Low-dimensional transition metal carbide adsorption filter membrane for recycling silver electrolysis waste liquid as well as preparation method and application of low-dimensional transition metal carbide adsorption filter membrane
By preparing low-dimensional transition metal carbide adsorption filter membrane, the problem of difficult recycling of small particles in silver electrolytic waste liquid is solved, and efficient silver recycling is achieved, with stable chemical properties and large specific surface area, and the silver recovery rate reaches 98%~99.5 %.
Patent Information
- Application Number
- CN202411226990.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-03
- Publication Date
- 2024-12-06
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
At this stage, small and particulate metal silver in silver electrolytic waste liquid is difficult to effectively recycle, resulting in increased waste of precious metals and wastewater treatment difficulties.
The preparation method of low-dimensional transition metal carbide adsorption filter membrane is adopted. By mixing transition metal oxide, alumina and graphite in a set proportion, molten salt electrolysis and interface selection etching are performed, the aluminum intercalation is removed, and the surface is modified. Form a low-dimensional transition metal carbide adsorbent for adsorption and enrichment of silver ions or particles in silver electrolytic waste liquid.
It realizes efficient recycling of silver in silver electrolytic waste liquid, has stable chemical properties and large specific surface area, and the silver recovery rate reaches 98%~99.5%, simplifying the recycling process.
Smart Images

Figure CN119075698A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of silver electrolysis waste liquid recovery, and in particular relates to a low-dimensional transition metal carbide adsorption filter membrane for recovering silver electrolysis waste liquid, and a preparation method and application thereof. Background Art
[0002] The production of high-purity silver in my country mainly adopts processes such as electrolytic refining and chemical reduction. Through multiple refining and purification, the purity of silver materials is gradually improved. In the process of silver smelting, the silver electrolytic waste liquid produced contains a large amount of metallic silver. Due to the high value of metallic silver, the recovery of metallic silver from the silver electrolytic waste liquid has become an urgent problem to be solved in the current industry.
[0003] The copper replacement method and sodium hydroxide neutralization method commonly used at this stage will produce a large number of extremely fine silver particles. The replaced small particles of metallic silver are difficult to enrich and recover, resulting in a huge waste of precious metals. It also increases the difficulty of subsequent wastewater treatment. Summary of the invention
[0004] In view of this, some embodiments disclose a method for preparing a low-dimensional transition metal carbide adsorption filter membrane for recovering silver electrolysis waste liquid, comprising the steps of:
[0005] S1. Mix transition metal oxides, aluminum oxide and graphite according to a set ratio, press and consolidate the sample to obtain a mixed sample block;
[0006] S2, subjecting the mixed sample block to molten salt electrolysis to obtain transition metal carbides with aluminum intercalation;
[0007] S3, performing interface selective etching on the transition metal carbide with aluminum intercalation to remove the aluminum intercalation to obtain a low-dimensional transition metal carbide;
[0008] S4, using a surface modifier to perform surface modification on the low-dimensional transition metal carbide, and then dispersing the low-dimensional transition metal carbide in ethanol or water to obtain a low-dimensional transition metal carbide adsorbent;
[0009] S5. Filter and dry the low-dimensional transition metal carbide adsorbent to obtain a low-dimensional transition metal carbide adsorption filter membrane.
[0010] Some embodiments disclose a method for preparing a low-dimensional transition metal carbide adsorption filter membrane for recovering silver electrolysis waste liquid, wherein the molar ratio of transition metal oxide, aluminum oxide and graphite is 3:1:2-4.
[0011] Some embodiments disclose a method for preparing a low-dimensional transition metal carbide adsorption filter membrane for recovering silver electrolysis waste liquid, wherein the transition metal includes one or more of vanadium, titanium, zirconium, chromium, molybdenum, and tungsten.
