), the unit of the mass fraction is mg, and the unit of the molar fraction is mmol;
[0038] S2, mixing the first powder and urea, grinding until uniform, and calcining at 500-600° C. for 2-2.5 hours under an inert gas atmosphere to obtain the high-copper-loaded single-atom nanozyme. In terms of mass fractions, the ratio of the first powder to urea is 1:(8-12).
[0039] In S1, the freeze drying is performed by freezing in liquid nitrogen for 15 to 30 minutes.
[0040] In S1, the Cu source is CuCl2.
[0041] Compared with the prior art, the present invention has the following beneficial effects:
[0042] 1. The operation of the present invention is simple and the manufacturing cost is very low. After the flexible dry electrode is prepared, it can be directly used for EEG testing without any processing. It is suitable for long-term EEG monitoring experiments. Due to the good cost control, it is suitable for mass production in enterprises. Compared with wet electrodes and semi-dry electrodes, the flexible dry electrode of the present invention can be directly fixed at the target position, and the EEG equipment can be turned on for direct collection. The operation is very simple and does not require conductive paste, physiological saline and other intermediate media to help signal collection. There is no need for cumbersome operations such as adding conductive paste in the middle, and there will be no crosstalk between adjacent electrodes due to excessive conductive paste.
[0043] 2. The flexible dry electrode of the present invention is safe, reliable and comfortable, and has high biocompatibility. During the entire test process, the subject will not feel discomfort when the flexible dry electrode contacts the scalp. The flexible dry electrode of the present invention is more durable.
[0044] 3. The present invention utilizes the biocompatibility of nanozyme biopolymers, liquid adsorption characteristics and high catalytic properties to replace conductive paste to realize the electron transmission channel between the flexible dry electrode and the surface of the scalp, and realizes EEG signal collection in a completely dry environment, thereby improving the current conversion rate, thereby greatly reducing the contact impedance between the flexible dry electrode and the scalp. Compared with other similar dry electrodes, the flexible dry electrode of the present invention has a lower average impedance, which fully meets the requirements of EEG testing for contact impedance.
[0045] 4. The EEG signals collected by the present invention are stable and reliable. The flexible dry electrode can be used in EEG collection tests under different EEG paradigms. The collection effect is close to that of traditional wet electrodes. Therefore, the flexible dry electrode of the present invention can easily collect EEG signals with the same quality and reliability as traditional wet electrodes, providing convenient and reliable conditions for characteristic analysis of EEG signals. BRIEF DESCRIPTION OF THE DRAWINGS
[0046] Figure 1 This is the appearance photo of the stamping die;
[0047] Figure 2 a is the SEM of titanium foil roll, Figure 2 b is the SEM of titanium foil;
[0048] Figure 3 a is a SEM image of the first iridium-coated titanium foil at 2000 times magnification. Figure 3 b is a SEM of the first iridium-coated titanium foil at 5000 times magnification;
[0049] Figure 4 This is a 5000x magnified SEM of the first iridium-coated titanium foil after anodization;
[0050] Figure 5 This is the SEM of the second iridium-coated titanium foil;
[0051] Figure 6 This is the SEM of the flexible dry electrode;
[0052] Figure 7 TEM of a flexible dry electrode;
[0053] Figure 8 XPS of flexible dry electrode;
[0054] Fig. 9 Impedance data for the third conventional wet electrode and the flexible dry electrode;
[0055] Fig.10 This is a comparison chart of the waveforms of open and closed eyes;
[0056] Fig.11 This is a comparison chart of blink waveforms;
[0057] Fig.12 This is a comparison chart of the teeth biting waveform;
[0058] Fig.13 The frequency impedance diagrams of the titanium foil, the first iridium-plated titanium foil, the first iridium-plated titanium foil after anodization, and the flexible dry electrode prepared in Example 1;
[0059] Fig.14 The Nyquist plots of the titanium foil, the first iridium-plated titanium foil, the first iridium-plated titanium foil after anodization, and the flexible dry electrode prepared in Example 1;
[0060] Fig.15 This is the correlation diagram of eye opening signals between flexible dry electrodes and traditional wet electrodes;
[0061] Fig.16 This is the correlation diagram of eye closing signal between flexible dry electrode and traditional wet electrode;
[0062] Fig.17 This is the correlation diagram of the blink signal between the flexible dry electrode and the traditional wet electrode;
[0063] Fig.18 This is the correlation diagram of the tooth biting signal between the flexible dry electrode and the traditional wet electrode. DETAILED DESCRIPTION
[0064] The technical solution of the present invention is further described below in conjunction with specific embodiments.
