Physical cross-linked network composite material loaded with acellular matrix particles

Through physical crosslinking network composite material technology, the combination of alginate and polymer polymer and metal ions is used to solve the system uniform stability and injectability of the microparticles loaded with decellularized matrix in the prior art, and the microparticles are maintained. Natural structure, realizes multifunctional characteristics and simplify operations, expanding the application field.

CN119075011APending Publication Date: 2024-12-06SHANGHAI BAIYIYUAN BIOENGINEERING CO LTD

Patent Information

Application Number
CN202411586371.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-11-08
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

The prior art has shortcomings in the uniform stability, injectability and natural structure maintenance of the system of loaded decellularized matrix particles, especially when chemical crosslinking agents are used, and the operation complexity is high.

Method used

Using physical crosslinking network composite materials, through the combination of alginate, polymer and metal ions, different metal ions are used to form a non-covalent crosslinking structure with different metal ions introduction methods to ensure the integrity and uniformity of the microparticle structure, and prepare It is an injection, gel or lyophilized sponge sample to suit different applications.

Benefits of technology

The tight embedding and uniform distribution of the particles loaded with decellularized matrix is ​​achieved, and the natural structure of the particles is maintained, which provides good antibacterial properties, water retention, mechanical properties and self-healing properties, simplifies the operation process, expands the application scenarios and field.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119075011A_ABST
    Figure CN119075011A_ABST
Patent Text Reader

Abstract

The invention relates to a physical cross-linked network composite material loaded with acellular matrix particles, and belongs to the technical field of biomedical materials. According to the invention, acellular matrix particles are uniformly embedded and loaded by using a high-molecular polymer system such as alginate, and three metal ion introduction modes can be selected to form a physical cross-linked structural framework mainly depending on the characteristic that alginate and metal cations are easy to be subjected to ionic cross-linking; on the basis, other high-molecular polymers can be further introduced. Through crosslinking of various non-covalent bonds between polymers and metal ions and between the polymers, the polymers in the system are interspersed and wound to form a semi-interpenetrating and interpenetrating polymer three-dimensional network structure, so that the network composite material loaded with acellular matrix particles is obtained.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of biomedical materials and relates to a physical cross-linked network composite material loaded with decellularized matrix particles. Background Art

[0002] Acellular matrix is ​​a natural extracellular matrix material processed by decellularization technology, mainly including collagen, adhesion molecules, glycosaminoglycans, bioactive functional molecules, etc. Acellular matrix particles have a biological three-dimensional grid structure and have removed immunogenic substances. The natural microstructure and crude fiber morphology are completely preserved. It also contains a variety of growth factors, which can provide a microenvironment close to nature, which is conducive to the growth and proliferation of cells and exerts an endogenous induction regeneration effect, promotes collagen regeneration, and provides a long-term tissue repair effect.

[0003] Hydrogel is a three-dimensional structure with high water content, similar to the extracellular matrix. The porous structure is conducive to the diffusion of macromolecular substances, allowing the decellularized matrix to be embedded and loaded. Alginate is a linear long-chain anionic polymer formed by the polymerization of α-L-guluronic acid and β-D-mannuronic acid through 1-4 glycosidic bonds. The carboxyl groups on it can form a cross-linked "egg-box" structure with a variety of metal cations. It is non-toxic, biocompatible, and biostable. It has been widely used in dressings, drug sustained release, filling and other fields.

[0004] Chinese patent CN101366978A discloses an injectable microparticle tissue filling material and a preparation method thereof, wherein the microparticle-decellularized biological derivative material is first mixed with a sustained-release microsphere containing a drug, and then calcium chloride is added thereto in the form of a coagulant, and then quickly mixed with a sodium alginate gel solution before use and injected as soon as possible, and the shaping is completed within 3 minutes. The patent contains drug sustained-release microspheres, but the calcium ions are directly mixed with the sodium alginate solution, which is easy to be uneven, and the gelling speed is very fast, which makes the operation difficult.

[0005] Chinese patent CN114159625A discloses a composite hydrogel and its preparation method and application. The invention includes alginate hydrogel and decellularized matrix hydrogel. The decellularized matrix hydrogel uses glutamine aminotransferase to catalyze the formation of isopeptide bonds between decellularized matrices, chemically cross-linking, and then mixing with alginate hydrogel to prepare the composite hydrogel. The alginate hydrogel is also directly introduced into the gel with metal cations, and the chemically cross-linked decellularized matrix hydrogel is changed in natural microstructure and crude fiber morphology compared to the decellularized matrix particles, and is more suitable for corneal applications.