[0012] Some embodiments disclose a method for preparing a low-dimensional transition metal carbide adsorption filter membrane for recovering silver electrolysis waste liquid, wherein the molten salt electrolyte selected for molten salt electrolysis in step S2 is a calcium-based Lewis acid electrolyte, and the electrolysis temperature is 850°C.
[0013] In some embodiments, the method for preparing a low-dimensional transition metal carbide adsorption filter membrane for recovering silver electrolysis waste liquid disclosed in step S3 specifically comprises:
[0014] The transition metal carbide with aluminum intercalation is set to react in a high-temperature chloride molten salt, the aluminum intercalation is dissolved in the chloride molten salt, and reacts with the chloride molten salt to generate AlCl3, thereby obtaining a low-dimensional transition metal carbide.
[0015] Some embodiments disclose a method for preparing a low-dimensional transition metal carbide adsorption filter membrane for recovering silver electrolysis waste liquid, wherein the chloride molten salt includes one or more of cobalt chloride, copper chloride, nickel chloride, and zinc chloride.
[0016] In some embodiments, the method for preparing a low-dimensional transition metal carbide adsorption filter membrane for recovering silver electrolysis waste liquid disclosed in step S3 specifically comprises:
[0017] By utilizing the water flow field leaching mechanism, a transition metal carbide with a metal aluminum intercalation layer is placed in a leaching solution to obtain a low-dimensional transition metal carbide, wherein the leaching solution includes hydrofluoric acid, a pH-adjusted acidic lithium chloride solution, and a KOH solution.
[0018] Some embodiments disclose a method for preparing a low-dimensional transition metal carbide adsorption filter membrane for recovering silver electrolysis waste liquid, wherein the surface modifier comprises a KOH solution, a LiOH solution, a HCl solution or a HF solution.
[0019] Some embodiments disclose a low-dimensional transition metal carbide adsorption filter membrane for recovering silver electrolysis waste liquid, which is prepared by the above-mentioned preparation method.
[0020] Some embodiments disclose an application of a low-dimensional transition metal carbide adsorption filter membrane for recovering silver electrolysis waste liquid, wherein the low-dimensional transition metal carbide adsorption filter membrane is used to enrich silver in the silver electrolysis waste liquid.
[0021] The low-dimensional transition metal carbide adsorption filter membrane for recovering silver electrolysis waste liquid disclosed in the embodiment of the present invention has stable chemical properties and a large specific surface area, has excellent adsorption affinity and reducibility to silver ions or silver particles, can be used as a good filtration medium, and can realize simple and convenient recovery of metallic silver from silver electrolysis waste liquid. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] Figure 1 Example 1: Microscopic morphology of low-dimensional transition metal carbide;
[0023] Figure 2 Example 3: Microscopic morphology of low-dimensional transition metal carbide adsorption filter membrane. DETAILED DESCRIPTION
[0024] The word "embodiment" used here as an "exemplary" does not necessarily mean that any embodiment described is superior to or better than other embodiments. Unless otherwise specified, the performance index tests in the embodiments of this application are performed using conventional test methods in the art. It should be understood that the terms described in this application are only used to describe specific implementation methods and are not used to limit the content disclosed in this application.
[0025] Unless otherwise specified, the technical and scientific terms used in this document have the same meanings as commonly understood by ordinary technicians in the technical field to which this application belongs; other experimental methods and technical means not specifically specified in this application refer to experimental methods and technical means commonly used by ordinary technicians in this field.
[0026] The terms "substantially" and "approximately" used herein are used to describe small fluctuations. For example, they can refer to less than or equal to ±5%, such as less than or equal to ±2%, such as less than or equal to ±1%, such as less than or equal to ±0.5%, such as less than or equal to ±0.2%, such as less than or equal to ±0.1%, such as less than or equal to ±0.05%. The numerical data represented or presented in the range format herein are used only for convenience and brevity, and should therefore be flexibly interpreted as including not only the values clearly listed as the limits of the range, but also all independent values or sub-ranges contained in the range. For example, the numerical range of "1-5%" should be interpreted as including not only the clearly listed values of 1% to 5%, but also the independent values and sub-ranges within the range shown. Therefore, independent values such as 2%, 3.5% and 4% and sub-ranges such as 1%-3%, 2%-4% and 3%-5% are included in this numerical range. This principle also applies to the range of only one numerical value. In addition, such an interpretation applies regardless of the width of the range or the characteristics described.