[0065] The sources of the drugs involved in the following embodiments are as follows:
[0066] Potassium oxalate: content not less than 99.0%, manufacturer: Tianjin Zhonglian Chemical Reagent Co., Ltd.;
[0067] Iridium trichloride: content not less than 52.0%, manufacturer: Tianjin Damao Chemical Reagent Factory;
[0068] Glycerol: content not less than 99.0%, manufacturer: Tianjin Benchmark Chemical Reagent Co., Ltd.;
[0069] Ammonium fluoride: content not less than 98.0%, manufacturer: Tianjin Kewei Co., Ltd.;
[0070] Tris-HCl buffer solution: purchased from Shanghai Aladdin Biochemical Technology Co., Ltd.;
[0071] Anhydrous ethanol: Tianjin Huihang Chemical Technology Co., Ltd.;
[0072] Titanium foil roll: 0.1mm*200mm*1m, manufacturer: Haiyuan Scientific Research Metal;
[0073] Potassium carbonate (anhydrous potassium carbonate): content not less than 99.0%, manufacturer: Tianjin Zhonglian Chemical Reagent Co., Ltd.;
[0074] Platinum sheet: 10*20*0.1mm, manufacturer: Omiko Electrochemical.
[0075] The sources of the experimental instruments and equipment involved in the following embodiments are as follows:
[0076] Programmable linear DC power supply: Product model: DP832A, manufacturer: RIGOL;
[0077] Brain-computer interface system: Product model: Grael 4K EEG Amplifier, Manufacturer: AustraliaCorpo-rateHQ;
[0078] Electrochemical analyzer: Product model: CHI660E, manufacturer: Shanghai Chenhua Instrument Co., Ltd.;
[0079] Electronic balance (d = 0.1 mg): Product model: Mettler Toledo, manufacturer: Mettler Toledo Instrument (Shanghai) Co., Ltd.;
[0080] CNC ultrasonic cleaner: Product model: KQ2200E, manufacturer: Kunshan Ultrasonic Instrument Co., Ltd.;
[0081] Vacuum drying oven: Product model: DZF-6050, manufacturer: Shanghai Yiheng Scientific Instrument Co., Ltd.;
[0082] Magnetic stirrer: Product model: German IKARCT basic type, manufacturer: IKARC (Guangzhou) Instrument Equipment Co., Ltd.
[0083] Muffle furnace: Product model: SX2-2.5-10N, manufacturer: Shanghai Yiheng Scientific Instrument Co., Ltd.;
[0084] Ultrapure water preparation machine: Product model: UPHW-III-90T, manufacturer: Sichuan UPHW Ultrapure Technology Co., Ltd.
[0085] Method for obtaining titanium foil: Because the surface of titanium foil will form a smooth and dense oxide film in the air, and the smooth surface is not conducive to the uniform deposition of iridium nanoparticles, a good quality titanium foil roll (thickness 0.1mm, purity 99.6%) is gently rubbed with sandpaper for 5 times, and then placed in Figure 1Mechanical stamping is performed in a stamping die to form an electrode structure with three cylindrical protrusions (the diameter of each protrusion is 3-4 mm and the depth is 1.5-2 mm) (one side of the protrusion is in contact with the test part during the signal acquisition test), and it is trimmed to obtain a circle with a diameter of 12 mm, and then placed in a beaker (the beaker is placed in a CNC ultrasonic cleaner) for cleaning: after placing it in the beaker, pour anhydrous ethanol into the beaker, ultrasonically clean it for 10 minutes to remove various attachments on the surface, replace the anhydrous ethanol in the beaker with ultrapure water, ultrasonically clean it again for 10 minutes, take it out, wipe it with a dust-free cloth, and dry it to obtain a titanium foil.
[0086] In the first electrodeposition solution / second electrodeposition solution, potassium oxalate mainly acts as a complexing agent and pH buffer. Potassium oxalate can form a stable oxalic acid complex with metal ions, control the concentration and state of metal ions in the solution, make metal ions easier to reduce and deposit on the cathode surface, and improve the deposition uniformity and adhesion of the metal film.
[0087] In the following examples, the interval between the working electrode and the counter electrode was 1 cm.
