Polylactic acid fiber filtering membrane as well as preparation method and application thereof
By introducing barium titanate carrier into the polylactate fiber filter membrane and optimizing the fiber structure, the problem of difficulty in taking into account the fracture strength, surface potential, antibacterial efficiency and filtration efficiency of fiber filter membranes in the prior art is solved, and efficient particulate matter is achieved Filtration and long-term stable antibacterial properties.
Patent Information
- Application Number
- CN202411478893.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-10-22
- Publication Date
- 2024-12-06
AI Technical Summary
The existing polylactic fiber filtration membranes are difficult to take into account the fracture strength, surface potential, antibacterial efficiency and filtration efficiency.
By introducing a barium titanate carrier into the polylactate fiber filter membrane and defining the composition and diameter ratio of the first fiber and the second fiber, a uniformly distributed fiber structure is formed, the porosity and distribution density of the fiber are improved, and the mechanics of the fiber are enhanced, and the mechanical of the fiber is enhanced. Performance and filtering performance.
A polylactic fiber filter membrane with high fracture strength, high surface potential, high antibacterial efficiency and high filtration efficiency can effectively remove PM0.3 and PM2.5 particles, and maintain good filtration performance and antibacterial effect for a long time. .
Smart Images

Figure CN119075712A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of fiber filter membranes, and in particular to a polylactic acid fiber filter membrane and a preparation method and application thereof. Background Art
[0002] Particulate matter (PM) in the air has a huge negative impact on human health and global climate. PM can be divided into coarse components (PM with a diameter of <10 μm) according to its diameter. 10 ), fine components (PM with a diameter <2.5 μm 2.5 ) and ultrafine components (UFPS with a diameter of <0.1μm), these particles can penetrate the respiratory system, cause health hazards, and have an impact on global climate and air quality. Due to their small mass, they are difficult to separate from other substances in the gas, and a filter medium is urgently needed to remove these particles.
[0003] Polylactic acid has good application prospects in the field of air filtration due to its good biodegradability. At present, polylactic acid is mostly used in combination with functional materials to obtain degradable filtration membranes with excellent performance. However, the doping of functional materials will affect the roughness, porosity and chemical properties of the filter membrane surface, making it difficult to take into account the breaking strength, surface potential, antibacterial efficiency and filtration efficiency, which is not conducive to the practical application of the filter membrane.
[0004] Therefore, how to provide a polylactic acid fiber filter membrane having high breaking strength, high surface potential, high antibacterial efficiency and high filtration efficiency is a technical problem to be solved urgently in this field. Summary of the invention
[0005] The main purpose of the present invention is to provide a polylactic acid fiber filter membrane and a preparation method and application thereof, so as to solve the problem in the prior art that it is difficult for the filter membrane to take into account the breaking strength, surface potential, antibacterial efficiency and filtration efficiency.
[0006] In order to achieve the above object, according to one aspect of the present invention, a polylactic acid fiber filter membrane is provided, the polylactic acid fiber filter membrane comprising a first fiber, a second fiber and a barium titanate support, the first fiber and the second fiber are randomly stacked, and the barium titanate support is supported on the surfaces of the first fiber and the second fiber;
[0007] The diameter ratio of the first fiber to the second fiber is 1:(10-500); the first fiber and the second fiber both include polylactic acid; the mass ratio of the first fiber, the second fiber and the barium titanate support is 1:(1.5-25):(15-150).
[0008] Furthermore, the diameter of the first fiber is 30-800 nm, and the average pore size is 1-25 nm; and / or, the diameter of the second fiber is 1-10 μm, and the average pore size is 2-50 nm; and / or, the barium titanate support is granular, and the average diameter of the barium titanate support is 10-80 nm.
[0009] Further, the first fiber and the second fiber both include left-handed polylactic acid and right-handed polylactic acid;
[0010] Preferably, the first fiber comprises a first left-handed polylactic acid and a first right-handed polylactic acid, and the second fiber comprises a second left-handed polylactic acid and a second right-handed polylactic acid;
[0011] wherein the molar ratio of the second L-polylactic acid to the second D-polylactic acid is greater than the molar ratio of the first L-polylactic acid to the first D-polylactic acid;
[0012] Preferably, the molar ratio of the first L-polylactic acid to the first D-polylactic acid is (5-10):1;
[0013] Preferably, the molar ratio of the second L-polylactic acid to the second D-polylactic acid is (10-15):1.
[0014] Furthermore, the weight average molecular weight of the first L-polylactic acid is 10KDa to 150KDa; and / or, the weight average molecular weight of the first D-polylactic acid is 200KDa to 350KDa; and / or, the weight average molecular weight of the second L-polylactic acid is 50KDa to 200KDa; and / or, the weight average molecular weight of the second D-polylactic acid is 300KDa to 450KDa.
