Absorption core body of SAP membrane structure and preparation method of absorption core body

By combining modified polylactic acid resin with SAP resin and cellulose-chitosan composite, an SAP film structure absorbing core is formed, which solves the problem of insufficient absorption rate and liquid storage capacity of the existing absorbing core, and realizes the Highly efficient water absorption and biodegradability, suitable for modern sanitary products.

CN119074398AActive Publication Date: 2024-12-06GUANGZHOU ANJIE CORE MATERIAL TECH CO LTD

Patent Information

Application Number
CN202411243585.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-05
Publication Date
2024-12-06
Estimated Expiration
2044-09-05

AI Technical Summary

Technical Problem

The existing absorbent core has insufficient absorption rate and liquid storage capacity, and the acrylic resin is difficult to biodegrade, resulting in difficult and high cost in recycling and processing, which cannot meet the needs of environmentally friendly and green development.

Method used

The SAP membrane structure absorbing core composed of modified polylactic acid resin, SAP resin and cellulose-chitosan composite is improved by grafting acrylate groups with polylactic acid and gelatin, and the hydrophilicity is improved with SAP. The resin and cellulose-chitosan composite form a synergistic effect, enhancing water absorption and liquid storage properties, and avoiding the use of chemical adhesives.

Benefits of technology

The SAP membrane structure absorbing core that effectively absorbs and stores liquids has excellent mechanical properties, water absorption properties and biodegradability, overcomes the shortcomings of the existing technology, and is suitable for products such as sanitary napkins and diapers.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005029970380000011
    Figure BDA0005029970380000011
  • Figure BDA0005029970380000041
    Figure BDA0005029970380000041
  • Figure BDA0005029970380000051
    Figure BDA0005029970380000051
Patent Text Reader

Abstract

The invention relates to an absorption core body of an SAP membrane structure and a preparation method of the absorption core body. The absorption core body of the SAP membrane structure comprises an upper non-woven fabric layer, an absorption layer and a lower non-woven fabric layer from top to bottom, the absorbing layer is prepared from the following raw materials in parts by mass: 20 to 50 parts of modified polylactic acid, 10 to 20 parts of SAP resin, 10 to 20 parts of a cellulose-chitosan compound, 0.5 to 5 parts of an auxiliary agent and 10 to 50 parts of a solvent; wherein the modified polylactic acid is obtained by reacting acrylic anhydride modified gelatin with acrylic acid grafted polylactic acid. The absorption core body not only has excellent water absorption capacity and can efficiently absorb and store liquid, but also has the characteristics of good biocompatibility and easiness in degradation, can meet the requirements of products such as sanitary napkins and paper diapers on performance, overcomes the defects in the prior art, and has a wide application prospect.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of sanitary products, and in particular to an absorbent core with a SAP film structure and a preparation method thereof. Background Art

[0002] Sanitary napkins and diapers are essential hygiene products in modern life, providing an important guarantee for the comfortable life of women, children and other groups. The absorbent core is the core part of sanitary napkins and diapers. The liquid absorption rate and liquid storage effect of the product are determined by the performance of the absorbent core.

[0003] The absorbent core is usually composed of absorbent resin and covering materials such as non-woven fabrics, paper towels or organic fibers. The absorbent resin includes polyacrylic resin, polyacrylate resin, etc. Although the current absorbent core has achieved an improvement in liquid absorption effect, it still has certain defects in absorption rate, liquid storage capacity, etc., and cannot take into account multiple performance aspects. In addition, acrylic resin is difficult to biodegrade, so the recycling and processing of the absorbent core is difficult and costly, which has caused great pressure on environmental protection and can no longer meet the current social trend of environmental friendliness and green development.

[0004] In summary, there is an urgent need to develop a new technical solution to solve the problems existing in the existing technology and meet the market and consumer needs. Summary of the invention

[0005] Based on this, the present invention provides an absorbent core with a SAP film structure and a preparation method thereof. The absorbent core with a SAP film structure provided by the present invention, which is composed of an absorbent layer made of modified polylactic acid resin, SAP resin, cellulose-chitosan composite and other components, not only has excellent water absorption capacity and can efficiently absorb and store liquid, but also has the characteristics of good biocompatibility and easy degradation, can meet the performance requirements of products such as sanitary napkins and diapers, overcomes the shortcomings of the prior art, and has broad application prospects.