[0088] The vertical titanium dioxide nanotube array obtained after the anodization reaction lacks a layer of strong conductive medium on the top to better transmit current signals, so it is necessary to electro-deposit a second iridium nanolayer on the first iridium-plated titanium foil after anodization, so that a large number of iridium nanoparticles are deposited on the top and side walls of the titanium dioxide nanotube array to help enhance the electron transmission effect.
[0089] Embodiments 1 to 4
[0090] A method for preparing a flexible dry electrode comprises the following steps:
[0091] Step 1, connect the titanium foil to the negative electrode of the programmable linear DC power supply, connect the first platinum sheet to the positive electrode of the programmable linear DC power supply, place the titanium foil and the first platinum sheet in a first electroplating solution, start the programmable linear DC power supply so that the titanium foil is used as a working electrode and the first platinum sheet is used as a counter electrode, the output voltage of the programmable linear DC power supply is 0.8V, the current of the programmable linear DC power supply is 0.1A, a magnetic rotor is placed in the first electroplating solution, and a magnetic stirrer is turned on for stirring during the reaction, and the reaction is carried out for 60 minutes at room temperature and under stirring conditions (stirring speed is 150r / min) to make the titanium foil on the titanium foil. Electrodepositing iridium nanoparticles as a first iridium nanolayer (using a direct current electrodeposition method to electrodeposit iridium nanoparticles on a titanium foil with a two-electrode system as the first iridium nanolayer), rinsing with ultrapure water to obtain a first iridium-plated titanium foil precursor, the first electrodeposition solution comprising: iridium trichloride, potassium oxalate and water, the pH of the first electrodeposition solution being 10.2 (using a potassium carbonate aqueous solution to adjust the pH of the first electrodeposition solution, the concentration of potassium carbonate in the potassium carbonate aqueous solution being 5 mmol / L), the concentration of iridium trichloride in the first electrodeposition solution being 0.8 mmol / L, and the concentration of potassium oxalate in the first electrodeposition solution being 8 mmol / L;
[0092] Step 2, placing the first iridium-plated titanium foil precursor in a muffle furnace, keeping the temperature at 500° C. for 30 minutes, and cooling the temperature from 500° C. to room temperature to obtain a first iridium-plated titanium foil, wherein the rate of heating from room temperature to 500° C. is 5° C. / min;
[0093] Step 3, connecting the first iridium-plated titanium foil to the positive electrode of the programmable linear DC power supply, connecting the second platinum sheet to the negative electrode of the programmable linear DC power supply, immersing the first iridium-plated titanium foil and the second platinum sheet in the first reaction solution at room temperature, starting the programmable linear DC power supply so that the first iridium-plated titanium foil is used as the working electrode and the second platinum sheet is used as the counter electrode (the output voltage of the programmable linear DC power supply is set to 15V, and the current of the programmable linear DC power supply is 110mA), reacting for 90min under stirring conditions (the speed of the magnetic stirrer is 700r / min) to obtain a vertical titanium dioxide nanotube array after an anodic oxidation reaction on the first iridium-plated titanium foil, using a numerically controlled ultrasonic cleaner for ultrasonic cleaning for 3 seconds to obtain a first iridium-plated titanium foil precursor after anodization, the first reaction solution is a mixture of glycerol, ultrapure water and ammonium fluoride, the volume fraction of glycerol, the volume fraction of water in step 3 and the mass fraction of ammonium fluoride The ratio is 35:5:0.45, the unit of volume fraction is mL, and the unit of mass fraction is g;
[0094] Step 4, placing the first iridium-plated titanium foil precursor after anodization in a muffle furnace, keeping the temperature at 500° C. for 150 minutes, and then cooling the temperature from 500° C. to room temperature to obtain the first iridium-plated titanium foil after anodization, wherein the rate of heating from room temperature to 500° C. is 5° C. / min;