[0015] Further, the thickness of the polylactic acid fiber filter membrane is 20 to 600 μm; and / or, the breaking strength of the polylactic acid fiber filter membrane is 17 to 36 MPa, preferably 25.6 to 36 MPa; and / or, at a temperature of 25°C and a humidity of 45%, the surface potential of the polylactic acid fiber filter membrane is 12 to 20 kV; and / or, the polylactic acid fiber filter membrane has a good resistance to PM 0.3 and PM 2.5 The filtration efficiency is ≥98%; and / or, at a gas flow rate of 10 to 85 L / min, the air resistance of the polylactic acid fiber filter membrane is ≤80 Pa; and / or, under light with a wavelength of 600 nm, the antibacterial rate of the polylactic acid fiber filter membrane against Escherichia coli and Staphylococcus aureus is ≥86%.
[0016] According to a second aspect of the present invention, there is provided a method for preparing the polylactic acid fiber filter membrane of the first aspect, comprising the following steps:
[0017] The first spinning solution, the second spinning solution and the barium titanate dispersion are subjected to multi-needle electrospinning to obtain a polylactic acid fiber filter membrane;
[0018] Wherein, the first spinning solution and the second spinning solution both contain polylactic acid.
[0019] Furthermore, the preparation method of the first spinning solution includes:
[0020] Dissolving the first polylactic acid in a first solvent to obtain a first spinning solution;
[0021] Furthermore, the preparation method of the second spinning solution comprises:
[0022] dissolving the second polylactic acid in a second solvent to obtain a second spinning solution;
[0023] Preferably, the first polylactic acid and the second polylactic acid both include left-handed polylactic acid and right-handed polylactic acid;
[0024] Preferably, the first polylactic acid includes a first left-handed polylactic acid and a first right-handed polylactic acid, and the second polylactic acid includes a second left-handed polylactic acid and a second right-handed polylactic acid; wherein the molar ratio of the second left-handed polylactic acid to the second right-handed polylactic acid is greater than the molar ratio of the first left-handed polylactic acid to the first right-handed polylactic acid;
[0025] Preferably, the molar ratio of the first L-polylactic acid to the first D-polylactic acid is (5-10):1;
[0026] Preferably, the sum of the mass fractions of the first L-polylactic acid and the first D-polylactic acid in the first spinning solution is 0.4% to 15%;
[0027] Preferably, the first solvent includes a first good solvent and a first non-good solvent, and the volume ratio of the first good solvent to the first non-good solvent is 1:(2-5);
[0028] Preferably, the molar ratio of the second L-polylactic acid to the second D-polylactic acid is (10-15):1;
[0029] Preferably, the sum of the mass fractions of the second right-handed polylactic acid and the second left-handed polylactic acid in the second spinning solution is 15% to 25%;
[0030] Preferably, the second solvent includes a second good solvent and a second non-good solvent, and the volume ratio of the second good solvent to the second non-good solvent is 1:(5-10);
[0031] Preferably, the first good solvent and the second good solvent each independently include at least one of dichloromethane, chloroform, dimethylformamide, N-methylpyrrolidone, tetrahydrofuran, and ethyl acetate, and the first non-good solvent and the second non-good solvent each independently include at least one of methanol, ethanol, isopropanol, glycerol, butanol, ethylene glycol, and propylene glycol;
[0032] More preferably, the first good solvent includes at least one of dichloromethane, chloroform, and dimethylformamide, the second good solvent includes at least one of dimethylformamide, N-methylpyrrolidone, ethyl acetate, and tetrahydrofuran, the first non-good solvent includes at least one of ethanol, methanol, isopropanol, and n-butanol, and the second non-good solvent includes at least one of butanol, glycerol, propylene glycol, and ethylene glycol.