[0006] Chinese patent CN114949359A discloses a decellularized matrix microparticle filler and a preparation method thereof, wherein a mixed gel phase comprising a cross-linked gel phase and a non-cross-linked gel phase is used as a carrier of the decellularized matrix microparticles, wherein the cross-linked gel phase uses a chemical cross-linking agent of glutaraldehyde, EDC, BDDE, PEGDE, and genipin, and the preparation process first forms a gel phase and then mixes it with the decellularized matrix microparticles for homogeneity.

[0007] Chinese patent CN108478868A discloses a method for preparing injectable allogeneic adipose decellularized matrix microparticles and their application, wherein human-derived fat particles are processed to obtain adipose decellularized matrix microparticles, and adipose decellularized matrix hydrogels are prepared by ultraviolet light, electron beam, gamma ray radiation or pepsin treatment to form gels, or chemical crosslinking agents. The natural microstructure of the decellularized matrix is ​​changed and provided in the form of a gel.

[0008] In summary, in the application of decellularized matrix, there are strategies such as using polymer gel phase as particle carrier or preparing decellularized matrix as gel, including non-cross-linked suspension system, chemically cross-linked gel system, physically cross-linked gel system, etc. However, there is still room for improvement in terms of system uniformity and stability, injectability, combination strategy of gel and particles, and maintaining the natural structure and components of decellularized matrix intact. Summary of the invention

[0009] The object of the present invention is to provide a physically cross-linked network composite material loaded with decellularized matrix particles, which has the characteristics of multiple functional properties.

[0010] The purpose of the present invention can be achieved through the following technical solutions: A physically cross-linked network composite material loaded with decellularized matrix particles, the composite material formula comprising: decellularized matrix particles, alginate, high molecular polymer, metal ions, and solvent; The method for preparing the decellularized matrix microparticles is as follows: S1.1: Disinfection and inactivation: clean the raw tissue, use a mixed aqueous solution of 1% peracetic acid and 20% ethanol, and soak it in ultrasound at 25°C for 1 hour; S1.2: Degrease by ultrasonic immersion in 95% ethanol at 25°C for 6 h, and then ultrasonically clean the surface three times with purified water or PBS; S1.3: Decellularization: subject the product obtained in step S1.2 to two freeze-thaw cycles at -20°C and 25°C, soak in a mixed aqueous solution containing 0.05% trypsin and 0.03% EDTA at 36°C for 45 min, then use PBS for ultrasonic cleaning three times, ultrasonically treat in a 3% sodium chloride hypertonic solution at 36°C for 45 min, wash with water three times, ultrasonically treat in a 25 mM NaOH aqueous solution at 36°C for 40 min, and finally wash with water or PBS at 25°C until neutral; S1.4: freeze drying, vacuum freeze drying the decellularized product, the vacuum freeze drying parameters are drying at -40°C for 4 h, drying at -25°C for 8 h, drying at -5°C for 8 h, drying at 10°C for 8 h, and drying at 30°C for 6 h; S1.5: Granulation: Cut the freeze-dried decellularized matrix into pieces, freeze-crush with liquid nitrogen, and sieve to obtain decellularized matrix microparticles; S1.6: sterilization, sterilizing the decellularized matrix microparticles by irradiation with cobalt 60 at 25 kGy to obtain the decellularized matrix microparticles; Wherein, the alginate is one or more of sodium alginate and its derivatives; Wherein, the high molecular polymer is one or more of chitosan and its derivatives, cellulose derivatives, sodium hyaluronate and its derivatives, polyvinyl pyrrolidone, sodium polyacrylate, water-soluble starch, carbomer, polyvinyl alcohol, polyethylene glycol, carboxymethyl konjac glucan, gelatin, silk fibroin, and chondroitin sulfate; Wherein, the metal ion is a soluble metal ion solution or a metal compound; The solvent is one or more of glycerol, saline, phosphate buffer, and water for injection. The composite material preparation method is as follows: S2.1: Dissolve alginate and high molecular polymer in a solvent in proportion at 25-100°C with stirring at a rate of 150 r / min for 1 h, and then perform ultrasound after stirring for 0.5-2 h to prepare a mixed solution A; S2.2: Add the acellular matrix microparticles to the mixed solution A obtained in step S2.1, stir at room temperature at a speed of 150 r / min, stir evenly, and then ultrasonicate for 0.5 to 2 h to obtain a suspension B; S2.3: Introducing metal ions into the suspension B to obtain the composite material.