[0095] Step 5, connecting the first iridium-plated titanium foil after anodization to the negative electrode of a programmable linear DC power supply, connecting the third platinum sheet to the positive electrode of the programmable linear DC power supply, placing the first iridium-plated titanium foil after anodization and the third platinum sheet in a second electrodeposition solution, starting the DC power supply so that the negative electrode serves as a working electrode and the positive electrode serves as a counter electrode (the output voltage of the programmable linear DC power supply is set to 15V, and the current of the programmable linear DC power supply is 150mA), reacting for 90min at room temperature and under stirring conditions (the speed of the magnetic stirrer is 250r / min) so that iridium nanoparticles are electrodeposited on the first iridium-plated titanium foil after anodization as a second iridium nanolayer, and rinsing with ultrapure water to obtain a second iridium-plated titanium foil, wherein the second electrodeposition solution is the same as the first electrodeposition solution;
[0096] Step 6. Under light-proof conditions, immerse the second iridium-coated titanium foil in an acidic nanozyme solution with a pH of 5.5 for 72 hours to form a nanozyme film on the second iridium-coated titanium foil. After taking it out, dry it to obtain a flexible dry electrode, wherein the nanozyme solution is a mixture of high-copper-loaded single-atom nanozyme and an acidic mitigation solution. The acidic mitigation solution is a mixture of Tris-hydrochloric acid buffer solution (the main components are tris(hydroxymethylaminomethane) and hydrochloric acid) and ultrapure water. The concentration of tris(hydroxymethylaminomethane) in the acidic mitigation solution is 0.09 mol / L. The method for preparing the nanozyme solution is as follows: pour 3 mL of Tris-hydrochloric acid buffer solution with a concentration of 1.5 mol / L into a beaker, first add 5 mL of ultrapure water to dilute it, and then add ultrapure water to make up to 50 mL to obtain an acidic mitigation solution, mix the high-copper-loaded single-atom nanozyme and the acidic mitigation solution to obtain a nanozyme solution (the concentration of high-copper-loaded single-atom nanozyme in the nanozyme solution is 8.92 mmol / L).
[0097] The method for preparing a high-copper-loaded single-atom nanozyme comprises the following steps:
[0098] S1, an aqueous solution of aminated graphene quantum dots with a concentration of 1 mg / mL and an aqueous solution of Cu source with a concentration of 5 mg / mL are mixed until uniform, ultrasonicated at room temperature for 15 min, and frozen in liquid nitrogen for 15 min to obtain a first powder, wherein the ratio of the mass fraction of the aminated graphene quantum dots to the molar fraction of Cu in the Cu source is X, the unit of the mass fraction is mg, the unit of the molar fraction is mmol, and the Cu source is CuCl2; the value of X is shown in Table 1.
[0099] S2, mixing the first powder and urea, grinding them until uniform, putting them into a corundum boat, then moving the corundum boat into a vacuum tube furnace, heating them to 500°C at a heating rate of 10°C / min under an argon atmosphere and calcining them at 500°C for 2h to obtain a high-loaded copper single-atom nanozyme. In terms of mass fractions, the ratio of the first powder to urea is 1:10.
[0100] The present invention prepares high-copper-loaded single-atom nanozymes through an in-situ anchoring strategy. During the preparation process, the Cu source is precisely confined in a carbon carrier composed of amino-modified graphene quantum dots, and urea is introduced to provide a nitrogen-rich coordination environment for the copper atoms. Under the protection of Ar gas, the chemical bond between the Cu atom and the carbon carrier is further stabilized through pyrolysis.
[0101] Table 1
[0102] Example X Example 1 30:0.01 Example 2 30:0.02 Example 3 30:0.03 Example 4 30:0.05
[0103] Figure 2 a is a scanning electron microscope image of a titanium foil roll, which has a smooth surface. Figure 2 Figure b is a scanning electron microscope image of a titanium foil with many scratches on its surface. A smooth surface is not conducive to the uniform deposition of iridium nanoparticles, while a surface with many scratches formed by grinding provides more nucleation sites for iridium nanoparticles, which helps to improve the performance of the flexible dry electrode.
[0104] Figure 3 a is the microscopic morphology of the first iridium-coated titanium foil magnified 2000 times. Figure 3 b is the microscopic morphology of the first iridium-coated titanium foil magnified 5000 times. Figure 3 b has clearly shown that after the first electrodeposition, a dense and evenly dispersed layer of iridium nanoparticles is formed on the surface of the titanium foil. There are some gaps between these iridium nanoparticles, which provide space for the subsequent growth of titanium dioxide nanotube arrays. These gaps will also control the diameter of titanium dioxide nanotubes in the subsequent titanium dioxide nanotube arrays to a certain extent (the height of the titanium dioxide nanotubes is about 100nm and the diameter is about 40nm). This unique structural feature will help improve the electrocatalytic performance of the flexible dry electrode.