[0033] Furthermore, the preparation method of the barium titanate dispersion includes:
[0034] mixing barium titanate, a dispersant and a third solvent to obtain a barium titanate dispersion;
[0035] Preferably, the preparation method of barium titanate comprises:
[0036] Mixing titanium dioxide, a barium compound and a fourth solvent, and subjecting the mixture to microwave treatment to obtain barium titanate;
[0037] Preferably, the dispersant includes at least one of polyvinyl pyrrolidone, dodecyltrimethylammonium bromide, sodium dodecyl sulfate, and sodium dodecylbenzene sulfonate;
[0038] Preferably, the third solvent comprises at least one of dimethylformamide, dichloromethane, chloroform, and N-methylpyrrolidone;
[0039] Preferably, the mass ratio of barium titanate to dispersant is 1:(10-100);
[0040] Preferably, the mass fraction of barium titanate in the barium titanate dispersion is 0.25% to 1%;
[0041] Preferably, the mass ratio of titanium dioxide to barium compound is 1:(1-10);
[0042] Preferably, the microwave treatment has a power of 500 to 1500 W, a temperature of 100 to 200° C., and a time of 20 to 120 min;
[0043] Preferably, the barium compound includes at least one of barium hydroxide, barium chloride dihydrate, barium acetate, barium nitrate, and barium peroxide;
[0044] Preferably, the fourth solvent comprises at least one of diethylene glycol, hexafluoroisopropanol, methanol, ethanol, isopropanol, glycerol, and water;
[0045] More preferably, the fourth solvent includes at least one of diethylene glycol, methanol, ethanol and isopropanol.
[0046] Further, in the multi-needle electrospinning process, the metal nozzles loaded with the first spinning solution, the second spinning solution and the barium titanate dispersion are respectively the first nozzle, the second nozzle and the third nozzle;
[0047] Preferably, the inner diameter of the first nozzle is 10-20 μm, the inner diameter of the second nozzle is 60-80 μm, and the inner diameter of the third nozzle is 30-60 μm;
[0048] Preferably, the voltages of the first nozzle, the second nozzle and the third nozzle are all 10 to 30 kV;
[0049] Preferably, the consumption rate of the first spinning solution is 0.8 to 2 mL / h, the consumption rate of the second spinning solution is 0.2 to 1.2 mL / h, and the consumption rate of the barium titanate dispersion is 0.2 to 1.5 mL / h;
[0050] Preferably, the receiving distances of the first nozzle, the second nozzle and the third nozzle are all 10-25 cm.
[0051] According to a third aspect of the present invention, there is provided an air filter comprising the polylactic acid fiber filter membrane provided by the first aspect or the polylactic acid fiber filter membrane prepared by the preparation method provided by the second aspect.
[0052] By applying the technical solution of the present invention, the composition and diameter ratio of the first fiber and the second fiber are limited, so that the fibers of the polylactic acid fiber filter membrane are evenly distributed, and the porosity and fiber distribution density of the polylactic acid fiber filter membrane are improved, thereby improving the filtration performance and breaking strength of the fiber filter membrane. At the same time, by using the barium titanate support body tightly loaded on the fiber surface and limiting the mass ratio of the first fiber, the second fiber and the barium titanate support body, the surface potential and antibacterial performance of the fiber filter membrane can be improved while ensuring the breaking strength and filtration performance, thereby obtaining a polylactic acid fiber filter membrane with high breaking strength, high surface potential, high antibacterial efficiency and high filtration efficiency. BRIEF DESCRIPTION OF THE DRAWINGS
[0053] Figure 1 This is a SEM image of the polylactic acid fiber filter membrane of Example 1 of the present invention;
[0054] Figure 2 This is the SEM image of the polylactic acid fiber filter membrane of Comparative Example 2 of the present invention. DETAILED DESCRIPTION
[0055] In order to make the purpose, technical scheme and advantages of the embodiments of the present invention clearer, the technical scheme in the embodiments of the present invention will be described clearly and completely below. If the specific conditions are not specified in the embodiments, they are carried out according to conventional conditions or conditions recommended by the manufacturer. If the manufacturer of the reagents or instruments used is not specified, they are all conventional products that can be purchased commercially.
[0056] As described in the background of the present invention, it is difficult for the polylactic acid fiber filter membrane in the prior art to take into account the problems of breaking strength, surface potential, antibacterial efficiency and filtration efficiency. In order to solve the above problems, the first aspect of the present invention provides a polylactic acid fiber filter membrane, which includes a first fiber, a second fiber and a barium titanate support, the first fiber and the second fiber are randomly stacked, and the barium titanate support is supported on the surface of the first fiber and the second fiber; wherein the diameter ratio of the first fiber to the second fiber is 1: (10-500); the first fiber and the second fiber both include polylactic acid; the mass ratio of the first fiber, the second fiber and the barium titanate support is 1: (1.5-25): (15-150).
[0057] The polylactic acid fiber filter membrane of the present invention comprises a matrix and a support. The matrix is a film formed by randomly stacking first fibers and second fibers, which can be realized by an electrostatic spinning process. Specifically, the first fibers and the second fibers are continuous straight filaments, and the orientation is randomly distributed, so as to form a film with a mesh structure. The component of the support is barium titanate, which is independently loaded on the surface of the first fibers and the second fibers.