[0011] Furthermore, the raw material tissue of the decellularized matrix particles in S1.1 is one of fish skin and mammalian skin, small intestine, pericardium, Achilles tendon, fascia, and diaphragm, Furthermore, the size of the decellularized matrix particles prepared in S1.6 is 30-400 μm.

[0012] Furthermore, the soluble metal ion solution is one or more of calcium chloride solution, calcium sulfate solution, zinc sulfate solution, and zinc chloride solution.

[0013] Furthermore, the metal compound is one or more of calcium carbonate, β-tricalcium phosphate, calcium hydrogen phosphate, hydroxyapatite, and ethylenediaminetetraacetic acid-calcium.

[0014] Furthermore, the metal ion introduction method in S2.3 includes method ① direct dripping method, method ② external gel method and method ③ internal gel method.

[0015] Furthermore, the method ① direct dropwise addition is to directly dropwise add a soluble metal ion solution with a concentration of 0.1 mol / L into the suspension B at a temperature of 4-50°C.

[0016] Furthermore, the external gel method of method ② is to freeze the suspension B, and the freezing treatment parameters are a temperature of -20°C, a duration of 12 hours, and then soak it in a 0.05~0.2mol / L soluble metal ion solution, a soaking time of 12~24 hours, and a soaking temperature of 20~30°C.

[0017] Furthermore, the method ③ internal gelation method is to introduce a metal compound into the suspension B, wherein the mass ratio of alginate to the metal contained in the metal compound is 1:(0.02~0.1), stirring at 20~30°C at a speed of 150r / min for 0.5h, and then ultrasonicating for 0.5~1h, and introducing glucono-δ-lactone GDL during gelation, wherein the molar ratio of GDL to the metal contained in the metal compound is (0.5~2):1, and continuing to stir rapidly at a speed of 150r / min.

[0018] A physical cross-linked network composite material loaded with decellularized matrix particles, including injection, gel-like, and freeze-dried sponge-like forms. The finished product can be used in the following ways: direct application of the gel-like, pushing out through a 27G needle of a syringe, and freeze-drying the gel-like (24-72 hours) to obtain a sponge-like solid.

[0019] The polymer network composite material loaded with acellular matrix particles in the present invention can have a variety of properties by adopting different combination schemes: such as physical cross-linking without destroying the structure and composition of the particles; the particles are tightly embedded without sedimentation and the load is uniform; the composite material is injectable or in situ phase-transformed into a gel after injection; the antibacterial properties, water retention, mechanical properties, self-healing properties, degradation properties, viscosity and other properties are regulated; it has the effects of instant filling of cross-linked polymers and endogenous induced regeneration of particles; it can be prepared into various forms such as injections, gel-like, freeze-dried sponge-like, etc. This composite material includes but is not limited to the above multiple functional characteristics, and a flexible combination scheme can be adopted according to the actual application, thereby improving the use effect of the polymer matrix material and expanding the application scenarios and fields of acellular matrix particles.

[0020] The purpose of the present invention is to improve the problems and defects existing in the prior art, and to provide a scheme for embedding and loading decellularized matrix microparticles by cross-linking high molecular polymers by physical methods. The prepared composite material has multiple functional properties, combines the advantages of physically cross-linked high molecular polymers and decellularized matrix microparticles, improves the use effect of polymer matrix materials, and expands the application scenarios and fields of decellularized matrix microparticles.

[0021] The decellularized matrix particles and the high molecular polymer are first mixed evenly and then cross-linked. This method can load the decellularized matrix particles tightly and firmly in the polymer matrix. The cross-linked polymer has a better loading effect on the particles, which improves the sedimentation and unevenness of the particles in the system. The cross-linking is carried out by a simple physical method without the introduction of chemical cross-linking agents, which will not destroy the natural microstructure and components in the decellularized matrix particles. Therefore, the decellularized matrix particles are retained to facilitate cell growth and proliferation, exert endogenous induction of regeneration, and provide long-term repair effects.

[0022] All three methods of introducing metal ions can complete ion crosslinking under mild conditions. Methods ① and ② directly gel the metal ions with polymers, which is a rapid process and prone to uneven crosslinking and ion concentration gradient distribution, but the preparation process is relatively simpler. Method ③ uses glucono-δ-lactone (GDL) to slowly and evenly replace metal ions in metal compounds such as calcium carbonate, and form gels uniformly in situ inside the polymer system, solving the problems of excessive local gelation and uneven colloid embedding of decellularized matrix microparticles caused by direct introduction of metal ions; and GDL has a slow reaction replacement rate at low temperatures, and can form gels within 5-60 minutes at 37°C, realizing that the polymer suspension system loaded with decellularized matrix microparticles is converted into a molded gel in situ at 37°C after injection; because this physical crosslinking method has certain self-healing properties, when the polymer and metal ions are within a specific concentration range, even after crosslinking and gelation, it can be extruded through a 27G needle in the form of a linear gel.