[0006] An object of the present invention is to provide an absorbent core of a SAP film structure, wherein the absorbent core of the SAP film structure comprises, from top to bottom: an upper non-woven fabric layer, an absorbent layer and a lower non-woven fabric layer;

[0007] The raw materials of the absorption layer include the following components in parts by weight:

[0008]

[0009] in,

[0010] The modified polylactic acid is obtained by reacting acrylic anhydride-modified gelatin with acrylic acid-grafted polylactic acid.

[0011] SAP resin (Super Absorbent Polymer) is a polymer material with extremely strong water absorption and water retention properties. This type of resin can absorb hundreds or even thousands of times its own weight in water, so it has been widely used in liquid-absorbing products such as sanitary napkins.

[0012] Furthermore, the preparation method of the modified polylactic acid comprises the following steps:

[0013] S1, mixing hydroxy-terminated polylactic acid, acrylic acid, a catalyst and a polymerization inhibitor, and heating the mixture for reaction to obtain acrylic acid-grafted polylactic acid;

[0014] S2, mixing gelatin and acrylic anhydride, and reacting at low temperature to obtain acrylic anhydride-modified gelatin;

[0015] S3, mixing the acrylic acid grafted polylactic acid, acrylic anhydride modified gelatin, a crosslinking agent and an initiator, and heating them under the protection of an inert gas to react, so as to obtain modified polylactic acid.

[0016] Furthermore, in step S1, the temperature of the heating reaction is 80-120°C; in step S2, the temperature of the low-temperature reaction is 0-5°C; in step S3, the temperature of the heating reaction is 60-90°C.

[0017] Furthermore, in step S1, the mass ratio of the terminal hydroxyl polylactic acid to acrylic acid is 1:(0.1-0.5).

[0018] Furthermore, in step S2, the mass ratio of gelatin to acrylic anhydride is 1:(0.5-2).

[0019] Furthermore, in step S3, the mass ratio of the acrylic acid grafted polylactic acid to the acrylic anhydride modified gelatin is 1:(0.1-2).

[0020] Furthermore, the cellulose-chitosan composite is a mixture of oxidized cellulose and carboxymethyl chitosan.

[0021] Furthermore, the mass ratio of the oxidized cellulose to carboxymethyl chitosan is 1:(2-5).

[0022] Another object of the present invention is to provide a method for preparing the absorbent core of the above-mentioned SAP film structure, comprising the following steps:

[0023] The modified polylactic acid, SAP resin, cellulose-chitosan composite and additives are laid on the surface of the lower non-woven fabric layer, and the solvent is sprayed to obtain an absorption layer. Then, an upper non-woven fabric layer is laid on the surface of the absorption layer, and an absorption core with a SAP membrane structure is obtained after drying.

[0024] The present invention has the following beneficial effects:

[0025] The absorbent core of the SAP film structure provided by the present invention adopts modified polylactic acid resin, SAP resin, cellulose-chitosan complex and other components to obtain an absorbent layer. Polylactic acid is a biodegradable polymer material with good mechanical properties and easy processing, but its hydrophilicity is poor. Its application in water-absorbing materials will cause a decrease in liquid absorption performance. The present invention further polymerizes polylactic acid and gelatin after grafting acrylate groups, thereby introducing gelatin molecules into the polylactic acid structure, greatly improving the hydrophilicity of polylactic acid, which is conducive to the flow and transfer of liquid in the polymer network, thereby improving the absorption rate and liquid storage capacity of water and blood. The modified polylactic acid also has good compatibility with SAP resin. After compounding with cellulose-chitosan complex, multiple components can synergize and further improve water absorption and liquid storage performance. In addition, the polylactic acid resin modified by gelatin has a certain bonding ability, and can also produce synergistic effects with the polar groups of the cellulose-chitosan complex through hydrogen bonds and intermolecular forces, thereby tightly combining with the upper and lower covering layers, avoiding the use of chemical adhesives. In summary, the absorbent core of the SAP membrane structure of the present invention has excellent mechanical properties, water absorption properties and liquid storage properties, and at the same time has strong biological affinity and is degradable, thus overcoming the shortcomings of the prior art and having good application prospects. DETAILED DESCRIPTION

[0026] In order to more clearly illustrate the technical solution of the present invention, the following examples are listed. Unless otherwise stated, the raw materials, reactions and post-treatment methods shown in the examples are common raw materials on the market and technical methods well known to those skilled in the art.