[0058] Among them, the first fiber and the second fiber have the same composition, both of which include polylactic acid. The polylactic acid molecular chains are stacked to form a polylactic acid stereocomplex, which has good interfacial compatibility, high crystallinity and well-arranged microstructure, thereby improving the mechanical properties and filtration performance of the polylactic acid fiber filter membrane. The diameter ratio of the first fiber to the second fiber is 1: (10-500), for example, 1: 10, 1: 20, 1: 30, 1: 40, 1: 50, 1: 60, 1: 100, 1: 200, 1: 300, 1: 400, 1: 500 or the range of any two of them. By limiting the first fiber and the second fiber to have the same composition and the diameter ratio within the above range, the fibers in the polylactic acid fiber filter membrane can be evenly distributed, while improving the porosity and fiber distribution density of the polylactic acid fiber filter membrane, thereby improving the filtration performance of the fiber filter membrane for particulate matter and its own breaking strength.
[0059] The introduction of barium titanate (BaTiO3) carrier can enhance the piezoelectric properties of polylactic acid fiber filter membrane, improve the electrostatic adsorption force, and increase the surface potential, so that the polylactic acid fiber filter membrane has good filtration performance and antibacterial properties.
[0060] According to the research of the present invention, by limiting the composition and diameter ratio of the first fiber and the second fiber, the fibers of the polylactic acid fiber filter membrane are evenly distributed, and the porosity and fiber distribution density of the polylactic acid fiber filter membrane are improved, thereby improving the filtration performance and breaking strength of the fiber filter membrane. At the same time, by using the barium titanate support body tightly loaded on the fiber surface and limiting the mass ratio of the first fiber, the second fiber and the barium titanate support body, the surface potential and antibacterial performance of the fiber filter membrane can be improved while ensuring the breaking strength and filtration performance, thereby obtaining a polylactic acid fiber filter membrane with high breaking strength, high surface potential, high antibacterial efficiency and high filtration efficiency.
[0061] The first fiber and the second fiber are both continuous straight filaments. In some embodiments, the diameter of the first fiber is 30 to 800 nm, for example, 30 nm, 100 nm, 200 nm, 300 nm, 400 nm, 500 nm, 600 nm, 700 nm, 800 nm, or a range consisting of any two thereof, and the average pore size is 1 to 25 nm, for example, 1 nm, 2 nm, 5 nm, 10 nm, 20 nm, 25 nm, or a range consisting of any two thereof; and / or, the diameter of the second fiber is 1 to 10 μm, for example, 1 μm, 2 μm, 3 μm, 4 μm, 5 μm, 6 μm, 7 μm, 8 μm, 9 μm, or a range consisting of any two thereof, and the average pore size is 2 to 50 nm, for example, 2 nm, 5 nm, 10 nm, 20 nm, 30 nm, 40 nm, 50 nm, or a range consisting of any two thereof. By limiting the diameter and average pore size of the first fiber and the second fiber, the air permeability and filtration performance of the polylactic acid fiber filter membrane can be further improved.
[0062] Specifically, the diameter of the first fiber refers to the diameter of the cross section of a single first fiber, and the diameter of the second fiber refers to the diameter of the cross section of a single second fiber. Specifically, the surface of the polylactic acid fiber filter membrane can be observed using a scanning electron microscope, and then the diameters of the first fiber and the second fiber can be measured, or the cross section of the polylactic acid fiber filter membrane can be observed using a transmission electron microscope, and then the diameters of the first fiber and the second fiber can be measured.
[0063] The fiber contains voids, i.e., the pores of the fiber, which may be continuous or discontinuous. The size and distribution of the pores have an important influence on many properties of the fiber, such as air permeability, filtering performance, etc. The average pore size of the fiber refers to the average value of the size of the pores in the fiber. By limiting the average pore size of the first fiber and the second fiber, the air permeability and filtering performance of the polylactic acid fiber filter membrane can be improved. In the specific implementation process of the present invention, the pore structure of the first fiber and the second fiber can be observed using scanning electron microscopy, transmission electron microscopy, or X-ray tomography. By measuring the size of the pores and calculating their average value, the average pore size of the first fiber and the second fiber can be obtained.
[0064] The material of the barium titanate support is barium titanate, which is loaded on the surface of the first fiber and the second fiber in a granular form. Granular barium titanate can further enhance the mechanical properties of the polylactic acid fiber filter membrane, such as breaking strength, which makes the polylactic acid fiber filter membrane have better performance under high load and harsh environmental conditions. Granular barium titanate can improve the adsorption performance of the polylactic acid fiber filter membrane, so that it has better applications in the fields of filtration, purification and separation. In some embodiments, the barium titanate support is granular, and the average diameter of the barium titanate support is 10 to 80 nm, such as 10 nm, 20 nm, 30 nm, 40 nm, 50 nm, 60 nm, 70 nm, 80 nm or any two of them. The average diameter of the barium titanate support can also be understood as the D50 particle size of the barium titanate support. By limiting the diameter of the barium titanate support to the above range, the surface potential and antibacterial performance of the polylactic acid fiber filter membrane can be further improved.