[0023] Composite materials prepared by non-covalent physical methods mainly rely on ionic crosslinking. According to the properties of different polymers, some polymers can interact with metal ions, and some polymers also contain other possible non-covalent bonds, such as electrostatic interactions between polyelectrolyte polymers, and hydrogen bonds between amino and carboxyl groups on the molecular chain, thereby forming possible weak interactions such as electrostatic interactions, hydrogen bonds, van der Waals forces, and hydrophilic and hydrophobic interactions. The mixed system of decellularized matrix particles and polymer matrix is ​​crosslinked by metal ions and other physical interactions, so that the polymer matrix in the system is interpenetrated and entangled to form a semi-interpenetrating and interpenetrating polymer three-dimensional network structure loaded with decellularized matrix particles. Due to the presence of physical crosslinking points, the mechanical properties of the entire system are improved and the polymer network is more compact, so it has better instant filling effect when used for filling, and better mechanical properties and covering protection effect when used for dressings.

[0024] Depending on the types of metal ions and polymers selected, as well as the type and particle size of the decellularized matrix particles, the method of introducing metal ions and other conditions, the different properties of the network composite system can be regulated, such as antibacterial properties, water retention, mechanical properties, self-healing properties, degradation properties, viscosity, etc., and the appropriate preparation scheme can be selected according to the specific situation, thereby improving and enhancing the actual application effect of the decellularized matrix.

[0025] The network composite material can be prepared into different forms such as injection, gel, freeze-dried sponge, etc., suitable for different applications. For example, injection and gel are suitable for injection, filling, sealing agent, etc.; freeze-dried sponge is suitable for hemostasis and dressing, etc. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] In order to facilitate understanding by those skilled in the art, the present invention is further described below with reference to the accompanying drawings.

[0027] Figure 1 This is a state diagram of the introduction of calcium ions into the mixed system of microparticles and polymers before and after cross-linking using method ①; Figure 2 This is a state diagram of the introduction of zinc ions into the mixed system of microparticles and polymers before and after crosslinking using method ①; Figure 3 This is the state diagram after the mixed system of particles and polymers is placed in a solution of calcium ions and zinc ions to form gel by adopting method ②; Figure 4 The state diagram of the CaCO3-GDL introduced into the mixed system of particles and polymers before and after cross-linking by using method ③; Figure 5 The gel system prepared by method ③ is left at room temperature for 24 hours; Figure 6To introduce CaCO3-GDL into the microparticle and polymer mixed system before and after crosslinking through the different states of the 27G syringe needle; Figure 7 This is an example of the composite material of the CaCO3-GDL system cross-linked being injected through a 27G needle; Figure 8 It is a sponge-like solid obtained by freeze-drying the cross-linked gel composite material. DETAILED DESCRIPTION

[0028] In order to further explain the technical means and effects adopted by the present invention to achieve the predetermined invention purpose, the specific implementation methods, structures, features and effects of the present invention are described in detail below in conjunction with the accompanying drawings and preferred embodiments.

[0029] The abbreviations of materials used in the examples are: SA (sodium alginate), CMC (sodium carboxymethyl cellulose), PVP (polyvinyl pyrrolidone), CMCS (carboxymethyl chitosan), HA (sodium hyaluronate), PAA-Na (sodium polyacrylate), GDL (gluconolactone), and SIS (porcine small intestinal submucosa).

[0030] The method for preparing the decellularized matrix microparticles is as follows: S1.1: Disinfection and inactivation: clean the submucosal tissue of the pig small intestine, use a mixed aqueous solution of 1% peracetic acid and 20% ethanol, and soak it in ultrasound at 25°C for 1 hour; S1.2: Degrease by ultrasonic immersion in 95% ethanol at 25°C for 6 h, and then ultrasonically clean the surface three times with purified water or PBS; S1.3: Decellularization: the product obtained in step S1.2 was first subjected to 2 freeze-thaw cycles, and then ultrasonically soaked in a mixed aqueous solution containing 0.05% trypsin and 0.03% EDTA at 36°C for 45 minutes, and then ultrasonically cleaned with PBS for 3 times, and then ultrasonically treated in a 3% sodium chloride hypertonic solution at 36°C for 45 minutes, and then washed with water for 3 times, and then ultrasonically treated in a 25 mM NaOH aqueous solution at 36°C for 40 minutes, and finally washed with water or PBS at 25°C until neutral; S1.4: freeze drying, vacuum freeze drying the decellularized product, the vacuum freeze drying parameters are drying at -40°C for 4 h, drying at -25°C for 8 h, drying at -5°C for 8 h, drying at 10°C for 8 h, and drying at 30°C for 6 h; S1.5: Granulation: Cut the freeze-dried decellularized matrix into pieces, freeze-crush with liquid nitrogen, and sieve to obtain decellularized matrix microparticles; S1.6: Sterilization: sterilize the decellularized matrix microparticles by radiation sterilization with cobalt 60 at 25 kGy to obtain the decellularized matrix microparticles.