[0027] In this document, including in the claims, transitional words such as "comprises," "includes," "with," "having," "containing," "involving," "accommodating," etc. are understood to be open-ended, i.e., meaning "including but not limited to." Only the transitional words "consisting of" and "composed of" are closed transitional words.
[0028] In order to better illustrate the content of the present application, numerous specific details are provided in the specific examples below. It should be understood by those skilled in the art that the present application can also be implemented without certain specific details. In the embodiments, some methods, means, instruments, equipment, etc. well known to those skilled in the art are not described in detail in order to highlight the main purpose of the present application.
[0029] Under the premise of no conflict, the technical features disclosed in the embodiments of the present application can be arbitrarily combined, and the obtained technical solutions belong to the contents disclosed in the embodiments of the present application. It should be noted that the terms "center", "longitudinal", "lateral", "up", "down", "front", "back", "left", "right", "vertical", "horizontal", "top", "bottom", "inside", "outside" and the like mentioned in the present application indicate the orientation or position relationship based on the orientation or position relationship shown in the accompanying drawings, which is only for the convenience of describing the technical features and simplifying the description, rather than indicating or implying that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as a limitation of the present invention, unless it conflicts with the context. In addition, the terms "first" and "second" are only used for descriptive purposes and cannot be understood as indicating or implying relative importance, unless it conflicts with the context.
[0030] In some embodiments, the method for preparing a low-dimensional transition metal carbide adsorption filter membrane for recovering silver electrolysis waste liquid comprises the steps of:
[0031] S1. Mix transition metal oxides, alumina and graphite according to a set ratio, press and consolidate the samples to obtain a mixed sample block; generally, the transition metal oxides can be selected from transition metal oxide waste as raw materials, for example, analytical pure chemical reagents, waste denitrification catalysts, high titanium slag or vanadium slag and other solid wastes;
[0032] S2. The mixed sample block is subjected to molten salt electrolysis. During the electrolysis process, the structures of the oxides are broken and reorganized. Oxygen enters the molten salt in the form of ions to form oxygen or carbon oxides at the anode. The metal remaining at the cathode undergoes carbothermal reduction and solid-phase diffusion reaction under the action of the double reduction potential of electrons and carbon, thereby obtaining a transition metal carbide with an aluminum intercalation layer.
[0033] S3, selectively etching the interface of the transition metal carbide with aluminum intercalation to remove the aluminum intercalation to obtain a low-dimensional transition metal carbide; the low-dimensional transition metal carbide has an excellent micro-nano structure and a functional group-rich surface, which can provide a large specific surface area, high thermal stability and chemical stability, and its surface functional group also has the unique advantage of adjustable design;
[0034] S4, using a surface modifier to modify the surface of the low-dimensional transition metal carbide, introducing a hydrophilic functional group on the surface of the low-dimensional transition metal carbide, and regulating its adsorption selectivity for silver, and then dispersing the low-dimensional transition metal carbide in ethanol or water to obtain a low-dimensional transition metal carbide adsorbent;
[0035] S5. Filter and dry the low-dimensional transition metal carbide adsorbent to obtain a low-dimensional transition metal carbide adsorption filter membrane. Generally, under the action of vacuum filtration, a low-dimensional transition metal carbide adsorption filter membrane stacked layer by layer is formed with a microporous filter membrane as the interface, wherein a plurality of modulators such as silica sol and a binder can be added to the low-dimensional transition metal carbide adsorbent to enhance the selective adsorption capacity and film-forming property of the low-dimensional transition metal carbide adsorption filter membrane.