[0027] The words "preferred", "preferably", "more preferably", etc. in the present invention refer to embodiments of the present invention that can provide certain beneficial effects in certain circumstances. However, other embodiments may also be preferred under the same circumstances or other circumstances. In addition, the description of one or more preferred embodiments does not imply that other embodiments are not applicable, nor is it intended to exclude other embodiments from the scope of the present invention.

[0028] It should be understood that, except in any operating examples, or where otherwise indicated, all numbers indicating, for example, the amounts of ingredients used in the specification and claims should be understood to be modified in all cases by the term "about". Therefore, unless indicated to the contrary, the numerical parameters set forth in the following specification and the appended claims are approximate values ​​that vary depending on the desired properties to be obtained by the present invention.

[0029] The SAP resin in the embodiment of the present invention is the SAP super absorbent resin NR-760H produced by Shandong Noel Biotechnology Co., Ltd.

[0030] The polylactic acid in the embodiments of the present invention was purchased from Shenzhen Guanghua Weiye Co., Ltd.; gelatin was purchased from Guangzhou Huayu Biotechnology Co., Ltd.

[0031] The preparation method of the modified polylactic acid in the embodiment of the present invention comprises the following steps:

[0032] S1. After dehydrating the polylactic acid by vacuum distillation, the mixture was heated at 120° C. in vacuum for 2 h, and then 0.5 wt % of a catalyst (stannous chloride and p-toluenesulfonic acid in a molar ratio of 1:1) and pentaerythritol (polylactic acid: pentaerythritol=10:41, m / m) were added, and the mixture was reacted at 145° C. for 2 h, and then the temperature was raised to 170° C. and the reaction was continued for 3 h to obtain hydroxy-terminated polylactic acid;

[0033] Using toluene as solvent, hydroxy-terminated polylactic acid, acrylic acid, p-toluenesulfonic acid and hydroquinone in a mass ratio of 60:19:0.3:0.09 were mixed, reacted at 120°C for 5 hours, and the solvent was removed under reduced pressure to obtain acrylic acid-grafted polylactic acid;

[0034] S2, using water as solvent, adding gelatin and stirring for 0.5h, adjusting the pH to 7.5 with 2mol / L NaOH solution, then adding methacrylic anhydride (gelatin: methacrylic anhydride = 1:0.9, m / m), reacting at 4°C for 24h, dialyzing for 3 days (KDa = 10000), and freeze-drying to obtain acrylic anhydride-modified gelatin;

[0035] S3. Using water as solvent, the acrylic acid grafted polylactic acid, acrylic anhydride modified gelatin and N,N-methylenebisacrylamide in a mass ratio of 1:1:0.2 are mixed, and then 1 wt% of potassium persulfate by mass of the system is added, and the mixture is reacted at 65° C. for 3 h under nitrogen protection, and the modified polylactic acid is obtained after centrifugation and drying.

[0036] The cellulose-chitosan composite in the embodiment of the present invention is prepared according to the method in “Zhao Hongkai, Zhang Kehan, Rui Shoupeng. Preparation and performance study of microcrystalline cellulose / chitosan water-absorbing materials [J]. New Chemical Materials, 2021(007):049.”

[0037] 10 g of microcrystalline cellulose, 12 g of NaIO4, and 10 g of NaCl were added to 500 mL of deionized water, stirred in a dark environment for 8 h, and then centrifuged, washed, and dried to obtain oxidized cellulose;

[0038] 1 g of NaOH was dissolved in a mixture of isopropanol (48 mL) and water (12 mL), and then 1 g of chitosan was added. After swelling at room temperature for 1 h, 1.5 g of chloroacetic acid (dissolved in 2 mL of isopropanol) was added, and after reacting for 12 h, the mixture was washed and dried to obtain carboxymethyl chitosan.

[0039] Oxidized cellulose (1 wt% solution) and carboxymethyl chitosan (1 wt% solution) in a mass ratio of 1:3 were mixed, stirred in a 60°C water bath for 1 h, and placed at room temperature for 6 h to form a cross-linked gel, which was then freeze-dried for 72 h and ground to obtain a cellulose-chitosan composite.

[0040] The auxiliary agent in the embodiment of the present invention is a nano silver antibacterial agent.