[0031] Example 1 This embodiment adopts the method ① to introduce calcium ions to prepare a cross-linked composite material. S2.1: Add 2.5%wt SA, 2%wt SA+0.5%wt CMC, 2%wt SA+1%wt PVP, 2%wt SA+1%wt CMCS, 2%wt SA+0.5%wt HA, 2%wt SA+0.5%wt PAA-Na polymers to a solvent at 40°C, respectively, stir to dissolve, stirring at a rate of 150 r / min for 1 h, and perform ultrasound after stirring for 30 min to prepare a uniform mixed solution A; S2.2: Add 1%wt of SIS particles with a particle size of 100-250μm to the mixed solution A in S2.1, stir at 150r / min at room temperature, and ultrasonicate for 1h to obtain a uniform suspension B; S2.3: The suspension B in S2.2 was added dropwise with 25% v / w of 0.1 mol / L calcium chloride aqueous solution under stirring at room temperature to obtain a calcium ion cross-linked gel composite material.

[0032] Example 2 Method ① is to introduce zinc ions to prepare cross-linked composite materials.

[0033] S2.1: Add 2.5%wt SA, 2%wt SA+0.5%wt CMC, 2%wt SA+1%wt PVP, 2%wt SA+1%wt CMCS, 2%wt SA+0.5%wt HA, 2%wt SA+0.5%wt PAA-Na polymers to a 40°C solvent, stir to dissolve, stirring at a rate of 150 r / min for 1 h, and perform ultrasound after stirring for 30 min to prepare a uniform mixed solution A; S2.2: Add 1%wt of SIS particles with a particle size of 100-250μm to the mixed solution A in S2.1, stir at 150r / min at room temperature, and ultrasonicate for 1h to obtain a uniform suspension B; S2.3: 25% v / w 0.1 mol / L zinc chloride aqueous solution was added dropwise to the suspension B in S2.2 under stirring at room temperature to obtain a zinc ion cross-linked gel composite material.

[0034] Example 3 Method ② is adopted to introduce calcium ions and zinc ions into the mixed system of particles and polymers for cross-linking to prepare a composite material.

[0035] S2.1: Add 2.5%wt SA, 2%wt SA+0.5%wt CMC, 2%wt SA+1%wt PVP, 2%wt SA+1%wt CMCS, 2%wt SA+0.5%wt HA, 2%wt SA+0.5%wt PAA-Na polymers to a 40°C solvent, stir to dissolve, stirring at a rate of 150 r / min for 1 h, and perform ultrasound after stirring for 30 min to prepare a uniform mixed solution A; S2.2: Add 1%wt of SIS particles with a particle size of 100-250μm to the mixed solution A in S2.1, stir at 150r / min at room temperature, and ultrasonicate for 1h to obtain a uniform suspension B; S2.3: After freezing the suspension B in S2.2 at -20°C for 8 hours, the suspension was placed in 0.1 mol / L calcium chloride and zinc chloride aqueous solutions respectively and immersed at room temperature for 12 hours to obtain a gel composite material cross-linked by calcium ions and zinc ions.

[0036] Example 4 Method ③ was adopted to prepare composite materials by introducing calcium ion cross-linking through the CaCO3-GDL system.

[0037] S2.1: Add 2.5%wt SA, 2%wt SA+0.5%wt CMC, 2%wt SA+0.5%wt PVP, 2%wt SA+0.5%wt CMCS, 2%wt SA+0.5%wt HA, and 2%wt SA+0.5%wt PAA-Na polymers to a 40°C solvent, stir to dissolve, the stirring rate is 150r / min, the stirring time is 1h, and ultrasonication is performed after stirring for 30min to prepare a uniform mixed solution A; S2.2: Add 1%wt of SIS particles with a particle size of 100-250μm to the mixed solution A in S2.1, stir at 150r / min at room temperature, and ultrasonicate for 1h to obtain a uniform suspension B; S2.3: Add 0.4%wt of light calcium carbonate powder to suspension B in S2.2, stir evenly at room temperature, and ultrasonicate for 1h to obtain a uniform suspension system; S2.4: Add 1.5 times the molar number of calcium carbonate GDL to the suspension system in S2.3, and stir rapidly at room temperature to mix evenly; S2.5: The suspension system was placed at 37°C and allowed to gel in 60 minutes.