[0065] The first fiber and the second fiber are made of the same material, both containing left-handed polylactic acid (PLLA) and right-handed polylactic acid (PDLA). In some embodiments, the first fiber includes a first left-handed polylactic acid and a first right-handed polylactic acid, and the second fiber includes a second left-handed polylactic acid and a second right-handed polylactic acid; wherein the molar ratio of the second left-handed polylactic acid to the second right-handed polylactic acid is greater than the molar ratio of the first left-handed polylactic acid to the first right-handed polylactic acid. By limiting the molar ratio of the components in the first fiber and the second fiber, it is not only helpful to achieve the diameters of the first fiber and the second fiber of 30 to 800 nm and 1 to 10 μm, respectively, but also to take into account the improvement of mechanical properties and filtration performance.
[0066] By adjusting the ratio of left-handed polylactic acid and right-handed polylactic acid, the performance of the polylactic acid stereocomplex can be regulated to meet the needs of different application fields. As the content of right-handed polylactic acid increases, the ability to form a polylactic acid stereocomplex is enhanced, but when it increases to a certain extent, it may affect the improvement of other properties. In some embodiments, the molar ratio of the first left-handed polylactic acid to the first right-handed polylactic acid is (5-10):1, for example, 5:1, 6:1, 7:1, 8:1, 9:1, 10:1 or a range consisting of any two thereof; and / or, the molar ratio of the second left-handed polylactic acid to the second right-handed polylactic acid is (10-15):1, for example, 10:1, 11:1, 12:1, 13:1, 14:1, 15:1 or a range consisting of any two thereof.
[0067] In some embodiments, the weight average molecular weight of the first L-polylactic acid is 10KDa to 150KDa; and / or, the weight average molecular weight of the first D-polylactic acid is 200KDa to 350KDa; and / or, the weight average molecular weight of the second L-polylactic acid is 50KDa to 200KDa; and / or, the weight average molecular weight of the second D-polylactic acid is 300KDa to 450KDa.
[0068] The present invention does not limit the specific parameters of the polylactic acid fiber filter membrane, as long as it meets the above requirements. In some embodiments, the thickness of the polylactic acid fiber filter membrane is 20 to 600 μm. The size of the polylactic acid fiber filter membrane can be adjusted according to actual needs to meet the application in different fields. In some embodiments, the breaking strength of the polylactic acid fiber filter membrane is 17 to 36 MPa. It can be understood that the polylactic acid fiber filter membrane has high mechanical strength. In some embodiments, at a temperature of 25°C and a humidity of 45%, the surface potential of the polylactic acid fiber filter membrane is 12 to 20 kV. By limiting the surface potential of the polylactic acid fiber filter membrane, it can better adsorb the substances to be filtered and improve the filtration efficiency. In some embodiments, the polylactic acid fiber filter membrane has good resistance to PM 0.3 and PM 2.5 The filtration efficiency of the polylactic acid fiber filtration membrane of the present invention is ≥98%. 0.3 and PM 2.5 The particles have a high filtration efficiency. In some embodiments, the air resistance of the polylactic acid fiber filter membrane is ≤80Pa at a gas flow rate of 10 to 85L / min. By limiting the air resistance of the polylactic acid fiber filter membrane, it has a lower air resistance at a certain gas flow rate, can better achieve air exchange at a high filtration rate, and has higher air permeability. In some embodiments, under light with a wavelength of 600nm, the antibacterial rate of the polylactic acid fiber filter membrane against Escherichia coli and Staphylococcus aureus is ≥86%. It can be understood that the polylactic acid fiber filter membrane has excellent antibacterial properties and can achieve long-term service.
[0069] In some preferred embodiments, the polylactic acid fiber filter membrane has a breaking strength of 17.5 to 36 MPa, more preferably 25.6 to 36 MPa, a surface potential of 12.0 to 18.3 kV, and a PM 0.3 The filtration efficiency is 98.1-99.8%, PM 2.5 The filtration efficiency is 98.7-99.9%. Under the light with a wavelength of 600nm, the antibacterial rate to Escherichia coli is 88.8-99.8%, and the antibacterial rate to Staphylococcus aureus is 86.4-98.9%.