[0105] Figure 4 This is the morphology of the first iridium-coated titanium foil after anodization, magnified 5000 times. It can be seen that the titanium dioxide nanotubes in the area have grown well and are arranged very neatly.
[0106] Figure 5 This is the morphology of the second iridium-plated titanium foil. It can be seen that many iridium nanoparticles are attached to the top of the titanium dioxide nanotubes, and a layered phenomenon occurs, showing a bottom-up arrangement of particles from small to large, which leads to a gradual increase in the capacitance formed during signal transmission. Such a structural design is more conducive to the transmission of electrical signals, providing more superior characteristics for the performance of flexible dry electrodes, and highlighting the great potential of this design in improving electrode performance.
[0107] Figure 6 The microscopic morphology of the flexible dry electrode prepared in Example 1. Figure 5 compared to, Figure 6 The iridium nanoparticles are no longer dispersed particles, but are completely coated with high-copper-loaded single-atom nanozymes.
[0108] Figure 7 Transmission electron microscope image of the flexible dry electrode prepared in Example 1 ( Figure 7 a~ Figure 7 d is an image at different positions). In a vacuum environment, the flexible dry electrode prepared in Example 1 was cut into a cross section of 5 mm*2 mm as a sample, placed in a bottle filled with anhydrous ethanol, the bottle mouth was sealed and ultrasonically vibrated for 1 min, and an electron beam was aligned with the sample for measurement to obtain Figure 7 From the transmission electron microscope image, we can see that Figure 7 The titanium dioxide nanotubes are still arranged neatly, indicating that the preparation method of the present invention is reliable and stable.
[0109] Figure 8 This is the XPS of the flexible dry electrode prepared in Example 1. Figure 8 It can be seen that the flexible dry electrode contains Ti, O, C, and Ir, among which Ti and O elements account for a relatively high proportion, while C and Ir account for a relatively low proportion.
[0110] The flexible dry electrode obtained in Example 1 was tested for impedance, eye opening and closing, eye blinking, and tooth clenching signal acquisition:
[0111] Prepare three traditional wet electrodes (Ag / AgCl electrodes produced by Beijing Qingjing Electronic Technology Co., Ltd.), a flexible dry electrode, conductive paste, scrub, syringe, medical tape, headband, and head net. Connect the flexible dry electrode to the signal acquisition device through a signal line. The signal acquisition device is a 32-lead EEG acquisition device of the Greal model from Neuroscan, an Australian company.
[0112] Signal acquisition: Use scrub to gently wipe the mastoids behind the ears of the subject to remove the stratum corneum, apply 0.3mL of conductive paste to each of the two traditional wet electrodes with a syringe, and use medical tape to fix the two traditional wet electrodes to the mastoids behind the ears, one of which is used as a reference electrode and the other as a ground electrode. Select two adjacent horizontal positions in the occipital region of the subject's head, wipe the two adjacent horizontal positions with scrub, apply 0.3mL of conductive paste to the third traditional wet electrode, fix the flexible dry electrode (flexible dry electrode does not require conductive paste) and the third traditional wet electrode to two adjacent horizontal positions in the occipital region of the subject's head with a headband, and finally fix them with a head net.
[0113] In the impedance signal test, the sampling rate is set to 4096, and the 50Hz and 60Hz power frequency signals are filtered out. The impedance data of the third conventional wet electrode and the flexible dry electrode are as follows: Fig. 9As shown, Fp1 represents the flexible dry electrode, and its impedance value is 5.6kΩ, and Fp2 represents the third traditional wet electrode, and its value is 1.3kΩ. It can be seen that the scalp / electrode contact impedance characteristics of the flexible dry electrode are close to those of the traditional wet electrode.
[0114] In the eye-opening and eye-closing signal test, the subjects closed their eyes at 2, 5, and 8 seconds respectively. The results are as follows: Fig.10 As shown, Fp1 represents the flexible dry electrode, and Fp2 represents the third traditional wet electrode. The original waveform of eye opening and closing ( Fig.10 ) showed that the subjects had corresponding α rhythm characteristics when closing their eyes at 2, 5, and 8 seconds, respectively. The signal frequency was low and the fluctuation amplitude was large in the closed-eye state, and the signal frequency was high and the fluctuation amplitude was small in the open-eye state. Fig.15 It can be seen that the correlation between the eye opening signal of the flexible dry electrode and the traditional wet electrode Ag / AgCl electrode is 99.81%. Fig.16 It can be seen that the correlation between the eye closing signal of the flexible dry electrode and the traditional wet electrode Ag / AgCl electrode is 99.76%.