[0036] In some embodiments, the molar ratio of transition metal oxide, aluminum oxide and graphite is 3:1:2-4.
[0037] In some embodiments, the transition metal includes one or more of vanadium, titanium, zirconium, chromium, molybdenum, and tungsten.
[0038] In some embodiments, the molten salt electrolyte selected for molten salt electrolysis in step S2 is a calcium-based Lewis acid electrolyte, and the electrolysis temperature is 850° C. Generally, before use, the molten salt is first dehydrated and dried in an oven at 200° C. for 24 hours, and then vacuumed three times at 300° C. after being placed in an electrolytic furnace to further remove crystal water.
[0039] In some implementations, step S3 specifically includes:
[0040] The transition metal carbide with aluminum intercalation is set to react in a high-temperature chloride molten salt. Since the temperature of the molten salt does not reach the melting point of the transition metal carbide with aluminum intercalation, the transition metal carbide with aluminum intercalation still exists in a solid phase and forms a solid-liquid two-phase interface with the molten salt on the surface; the molten salt at high temperature is an ionic electrolyte, so the intercalated aluminum with higher activity is easy to combine with anions with greater polarity, causing the aluminum intercalation to dissolve into the chloride molten salt, react with the chloride molten salt to generate AlCl3, and obtain a low-dimensional transition metal carbide.
[0041] In some embodiments, the chloride molten salt includes one or more of cobalt chloride, copper chloride, nickel chloride, and zinc chloride.
[0042] In some implementations, step S3 specifically includes:
[0043] By utilizing the aqueous flow field leaching mechanism, a transition metal carbide with aluminum intercalation is placed in a leaching solution to obtain a low-dimensional transition metal carbide, wherein the leaching solution includes hydrofluoric acid, pH-adjusted acidic lithium chloride solution, and KOH solution. In this process, aluminum has relatively active reaction activity and is corroded as a priority attack point at the interface between the two phases. The flow field assistance provided by the continuous magnetic stirring in this process strengthens the diffusion process of the reaction products and reactants, regulates the reaction kinetics, and thus accelerates or promotes the reaction. The aqueous reaction environment can adjust the structure of the low-dimensional transition metal carbide to form a one-dimensional linear or two-dimensional sheet-like nanostructure, and can also introduce rich hydrophilic functional group structures such as hydroxyl and -O into the surface of the low-dimensional transition metal carbide.
[0044] In some embodiments, the surface modifying agent includes KOH solution, LiOH solution, HCl solution, or HF solution.
[0045] In some embodiments, the low-dimensional transition metal carbide adsorption filter membrane for recovering silver electrolysis waste liquid is prepared by the above-mentioned preparation method.
[0046] In some embodiments, the application of low-dimensional transition metal carbide adsorption filter membrane for recovering silver electrolysis waste liquid, the low-dimensional transition metal carbide adsorption filter membrane is used to enrich the silver in the silver electrolysis waste liquid. For example: using the synergistic effect of polybasic mixed acids such as nitric acid and hydrofluoric acid, the pH of the silver electrolysis waste liquid is adjusted to about 4, and then a solution containing 20-30% ethoxyethane is mixed with the silver electrolysis waste liquid at a mass ratio of 1-6% and stirred for 20-180 minutes;
[0047] The treated silver electrolysis waste liquid is filtered and adsorbed by a low-dimensional transition metal carbide adsorption filter membrane for 10 to 180 minutes to obtain a filter membrane enriched with silver particles and silver ions, thereby realizing efficient recycling of the silver electrolysis waste liquid.
[0048] The technical details are further illustrated below in conjunction with embodiments.