[0070] The second aspect of the present invention provides a method for preparing a polylactic acid fiber filter membrane, comprising the following steps:
[0071] The first spinning solution, the second spinning solution and the barium titanate dispersion are subjected to multi-needle electrospinning to obtain a polylactic acid fiber filter membrane;
[0072] Wherein, the first spinning solution and the second spinning solution both contain polylactic acid.
[0073] In the multi-needle electrospinning process, the first spinning solution and the second spinning solution are respectively formed into the first fiber and the second fiber, and the first fiber and the second fiber are randomly stacked. At the same time, barium titanate can be loaded on the surface of the first fiber and the second fiber.
[0074] Specifically, multi-needle electrospinning can be implemented using a multi-needle electrospinning device, which is usually composed of multiple nozzles, and each nozzle can be independently electrospun. In the multi-needle electrospinning process, the multi-needle electrospinning device is started, so that the first spinning solution, the second spinning solution, and the barium titanate dispersion are ejected from the nozzle under the action of a high-voltage electrostatic field to form a charged jet stream. The jet stream is subjected to the effects of electric field force, surface tension, and air resistance during flight. The first spinning solution and the second spinning solution are gradually stretched and refined, and the solvent evaporates, and finally deposited on the receiving device to form the first fiber and the second fiber. At the same time, the barium titanate dispersion is attached to the surface of the first fiber and the second fiber in a spray state, and the solvent evaporates and is loaded on the surface of the first fiber and the second fiber to form a barium titanate support. In addition, in the multi-needle electrospinning process, it is necessary to collect and organize the first fiber and the second fiber. For example, the deposition density and arrangement of the first fiber and the second fiber can be controlled by adjusting the movement speed and direction of the receiving device, as well as the distance between the nozzle and the receiving device, so that the first fiber and the second fiber are randomly stacked to form a mesh fiber membrane.
[0075] The polylactic acid is mixed with a solvent, and the polylactic acid is fully dissolved by stirring or ultrasound to form a uniform spinning solution. In some embodiments, the method for preparing the first spinning solution includes: dissolving the first polylactic acid in a first solvent to obtain a first spinning solution; the method for preparing the second spinning solution includes: dissolving the second polylactic acid in a second solvent to obtain a second spinning solution; wherein the first polylactic acid and the second polylactic acid both include left-handed polylactic acid and right-handed polylactic acid. Specifically, the first polylactic acid includes a first left-handed polylactic acid and a first right-handed polylactic acid, and the second polylactic acid includes a second left-handed polylactic acid and a second right-handed polylactic acid, wherein the molar ratio of the second left-handed polylactic acid to the second right-handed polylactic acid is greater than the molar ratio of the first left-handed polylactic acid to the first right-handed polylactic acid.
[0076] Parameters such as the concentration, viscosity and surface tension of the spinning solution can be adjusted according to actual needs. In some preferred embodiments, the molar ratio of the first left-handed polylactic acid to the first right-handed polylactic acid is (5-10):1, for example, 5:1, 6:1, 7:1, 8:1, 9:1, 10:1 or a range consisting of any two thereof; the molar ratio of the second left-handed polylactic acid to the second right-handed polylactic acid is (10-15):1, for example, 10:1, 11:1, 12:1, 13:1, 14:1, 15:1 or a range consisting of any two thereof; in some preferred embodiments, the sum of the mass fractions of the first left-handed polylactic acid and the first right-handed polylactic acid in the first spinning solution is 0.4%-15%, for example, 0.4%, 1%, 5%, 10%, 15% or a range consisting of any two thereof; the sum of the mass fractions of the second right-handed polylactic acid and the second left-handed polylactic acid in the second spinning solution is 15%-25%, for example, 15%, 20%, 25% or a range consisting of any two thereof.
[0077] The present invention uses left-handed polylactic acid and right-handed polylactic acid as matrix polymers, and dissolves them in a mixed solvent composed of a good solvent and a non-good solvent to prepare a first spinning solution and a second spinning solution with a concentration gradient, which is helpful to achieve the preparation of the above-mentioned polylactic acid fiber filter membrane with excellent performance. In some preferred embodiments, the first solvent includes a first good solvent and a first non-good solvent, and the volume ratio of the first good solvent to the first non-good solvent is 1: (2-5), such as 1: 2, 1: 3, 1: 4, 1: 5 or a range composed of any two thereof; the second solvent includes a second good solvent and a second non-good solvent, and the volume ratio of the second good solvent to the second non-good solvent is 1: (5-10), such as 1: 5, 1: 6, 1: 8, 1: 10 or a range composed of any two thereof. By constructing a "non-good solvent-good solvent-polymer" ternary system, the principle of non-good solvent-induced phase separation can be used to generate three-dimensional interconnected pores on the fiber surface in situ, further reducing air resistance. Preferably, the first good solvent and the second good solvent independently include at least one of dichloromethane, chloroform, dimethylformamide, N-methylpyrrolidone, tetrahydrofuran, and ethyl acetate, and the first non-good solvent and the second non-good solvent independently include at least one of methanol, ethanol, isopropanol, glycerol, butanol, ethylene glycol, and propylene glycol. More preferably, the first good solvent includes at least one of dichloromethane, chloroform, and dimethylformamide, the second good solvent includes at least one of dimethylformamide, N-methylpyrrolidone, ethyl acetate, and tetrahydrofuran, the first non-good solvent includes at least one of ethanol, methanol, isopropanol, and n-butanol, and the second non-good solvent includes at least one of butanol, glycerol, propylene glycol, and ethylene glycol. By further limiting the specific type of solvent, the optimization of the performance of the polylactic acid fiber filter membrane can be achieved.