[0038] Example 5 The sponge-like composite material was prepared by cross-linking the gel by CaCO3-GDL system. S2.1: Add 2.5%wt SA, 2%wt SA+0.5%wt CMC, 2%wt SA+0.5%wt PVP, 2%wt SA+0.5%wt CMCS, 2%wt SA+0.5%wt HA, and 2%wt SA+0.5%wt PAA-Na polymers to a 40°C solvent, stir to dissolve, the stirring rate is 150r / min, the stirring time is 1h, and ultrasonication is performed after stirring for 30min to prepare a uniform mixed solution A; S2.2: Add 1%wt of SIS particles with a particle size of 200-300μm to the mixed solution A in S2.1, stir at 150r / min at room temperature, and ultrasonicate for 1h to obtain a uniform suspension B; S2.3: Add 0.4%wt of light calcium carbonate powder to the suspension B in step S2.2, stir evenly at room temperature, and ultrasonicate for 1h to obtain a uniform suspension system; S2.4: Add 1.5 times the molar number of calcium carbonate GDL to the suspension system in S2.3, stir and mix evenly at room temperature, pour into a culture dish, and place at 37°C for 60 minutes to obtain a gel sample; S2.5: The gel sample obtained in S2.4 is vacuum freeze-dried for 24 hours to obtain a porous sponge-like composite material.

[0039] Comparative Example 1 This comparative example does not use calcium chloride for crosslinking, and the remaining steps are consistent with Example 1.

[0040] Comparative Example 2 This comparative example does not use zinc chloride crosslinking, and the remaining steps are consistent with Example 2.

[0041] Comparative Example 3 In this comparative example, the S2.5 operation was not performed, that is, the cross-linking was not completed after the GDL suspension system was just added, and the remaining steps were consistent with Example 4.

[0042] Comparative Example 4 In this comparative example, operations S2.4 and S2.5 were not performed, that is, GDL was not added and cross-linking was not initiated. The remaining steps were consistent with those in Example 4.

[0043] The performance of the embodiments and comparative examples was tested: Viscosity of polymer solution system The dynamic viscosity of the polymer solution system of each component was tested using a rotational viscometer. The test conditions were: No. 2 rotor, room temperature, and a speed of 12 rpm. The test results are shown in Table 1. Table 1 Dynamic viscosity of different polymer solution systems.

[0044] The results showed that the viscosity of the three solutions containing CMC, HA, and PAA-Na was greater than that of the pure SA solution, and the viscosity of the two solutions containing CMCS and PVP was lower than that of the SA group. This may be related to the properties of the polymer materials, because the viscosity of the three polymers CMC, HA, and PAA-Na is many times greater than that of SA, so the viscosity of their mixture is also greater than that of the pure SA group.

[0045] Method ① Cross-linking into gel Examples 1 and 2 both adopted the ionic crosslinking method ①, and the results were as follows Figure 1 , 2 The figures show the states before and after the introduction of calcium chloride and zinc chloride, respectively. Comparative Examples 1 and 2 correspond to the flow state before cross-linking. The calcium ions and zinc ions introduced in Examples 1 and 2 immediately chelate the polymer segments at room temperature to interact with each other, and the cross-linked system solidifies into a gel composite material.

[0046] Method ② Cross-linking into gel Example 3: The ionic crosslinking was carried out by method ②. The cured gel composite material contained calcium ions and zinc ions respectively. The results after being placed in an open environment at room temperature for 20 days were as follows: Figure 3 As shown in the figure, the water loss of SA and PAA-Na groups is faster than that of the other four groups, which is related to the degree of binding between polymers and metal ions, the interaction between polymers, the movement of network segments, the hydrophilic and hydrophobic groups of molecular chains, etc. The water retention of the four composite materials containing CMC, PVP, CMCS, and HA will be stronger. In addition, the gel formed by calcium ions has bacteria growing, and the main component of decellularized matrix particles, collagen, and the high water content of the gel are easy to grow bacteria. The situation of the CMCS group is slightly better because CMCS has a corresponding inhibitory effect on certain bacteria and has a certain antibacterial effect; for the gel formed by zinc ions, due to the broad-spectrum antibacterial property of zinc ions, no bacteria grow in each group.