[0049] Example 1
[0050] Example 1 discloses a method for preparing a low-dimensional transition metal carbide adsorption filter membrane, which specifically includes:
[0051] According to the set molar ratio of 3:1:2, waste denitrification catalysts containing various rare and refractory metal elements such as vanadium, titanium, molybdenum, and tungsten, alumina, and graphite are mixed, and the samples are pressed and consolidated at 80 MPa to obtain mixed sample blocks;
[0052] The mixed sample block is placed in an argon atmosphere and in a calcium-based Lewis acid electrolyte at 850°C for molten salt electrolysis to obtain a transition metal carbide with an aluminum intercalation layer; wherein the molten salt is first dehydrated and dried in an oven at 200°C for 24 hours before use, and then vacuumed three times at 300°C after being placed in an electrolytic furnace to further remove crystal water; wherein the electrolysis voltage is 3.2V and the electrolysis time is 8 hours;
[0053] The transition metal carbide with aluminum intercalation was repeatedly washed with deionized water and dilute hydrochloric acid until the molten salt was completely removed and dried, and then the transition metal carbide with aluminum intercalation was mixed with Co-based chloride salt in a mixing ratio of 1:5, and then heated to 600 ° C in an argon atmosphere for 8 hours, and the interface was selectively etched to remove the aluminum intercalation to obtain Figure 1 The low-dimensional transition metal carbides shown;
[0054] The low-dimensional transition metal carbide is surface-modified using a 5M LiOH alkaline solution for 12 hours, and then the low-dimensional transition metal carbide is dispersed in ethanol or water to obtain a low-dimensional transition metal carbide adsorbent;
[0055] The low-dimensional transition metal carbide adsorbent is filtered and dried to obtain a low-dimensional transition metal carbide adsorption filter membrane.
[0056] The low-dimensional transition metal carbide adsorption filter membrane prepared in Example 1 is used to enrich silver in silver electrolysis waste liquid, specifically comprising:
[0057] The pH of the silver electrolytic waste liquid is adjusted to about 4 by using the synergistic effect of polybasic mixed acids such as nitric acid and hydrofluoric acid, and then a solution containing 20 to 30% of ethoxyethane is mixed with the silver electrolytic waste liquid at a mass ratio of 1 to 6% and stirred for 20 to 180 minutes;
[0058] The treated silver electrolysis waste liquid is filtered and adsorbed by a low-dimensional transition metal carbide adsorption filter membrane for 10 to 180 minutes to obtain a filter membrane enriched with silver particles and silver ions, and the silver recovery rate is 98%.
[0059] Example 2
[0060] Example 2 discloses a method for preparing a low-dimensional transition metal carbide adsorption filter membrane, which specifically includes:
[0061] Titanium dioxide, aluminum oxide, and graphite were mixed at a set molar ratio of 3:1:3, and pressed and consolidated at 80 MPa to obtain a mixed sample block;
[0062] The mixed sample block is placed in an argon atmosphere and in a calcium-based Lewis acid electrolyte at 900°C for molten salt electrolysis to obtain a transition metal carbide with an aluminum intercalation layer; wherein the molten salt is first dehydrated and dried in an oven at 200°C for 24 hours before use, and then vacuumed three times at 300°C after being placed in an electrolytic furnace to further remove crystal water; wherein the electrolysis voltage is 3.4V and the electrolysis time is 12h;
[0063] The transition metal carbide with aluminum intercalation is repeatedly washed with deionized water and dilute hydrochloric acid until the molten salt is completely removed and dried, and then the transition metal carbide with aluminum intercalation is hydrothermally reacted with a 10M LiOH aqueous solution at 200° C. for 18 hours to remove the aluminum intercalation and obtain a low-dimensional transition metal carbide;
[0064] Dispersing low-dimensional transition metal carbide in ethanol or water to obtain a low-dimensional transition metal carbide adsorbent;
[0065] The low-dimensional transition metal carbide adsorbent is filtered and dried to obtain a low-dimensional transition metal carbide adsorption filter membrane.