[0078] In some embodiments, a method for preparing a barium titanate dispersion includes: mixing barium titanate, a dispersant, and a third solvent to obtain a barium titanate dispersion. The dispersant helps prevent the aggregation of barium titanate particles and improves the stability of the barium titanate dispersion. The dispersant includes at least one of polyvinyl pyrrolidone, dodecyltrimethylammonium bromide, sodium dodecyl sulfate, and sodium dodecylbenzene sulfonate; and the third solvent includes at least one of dimethylformamide, dichloromethane, chloroform, and N-methylpyrrolidone.
[0079] By adjusting the concentration of the barium titanate dispersion, uneven spraying can be prevented from affecting the performance of the polylactic acid fiber filter membrane. In some embodiments, the mass ratio of barium titanate to dispersant is 1:(10-100), such as 1:10, 1:20, 1:50, 1:80, 1:100 or a range consisting of any two thereof; the mass fraction of barium titanate in the barium titanate dispersion is 0.25%-1%, such as 0.25%, 0.5%, 0.75%, 1% or a range consisting of any two thereof.
[0080] Barium titanate can be obtained by commercial purchase or conventional preparation methods. In some embodiments, the preparation method of barium titanate includes: mixing titanium dioxide, a barium compound and a fourth solvent, and subjecting them to microwave treatment to obtain barium titanate. Among them, the preparation of barium titanate can be achieved by microwave assistance to improve the yield. In some preferred embodiments, the power of microwave treatment is 500-1500W, the temperature is 100-200°C, and the time is 20-120min. In addition, the yield of barium titanate can be improved by adjusting the amount of raw materials added. In some embodiments, the mass ratio of titanium dioxide to barium compounds is 1: (1-10), for example, 1: 1, 1: 2, 1: 5, 1: 8, 1: 10 or a range of any two of them.
[0081] The present invention does not limit the specific type of raw materials, and can be adjusted and obtained according to actual needs. In some embodiments, the barium compound includes at least one of barium hydroxide, barium chloride dihydrate, barium acetate, barium nitrate, and barium peroxide; the fourth solvent includes at least one of diethylene glycol, hexafluoroisopropanol, methanol, ethanol, isopropanol, glycerol, and water; in some more preferred embodiments, the fourth solvent includes at least one of diethylene glycol, methanol, ethanol, and isopropanol.
[0082] In the multi-needle electrospinning process, the first spinning solution, the second spinning solution, and the barium titanate dispersion need to be loaded into the container of the nozzle respectively, and ensure that the aperture of the nozzle meets the required fiber size. In some embodiments, in the multi-needle electrospinning process, the metal nozzles loaded with the first spinning solution, the second spinning solution, and the barium titanate dispersion are the first nozzle, the second nozzle, and the third nozzle respectively; the inner diameter of the first nozzle is 10 to 20 μm, the inner diameter of the second nozzle is 60 to 80 μm, and the inner diameter of the third nozzle is 30 to 60 μm.
[0083] In addition, in the multi-needle electrospinning process, a high voltage electrostatic field needs to be applied to charge the spinning solution. According to the properties and viscosity of the spinning solution, a suitable voltage range is selected. In some preferred embodiments, the voltages of the first nozzle, the second nozzle, and the third nozzle are all 10 to 30 kV.
[0084] By limiting the consumption rates of the first spinning solution, the first spinning solution and the barium titanate dispersion, the preparation of polylactic acid fiber filter membranes with different mass ratios can be achieved. In some embodiments, the consumption rate of the first spinning solution is 0.8 to 2 mL / h, the consumption rate of the first spinning solution is 0.2 to 1.2 mL / h, and the consumption rate of the barium titanate dispersion is 0.2 to 1.5 mL / h.