[0047] Method ③ Cross-linking into gel Example 4 adopts the ionic crosslinking method ③, and the results before and after crosslinking are as follows Figure 4 As shown. In each group of comparative example 3, the suspension after adding GDL failed to complete crosslinking, so it was still in a flowing state. After 50 minutes at 37°C, GDL slowly replaced enough calcium ions to form a solidified gel. Figure 4The SA group on the far left was prepared according to Comparative Example 4 and did not contain GDL, so even after 37°C, it could not be cross-linked and cured after 50 minutes. It was found that there were differences in gel curing between the groups. For example, one of the mechanism effects would make CMC and HA gel a little slower, probably because they are both anionic polysaccharides like SA, and the electrostatic repulsion between the two slowed down the gel formation. Similarly, carboxymethylated konjac glucomannan and the like would also produce similar effects. However, in the examples, all groups completed gel curing within 10 to 60 minutes at 37°C.

[0048] Loading capacity of polymer matrix on acellular matrix microparticles The uncrosslinked SA group prepared in Comparative Example 4 and the crosslinked gel groups prepared in Example 4 were left standing at room temperature for 24 hours. Figure 5 As shown, in the uncross-linked SA system on the far left, the SIS particles have precipitated, the solid and liquid have separated, and the system is no longer uniform; while the cross-linked systems can still fix the SIS particles in the gel network due to the improvement of mechanical properties, and no sedimentation occurs.

[0049] Injection via syringe with 27G needle Figure 6 and Figure 7 The composite material prepared using the CaCO3-GDL system is shown passing through a 27G needle. Figure 6 In the groups prepared according to Comparative Example 3, the suspension just after adding GDL failed to complete crosslinking, and was in a droplet state when squeezed out through a needle; after 50 minutes at 37°C, the system was crosslinked, and a linear gel was squeezed out through a needle. The uncrosslinked SA group prepared according to Comparative Example 4 was always in a droplet state. Figure 7 The cross-linked gel is pushed out of the needle in a more compact state, and the linear shape can directly self-heal into a mass by relying on the non-covalent bonds of the physical cross-linking, and has a certain shape plasticity. However, the uncross-linked SA group is pushed out of the needle in a rather loose state.

[0050] Freeze-dried sponge Figure 8 It shows that each group of cross-linked gel samples prepared according to Example 4, after 24 hours of vacuum freeze drying, all of them have removed moisture to form a porous sponge-like network composite material.

[0051] The above description is only a preferred embodiment of the present invention and does not limit the present invention in any form. Although the present invention has been disclosed as a preferred embodiment as above, it is not used to limit the present invention. Any technical personnel in this field can make some changes or modify the technical contents disclosed above into equivalent embodiments without departing from the scope of the technical solution of the present invention. However, any brief modifications, equivalent changes and modifications made to the above embodiments based on the technical essence of the present invention without departing from the content of the technical solution of the present invention are still within the scope of the technical solution of the present invention.

Claims

1. A physically cross-linked network composite material loaded with decellularized matrix particles, characterized in that: The composite material formula includes: decellularized matrix particles, alginate, high molecular polymer, metal ions, and solvent; The method for preparing the decellularized matrix microparticles is as follows: S1.1: Disinfection and inactivation: clean the raw tissue, use a mixed aqueous solution of 1% peracetic acid and 20% ethanol, and soak it in ultrasound at 25°C for 1 hour; S1.2: Degrease by ultrasonic immersion in 95% ethanol at 25°C for 6 h, and then ultrasonically clean the surface three times with purified water or PBS; S1.3: Decellularization: subject the product obtained in step S1.2 to two freeze-thaw cycles at -20°C and 25°C, soak in a mixed aqueous solution containing 0.05% trypsin and 0.03% EDTA at 36°C for 45 min, then use PBS for ultrasonic cleaning three times, ultrasonically treat in a 3% sodium chloride hypertonic solution at 36°C for 45 min, wash with water three times, ultrasonically treat in a 25 mM NaOH aqueous solution at 36°C for 40 min, and finally wash with water or PBS at 25°C until neutral; S1.4: freeze drying, vacuum freeze drying the decellularized product, the vacuum freeze drying parameters are drying at -40°C for 4 h, drying at -25°C for 8 h, drying at -5°C for 8 h, drying at 10°C for 8 h, and drying at 30°C for 6 h; S1.5: Granulation: Cut the freeze-dried decellularized matrix into pieces, freeze-crush with liquid nitrogen, and sieve to obtain decellularized matrix microparticles; S1.6: sterilization, sterilizing the decellularized matrix microparticles by irradiation with cobalt 60 at 25 kGy to obtain the decellularized matrix microparticles; Wherein, the alginate is one or more of sodium alginate and its derivatives; Wherein, the high molecular polymer is one or more of chitosan and its derivatives, cellulose derivatives, sodium hyaluronate and its derivatives, polyvinyl pyrrolidone, sodium polyacrylate, water-soluble starch, carbomer, polyvinyl alcohol, polyethylene glycol, carboxymethyl konjac glucan, gelatin, silk fibroin, and chondroitin sulfate; Wherein, the metal ion is a soluble metal ion solution or a metal compound; Wherein, the solvent is one or more of glycerol, physiological saline, phosphate buffer, and water for injection; The composite material preparation method is as follows: S2.1: Dissolve alginate and high molecular polymer in a solvent in proportion at 25-100°C with stirring at a rate of 150 r / min for 1 h, and then perform ultrasound after stirring for 0.5-2 h to prepare a mixed solution A; S2.2: Add the acellular matrix microparticles to the mixed solution A obtained in step S2.1, stir at room temperature at a speed of 150 r / min, stir evenly, and then ultrasonicate for 0.5 to 2 h to obtain a suspension B; S2.3: Introducing metal ions into the suspension B to obtain the composite material.