[0066] The low-dimensional transition metal carbide adsorption filter membrane prepared in Example 2 is used to enrich silver in the silver electrolysis waste liquid, specifically comprising:
[0067] The pH of the silver electrolytic waste liquid is adjusted to about 4 by using the synergistic effect of polybasic mixed acids such as nitric acid and hydrofluoric acid, and then a solution containing 20 to 30% of ethoxyethane is mixed with the silver electrolytic waste liquid at a mass ratio of 1 to 6% and stirred for 20 to 180 minutes;
[0068] The treated silver electrolysis waste liquid is filtered and adsorbed by a low-dimensional transition metal carbide adsorption filter membrane for 10 to 180 minutes to obtain a filter membrane enriched with silver particles and silver ions, and the silver recovery rate is 99%.
[0069] Example 3
[0070] Example 3 discloses a method for preparing a low-dimensional transition metal carbide adsorption filter membrane, which specifically includes:
[0071] According to the set molar ratio of 3:1:3, high titanium slag containing oxides such as vanadium and titanium, alumina and graphite are mixed, and the sample is pressed and consolidated at 80 MPa to obtain a mixed sample block;
[0072] The mixed sample block is placed in an argon atmosphere and a calcium-based Lewis acid electrolyte at 850°C for molten salt electrolysis to obtain a transition metal carbide with an aluminum intercalation layer; wherein the molten salt is first dehydrated and dried in an oven at 200°C for 24 hours before use, and then vacuumed three times at 300°C after being placed in an electrolytic furnace to further remove crystal water; wherein the electrolysis voltage is 3.3V and the electrolysis time is 16 hours;
[0073] The transition metal carbide with aluminum intercalation is repeatedly washed with deionized water and dilute hydrochloric acid until the molten salt is completely removed and dried, and then the transition metal carbide with aluminum intercalation is hydrothermally reacted with hydrofluoric acid at 40° C. for 48 hours to remove the aluminum intercalation to obtain a low-dimensional transition metal carbide;
[0074] Dispersing low-dimensional transition metal carbide in ethanol or water to obtain a low-dimensional transition metal carbide adsorbent;
[0075] The low-dimensional transition metal carbide adsorbent is filtered and dried to obtain a low-dimensional transition metal carbide adsorption filter membrane. The microscopic morphology of the low-dimensional transition metal carbide adsorption filter membrane is as follows: Figure 2 shown.
[0076] The low-dimensional transition metal carbide adsorption filter membrane prepared in Example 3 is used to enrich the silver in the silver electrolysis waste liquid, specifically comprising:
[0077] The pH of the silver electrolytic waste liquid is adjusted to about 4 by using the synergistic effect of polybasic mixed acids such as nitric acid and hydrofluoric acid, and then a solution containing 20 to 30% of ethoxyethane is mixed with the silver electrolytic waste liquid at a mass ratio of 1 to 6% and stirred for 20 to 180 minutes;
[0078] The treated silver electrolysis waste liquid is filtered and adsorbed by a low-dimensional transition metal carbide adsorption filter membrane for 10 to 180 minutes to obtain a filter membrane enriched with silver particles and silver ions, and the silver recovery rate is 99.5%.
[0079] The low-dimensional transition metal carbide adsorption filter membrane for recovering silver electrolysis waste liquid disclosed in the embodiment of the present invention has stable chemical properties and a large specific surface area, has excellent adsorption affinity and reducibility to silver ions or silver particles, can be used as a good filtration medium, and can realize simple and convenient recovery of metallic silver from silver electrolysis waste liquid.
[0080] The technical solutions disclosed in the present invention and the technical details disclosed in the embodiments are merely illustrative of the inventive concept of the present invention and do not constitute a limitation on the technical solutions of the present invention. Any conventional changes, substitutions or combinations of the technical details disclosed in the embodiments of the present invention have the same inventive concept as the present invention and are within the protection scope of the claims of the present invention.