[0115] In the blink signal test, the subjects blinked at 2, 5, and 8 seconds respectively. The results are as follows: Fig.11 As shown, Fp1 represents the flexible dry electrode, and Fp2 represents the third traditional wet electrode. The original waveform of blinking ( Fig.11 ) shows that when the subjects blink at 2, 5, and 8 seconds, there will be corresponding negative peaks. Fig.17 It can be seen that the correlation between the blinking signals of the flexible dry electrode and the traditional wet electrode Ag / AgCl electrode is 99.75%.
[0116] In the teeth-gritting signal test, the subjects clenched their teeth at 2, 5, and 8 seconds respectively. The results are as follows: Fig.12 As shown, Fp1 represents the flexible dry electrode, and Fp2 represents the third conventional wet electrode. Fig.12 It is known that when the subjects clench their teeth at 2, 5, and 8 seconds, corresponding sawtooth-shaped peaks will appear. Fig.18 It can be seen that the correlation between the teeth biting signal of the flexible dry electrode and the traditional wet electrode Ag / AgCl electrode is 99.67%.
[0117] In summary, although the flexible dry electrode is not coated with conductive paste, the signal quality of the flexible dry electrode is as good as that of the traditional wet electrode. The performance of the flexible dry electrode of the present invention is completely equivalent to that of the traditional wet electrode.
[0118] The titanium foil, the first iridium-plated titanium foil, ( Fig.13 "Iridium-plated titanium foil"), the first iridium-plated titanium foil after anodizing ( Fig.13 The electrochemical impedance spectroscopy (EIS) test was performed on the flexible dry electrode prepared in Example 1, and the results were as follows: Fig.13The frequency impedance diagram is shown. Fig.13 It can be observed that with the increase of frequency, the impedance modulus of the titanium foil, the first iridium-coated titanium foil, the first iridium-coated titanium foil after anodization, and the flexible dry electrode prepared in Example 1 gradually decreases, the impedance change amplitude of the titanium foil is the smallest (the impedance modulus decreases the slowest), and the impedance change amplitude of the flexible dry electrode is the largest (the impedance modulus decreases the fastest), indicating that the flexible dry electrode has a low resistance in the high-frequency range.
[0119] The titanium foil, the first iridium-plated titanium foil, ( Fig.14 "Iridium-plated titanium foil"), the first iridium-plated titanium foil after anodizing ( Fig.14 The electrochemical impedance spectroscopy (EIS) test was performed on the flexible dry electrode prepared in Example 1, and the results were as follows: Fig.14 The Nyquist curve diagram shown. It can be observed that all the curves form a semicircle, the diameter of the semicircle can reflect the resistance of the material, and the frequency corresponding to the peak of the semicircle can reflect the capacitance characteristics. Fig.14 The semicircle diameter of the titanium foil is the largest, indicating that it has a higher resistance. The semicircle diameter of the flexible dry electrode is the smallest, indicating that it has the lowest resistance.
[0120] The present invention is described above by way of example. It should be noted that, without departing from the core of the present invention, any simple deformation, modification or other equivalent replacement that can be made by those skilled in the art without inventive effort falls within the protection scope of the present invention.
Claims
1. A flexible dry electrode, characterized in that: It is a layered structure, which is composed of: a nanozyme film, a second iridium nanolayer, a titanium dioxide nanotube array, a first iridium nanolayer and a flexible substrate from top to bottom. The nanozyme film includes: amino graphene quantum dots loaded with copper single atoms.