2. The physically cross-linked network composite material loaded with acellular matrix particles according to claim 1, characterized in that: The raw material tissue of the decellularized matrix particles in S1.1 is one of fish skin and mammalian skin, small intestine, pericardium, Achilles tendon, fascia, and diaphragm.

3. The physically cross-linked network composite material loaded with acellular matrix particles according to claim 1, characterized in that: The size of the decellularized matrix particles prepared in S1.6 is 30-400 μm.

4. The physically cross-linked network composite material loaded with acellular matrix particles according to claim 1, characterized in that: The soluble metal ion solution is one or more of calcium chloride solution, calcium sulfate solution, zinc sulfate solution and zinc chloride solution.

5. The physically cross-linked network composite material loaded with acellular matrix particles according to claim 1, characterized in that: The metal compound is one or more of calcium carbonate, β-tricalcium phosphate, calcium hydrogen phosphate, hydroxyapatite, and ethylenediaminetetraacetic acid-calcium.

6. The physically cross-linked network composite material loaded with acellular matrix particles according to claim 1, characterized in that: The metal ion introduction method in S2.3 includes method ① direct dripping method, method ② external gelation method and method ③ internal gelation method.

7. The physically cross-linked network composite material loaded with acellular matrix particles according to claim 6, characterized in that: The method ① direct dropwise addition is to dropwise add a soluble metal ion solution with a concentration of 0.1 mol / L directly into the suspension B at a temperature of 4-50°C.

8. The physically cross-linked network composite material loaded with acellular matrix particles according to claim 6, characterized in that: The method ② external gel method is to freeze the suspension B, the freezing treatment parameters are temperature of -20°C, time of 12 hours, and then soak in 0.05~0.2mol / L soluble metal ion solution, soaking time of 12~24h, soaking temperature of 20~30°C.

9. The physically cross-linked network composite material loaded with acellular matrix particles according to claim 6, characterized in that: The method ③ of the internal gel method is to introduce a metal compound into the suspension B, wherein the mass ratio of alginate to the metal contained in the metal compound is 1:(0.02~0.1), stir at 20~30°C at a speed of 150r / min for 0.5h, and then perform ultrasound for 0.5~1h. During gelation, glucono-δ-lactone GDL is introduced, wherein the molar ratio of GDL to the metal contained in the metal compound is (0.5~2):1, and continue to stir rapidly at a speed of 150r / min.

10. A use form of the physically cross-linked network composite material loaded with acellular matrix particles according to any one of claims 1 to 9, characterized in that: It includes injection, gel-like, and freeze-dried sponge-like usage forms.

Citation Information

Patent Citations

  • Fine particle tissue hydraulic fill for injection and preparation method thereof

    CN101366978A

  • Preparation method and application of injectable allogeneic adipose acellular matrix particles

    CN108478868A

  • Composite hydrogel as well as preparation method and application thereof

    CN114159625A

  • Acellular matrix particle filler and preparation method thereof

    CN114949359A

  • Hernia bioremediation mesh and preparation method thereof

    CN109248339A

Cited By

  • Injectable self-healing conductive hydrogel as well as preparation method and application thereof

    CN119701080A