Claims
1. A method for preparing a low-dimensional transition metal carbide adsorption filter membrane for recovering silver electrolysis waste liquid, characterized in that: Includes steps: S1. Mix transition metal oxides, aluminum oxide and graphite according to a set ratio, press and consolidate the sample to obtain a mixed sample block; S2, subjecting the mixed sample block to molten salt electrolysis to obtain transition metal carbides with aluminum intercalation; S3, performing interface selective etching on the transition metal carbide with aluminum intercalation to remove the aluminum intercalation to obtain a low-dimensional transition metal carbide; S4, using a surface modifier to perform surface modification on the low-dimensional transition metal carbide, and then dispersing the low-dimensional transition metal carbide in ethanol or water to obtain a low-dimensional transition metal carbide adsorbent; S5. Filter and dry the low-dimensional transition metal carbide adsorbent to obtain a low-dimensional transition metal carbide adsorption filter membrane.
2. The method for preparing a low-dimensional transition metal carbide adsorption filter membrane for recovering silver electrolysis waste liquid according to claim 1, characterized in that: The molar ratio of the transition metal oxide, the aluminum oxide and the graphite is 3:1:2-4.
3. The method for preparing a low-dimensional transition metal carbide adsorption filter membrane for recovering silver electrolysis waste liquid according to claim 1, characterized in that: The transition metal includes one or more of vanadium, titanium, zirconium, chromium, molybdenum and tungsten.
4. The method for preparing a low-dimensional transition metal carbide adsorption filter membrane for recovering silver electrolysis waste liquid according to claim 1, characterized in that: The molten salt electrolyte selected for molten salt electrolysis in step S2 is a calcium-based Lewis acid electrolyte, and the electrolysis temperature is 850°C.
5. The method for preparing a low-dimensional transition metal carbide adsorption filter membrane for recovering silver electrolysis waste liquid according to claim 1, characterized in that: Step S3 specifically includes: The transition metal carbide with aluminum intercalation is set to react in a high-temperature chloride molten salt, the aluminum intercalation is dissolved in the chloride molten salt, and reacts with the chloride molten salt to generate AlCl3, thereby obtaining a low-dimensional transition metal carbide.
6. The method for preparing a low-dimensional transition metal carbide adsorption filter membrane for recovering silver electrolysis waste liquid according to claim 5, characterized in that: The chloride molten salt includes one or more of cobalt chloride, copper chloride, nickel chloride and zinc chloride.
7. The method for preparing a low-dimensional transition metal carbide adsorption filter membrane for recovering silver electrolysis waste liquid according to claim 1, characterized in that: Step S3 specifically includes: The method utilizes the water flow field leaching mechanism to place the transition metal carbide with aluminum intercalation in a leaching solution to obtain a low-dimensional transition metal carbide; wherein the leaching solution includes hydrofluoric acid, pH-adjusted acidic lithium chloride solution or KOH solution.
8. The method for preparing a low-dimensional transition metal carbide adsorption filter membrane for recovering silver electrolysis waste liquid according to claim 1, characterized in that: The surface modifier includes KOH solution, LiOH solution, HCl solution or HF solution.
9. A low-dimensional transition metal carbide adsorption filter membrane for recovering silver electrolysis waste liquid, characterized in that: It is prepared by the preparation method according to any one of claims 1 to 8.
10. The use of the low-dimensional transition metal carbide adsorption filter membrane for recovering silver electrolysis waste liquid as claimed in claim 9, characterized in that: The low-dimensional transition metal carbide adsorption filter membrane is used for enriching silver in silver electrolysis waste liquid.
Citation Information
Patent Citations
Preparation method of two-dimensional titanium carbide adsorbing material
CN106268610A
Surface modification method of MXene material
CN114349006A
Method for preparing titanium carbide MXene through microwave fused salt etching
CN114671436A
Transition metal carbide-based composite material as well as preparation method and application thereof
CN116905004A
Method for recovering metallic silver from printing film and fixing solution
CN116987899A