[0041] The "parts" in the embodiments of the present invention refer to parts by mass.

[0042] Example 1

[0043] An absorbent core of a SAP film structure, the absorbent core of the SAP film structure comprising, from top to bottom, an upper non-woven fabric layer, an absorbent layer and a lower non-woven fabric layer;

[0044] The raw materials of the absorption layer include the following components in parts by weight:

[0045]

[0046] The method for preparing the absorbent core of the SAP film structure comprises the following steps:

[0047] According to the above-mentioned mass fractions, the modified polylactic acid, SAP resin, cellulose-chitosan composite and additives are evenly mixed and laid on the surface of the lower non-woven fabric layer, and deionized water is sprayed to obtain an absorption layer with a thickness of 2 mm. Then, an upper non-woven fabric layer is laid on the surface of the absorption layer. After drying, an absorption core with a SAP membrane structure is obtained.

[0048] Example 2

[0049] An absorbent core of a SAP film structure, the absorbent core of the SAP film structure comprising, from top to bottom, an upper non-woven fabric layer, an absorbent layer and a lower non-woven fabric layer;

[0050] The raw materials of the absorption layer include the following components in parts by weight:

[0051]

[0052]

[0053] The method for preparing the absorbent core of the SAP film structure comprises the following steps:

[0054] According to the above-mentioned mass fractions, the modified polylactic acid, SAP resin, cellulose-chitosan composite and additives are evenly mixed and laid on the surface of the lower non-woven fabric layer, and deionized water is sprayed to obtain an absorption layer with a thickness of 2 mm. Then, an upper non-woven fabric layer is laid on the surface of the absorption layer. After drying, an absorption core with a SAP membrane structure is obtained.

[0055] Example 3

[0056] An absorbent core of a SAP film structure, the absorbent core of the SAP film structure comprising, from top to bottom, an upper non-woven fabric layer, an absorbent layer and a lower non-woven fabric layer;

[0057] The raw materials of the absorption layer include the following components in parts by weight:

[0058]

[0059] The method for preparing the absorbent core of the SAP film structure comprises the following steps:

[0060] According to the above-mentioned mass fractions, the modified polylactic acid, SAP resin, cellulose-chitosan composite and additives are evenly mixed and laid on the surface of the lower non-woven fabric layer, and deionized water is sprayed to obtain an absorption layer with a thickness of 2 mm. Then, an upper non-woven fabric layer is laid on the surface of the absorption layer. After drying, an absorption core with a SAP membrane structure is obtained.

[0061] Comparative Example 1

[0062] An absorbent core with a SAP film structure. The difference between this comparative example and Example 1 is that the modified polylactic acid is replaced by a physical mixture of polylactic acid and gelatin in a mass ratio of 1:1, and the other ingredients and preparation method are the same as those in Example 1.

[0063] Comparative Example 2

[0064] An absorbent core with a SAP film structure. The difference between this comparative example and Example 1 is that the cellulose-chitosan composite is replaced with an equal mass of SAP resin, and the other components and preparation method are the same as those in Example 1.

[0065] Test Case

[0066] A performance comparison test was performed on Examples 1-3 and Comparative Examples 1-2.

[0067] Test method: GB / T14207-2008 is used to test water absorption and blood absorption.

[0068] The test results are shown in Table 1.

[0069] Table 1 Absorption performance test results

[0070] project Example 1 Example 2 Example 3 Comparative Example 1 Comparative Example 2 Water absorption (g) 50.8 50.3 50.1 44.9 48.6 Artificial menstrual blood penetration time (s) 5.85 5.76 5.79 7.83 6.21 Artificial menstrual blood backflow volume (g) 0.69 0.72 0.71 1.67 0.98

[0071] According to Table 1, it can be concluded that the absorbent core of the SAP film structure prepared in the embodiment of the present invention has excellent absorption performance, a large water absorption capacity, and both a high absorption rate and a low rewet amount. However, in Comparative Examples 1-2, the polylactic acid is not modified, or a cellulose-chitosan composite is not used as a component, resulting in a decrease in the hydrophilicity of the material, making it difficult to form a synergistic effect between the components, and the absorption rate of the absorbent core is significantly reduced, the water absorption capacity is reduced, and the rewet amount is increased, and the ideal performance improvement cannot be achieved.