2. The flexible dry electrode according to claim 1, characterized in that: The flexible substrate is a titanium foil.
3. A method for preparing a flexible dry electrode, comprising the following steps: Step 1, connecting the titanium foil to the negative electrode of a direct current power supply, connecting the first platinum sheet to the positive electrode of the direct current power supply, placing the titanium foil and the first platinum sheet in a first electrodeposition solution, starting the direct current power supply so that the titanium foil serves as a working electrode and the first platinum sheet serves as a counter electrode, reacting at room temperature and under stirring conditions so that iridium nanoparticles are electrodeposited on the titanium foil as a first iridium nanolayer, and washing to obtain a first iridium-plated titanium foil precursor, wherein the first electrodeposition solution comprises: iridium trichloride, potassium oxalate and water; Step 2, placing the first iridium-plated titanium foil precursor in a muffle furnace, keeping the temperature at 500-600° C. for 30-40 minutes, and cooling to room temperature to obtain a first iridium-plated titanium foil; Step 3, connecting the first iridium-coated titanium foil to the positive electrode of a direct current power supply, connecting the second platinum sheet to the negative electrode of the direct current power supply, immersing the first iridium-coated titanium foil and the second platinum sheet in a first reaction solution at room temperature, starting the direct current power supply so that the first iridium-coated titanium foil serves as a working electrode and the second platinum sheet serves as a counter electrode, reacting under stirring conditions, so that an anodic oxidation reaction occurs on the first iridium-coated titanium foil to obtain a vertical titanium dioxide nanotube array, and washing to obtain a first iridium-coated titanium foil precursor after anodization; Step 4, placing the anodized first iridium-plated titanium foil precursor in a muffle furnace, keeping the temperature at 500-600° C. for 150-200 min, and cooling to room temperature to obtain an anodized first iridium-plated titanium foil; Step 5, connecting the first iridium-plated titanium foil after anodization to the negative electrode of a direct current power supply, connecting the third platinum sheet to the positive electrode of the direct current power supply, placing the first iridium-plated titanium foil after anodization and the third platinum sheet in a second electrodeposition solution, starting the direct current power supply, so that the first iridium-plated titanium foil after anodization is used as a working electrode and the third platinum sheet is used as a counter electrode, reacting at room temperature and under stirring conditions, so that iridium nanoparticles are electrodeposited on the first iridium-plated titanium foil after anodization as a second iridium nanolayer, washing, and obtaining a second iridium-plated titanium foil, wherein the second electrodeposition solution comprises: iridium trichloride, potassium oxalate and water; Step 6, under light-proof conditions, immerse the second iridium-coated titanium foil in an acidic nanozyme solution, form a nanozyme film on the second iridium-coated titanium foil, take it out, and dry it to obtain a flexible dry electrode, wherein the nanozyme solution includes: high-copper-loaded single-atom nanozyme, and the concentration of the high-copper-loaded single-atom nanozyme in the nanozyme solution is 7 to 10 mmol / L.
4. The preparation method according to claim 3, characterized in that: The method for preparing the high-copper-loaded single-atom nanozyme comprises the following steps: S1, mixing the aqueous solution of aminated graphene quantum dots and a Cu source until uniform, ultrasonicating, and freeze-drying to obtain a first powder, wherein the ratio of the mass fraction of the aminated graphene quantum dots to the molar fraction of Cu in the Cu source is 30:(0.01-0.05), the unit of the mass fraction is mg, and the unit of the molar fraction is mmol; S2, mixing the first powder and urea, grinding until uniform, and calcining at 500-600° C. for 2-2.5 hours under an inert gas atmosphere to obtain the high-copper-loaded single-atom nanozyme. In terms of mass fractions, the ratio of the first powder to urea is 1:(8-12).
5. The preparation method according to claim 3, characterized in that: In step 1, the concentration of iridium trichloride in the first electrodeposition solution is 0.64-0.96 mmol / L, and the concentration of potassium oxalate in the first electrodeposition solution is 6.4-9.6 mmol / L; in step 5, the concentration of iridium trichloride in the second electrodeposition solution is 0.64-0.96 mmol / L, and the concentration of potassium oxalate in the second electrodeposition solution is 6.4-9.6 mmol / L.
6. The preparation method according to claim 3, characterized in that: In step 1, the pH of the first electrodeposition solution is 10.2-10.5; in step 5, the pH of the second electrodeposition solution is 10.2-10.
5.
7. The preparation method according to claim 3, characterized in that: In step 6, the pH value of the nanozyme solution is 5.4-5.
6.
8. The preparation method according to claim 3, characterized in that: In step 3, the output voltage of the DC power supply is 15-15.5V, and the current of the DC power supply is 110-115mA.
9. The preparation method according to claim 3, characterized in that: In step 1, the output voltage of the DC power supply is 0.8-1.0V, and the current of the DC power supply is 0.1-0.12A.
10. The preparation method according to claim 3, characterized in that: In step 5, the output voltage of the DC power supply is 15-15.5V, and the current of the DC power supply is 150-160mA.