[0072] It will be apparent to those skilled in the art that the present invention is not limited to the details of the exemplary embodiments described above and that the present invention can be implemented in other specific forms without departing from the spirit or essential features of the present invention. Therefore, the embodiments should be considered exemplary and non-restrictive in all respects, and the scope of the present invention is defined by the appended claims rather than the above description, and it is intended that all changes falling within the meaning and scope of the equivalent elements of the claims be included in the present invention.

[0073] In addition, it should be understood that although the present specification is described according to implementation modes, not every implementation mode contains only one independent technical solution. This description of the specification is only for the sake of clarity. Those skilled in the art should regard the specification as a whole. The technical solutions in each embodiment may also be appropriately combined to form other implementation modes that can be understood by those skilled in the art.

Claims

1. An absorbent core of a SAP film structure, characterized in that: The absorbent core of the SAP film structure comprises, from top to bottom, an upper non-woven fabric layer, an absorbent layer and a lower non-woven fabric layer; The raw materials of the absorption layer include the following components in parts by weight: Modified polylactic acid 20-50 parts 10-20 parts of SAP resin 10-20 parts of cellulose-chitosan complex Additives 0.5-5 parts 10-50 parts of solvent; in, The modified polylactic acid is obtained by reacting acrylic anhydride-modified gelatin with acrylic acid-grafted polylactic acid.

2. The absorbent core of the SAP film structure according to claim 1, characterized in that: The preparation method of the modified polylactic acid comprises the following steps: S1, mixing hydroxy-terminated polylactic acid, acrylic acid, a catalyst and a polymerization inhibitor, and heating the mixture for reaction to obtain acrylic acid-grafted polylactic acid; S2, mixing gelatin and acrylic anhydride, and reacting at low temperature to obtain acrylic anhydride-modified gelatin; S3, mixing the acrylic acid grafted polylactic acid, acrylic anhydride modified gelatin, a crosslinking agent and an initiator, and heating them under the protection of an inert gas to react, so as to obtain modified polylactic acid.

3. The absorbent core of the SAP film structure according to claim 2, characterized in that: In step S1, the temperature of the heating reaction is 80-120°C; in step S2, the temperature of the low-temperature reaction is 0-5°C; in step S3, the temperature of the heating reaction is 60-90°C.

4. The absorbent core of the SAP film structure according to claim 2, characterized in that: In step S1, the mass ratio of the terminal hydroxyl polylactic acid to acrylic acid is 1:(0.1-0.5).

5. The absorbent core of the SAP film structure according to claim 2, characterized in that: In step S2, the mass ratio of gelatin to acrylic anhydride is 1:(0.5-2).

6. The absorbent core of the SAP film structure according to claim 2, characterized in that: In step S3, the mass ratio of the acrylic acid grafted polylactic acid to the acrylic anhydride modified gelatin is 1:(0.1-2).

7. The absorbent core of the SAP film structure according to claim 1, characterized in that: The cellulose-chitosan composite is a mixture of oxidized cellulose and carboxymethyl chitosan.

8. The absorbent core of the SAP film structure according to claim 7, characterized in that: The mass ratio of the oxidized cellulose to carboxymethyl chitosan is 1:(2-5).

9. The method for preparing an absorbent core of a SAP film structure according to any one of claims 1 to 8, characterized in that: The steps include: The modified polylactic acid, SAP resin, cellulose-chitosan composite and additives are laid on the surface of the lower non-woven fabric layer, and the solvent is sprayed to obtain an absorption layer. Then, an upper non-woven fabric layer is laid on the surface of the absorption layer, and an absorption core with a SAP membrane structure is obtained after drying.

Citation Information

Patent Citations

  • Surface-modified hydrogels and hydrogel microparticles

    CN102762655A

  • Highly-antibacterial novel slightly-soluble healthcare sanitary pad capable of adsorbing heavy metal particles

    CN105616075A

  • Super absorbent polymer with high CRC / TAC ratio for absorbing paper diaper core

    CN107260406A

  • Preparation method of magnetic anti-haemorrhoids elastic diaper absorbent core

    CN110090113A

  • Preparation method of breathable and anti-allergic material for adult paper diapers

    CN114015032A

Cited By

  • Comfortable medical nursing pad with multi-layer structure and preparation process of comfortable medical nursing pad

    CN119837707A