[0085] The receiving device of multi-needle electrospinning can be a rotating drum, a flat plate or a mesh structure, etc. The distance of the receiving device will affect the deposition morphology and arrangement of the fibers. In some preferred embodiments, the receiving distances of the first nozzle, the second nozzle and the third nozzle are all 10 to 25 cm.
[0086] In some embodiments, the spinning temperature is 20-45° C., and the relative humidity of the environment is 25%-45%.
[0087] The third aspect of the present invention provides an air filter, comprising the polylactic acid fiber filter membrane provided by the first aspect or the polylactic acid fiber filter membrane prepared by the preparation method provided by the second aspect.
[0088] Due to the inclusion of the above-mentioned excellent performance polylactic acid fiber filter membrane, the air filter can achieve PM 0.3 and PM 2.5 It can effectively intercept particulate matter such as chlorine and can achieve long-term service.
[0089] The present application is further described in detail below in conjunction with specific examples, which should not be construed as limiting the scope of protection claimed in the present application. The weight average molecular weight of left-handed polylactic acid (PLLA) is 10KDa to 200KDa; the weight average molecular weight of right-handed polylactic acid (PDLA) is 200KDa to 450KDa.
[0090] Example 1
[0091] The preparation method of the polylactic acid fiber filter membrane of this embodiment comprises the following steps:
[0092] Step S11, preparing BaTiO3 nanoparticles: mixing titanium dioxide, barium chloride dihydrate and methanol to perform microwave-assisted synthesis of BaTiO3 nanoparticles, wherein the average diameter of the BaTiO3 nanoparticles is 10 nm; wherein the mass ratio of titanium dioxide to barium chloride dihydrate is 1:1, the amount of methanol is 40 mL, the output power of the microwave reactor is 800 W, the reaction temperature is 180° C., and the reaction time is 60 min;
[0093] Step S12, preparing a BaTiO3 dispersion: mixing BaTiO3 with dimethylformamide, and then adding polyvinyl pyrrolidone to obtain a BaTiO3 dispersion; wherein the mass ratio of BaTiO3 to the dispersant is 1:100, and the mass fraction of BaTiO3 in the dispersion is 0.25wt%;
[0094] Step S13, preparing spinning solution A and spinning solution B: PDLA and PLLA are mixed in a molar ratio of 1:10 as a matrix polymer, and the mixture is dissolved in a mixed solvent consisting of dichloromethane and ethanol (the volume ratio of dichloromethane to ethanol is 1:2) to prepare a spinning solution A with a concentration of 0.4wt%; PDLA and PLLA are mixed in a molar ratio of 1:15 as a matrix polymer, and the mixture is dissolved in a mixed solvent consisting of dimethylformamide and butanol (the volume ratio of dimethylformamide to butanol is 1:5) to prepare a spinning solution B with a concentration of 15wt%;
[0095] Step S14, preparing a polylactic acid fiber filter membrane: according to the mass ratio of the formed first fiber, the second fiber and the barium titanate support being 1:6.4:60, the spinning solution A and the spinning solution B of step S13 and the BaTiO3 dispersion of step S12 are subjected to multi-needle electrospinning to obtain a polylactic acid fiber filter membrane with a thickness of 300 μm; wherein the inner diameter of the nozzle used for the spinning solution A is 15 μm, the inner diameter of the nozzle used for the spinning solution B is 60 μm, and the inner diameter of the nozzle used for the BaTiO3 dispersion is 30 μm. m, the electrospinning voltage is 10 kV, the spinning temperature is 20 ℃, the relative humidity of the environment is 25%, the consumption rate of BaTiO3 dispersion is 0.2 mL / h, the consumption rate of spinning solution A is 0.8 mL / h, the consumption rate of spinning solution B is 0.2 mL / h, the spinning time is 1 h, the receiving distance is 17 cm, the diameter of the first fiber formed by spinning solution A is 100 nm, and the average pore size is 1 nm; the diameter of the second fiber formed by spinning solution B is 1 μm, and the average pore size is 2 nm.
[0096] Example 2
[0097] The preparation method of the polylactic acid fiber filter membrane of this embodiment comprises the following steps:
[0098] Step S21, preparing BaTiO3 nanoparticles: mixing titanium dioxide, barium acetate and ethanol to perform microwave-assisted synthesis of BaTiO3 nanoparticles, wherein the average diameter of the BaTiO3 nanoparticles is 15 nm; wherein the mass ratio of titanium dioxide to barium acetate is 1:4, the amount of ethanol is 30 mL, the output power of the microwave reactor is 700 W, the reaction temperature is 160° C., and the reaction time is 80 min;
[0099] Step S22, preparing a BaTiO3 dispersion: mixing BaTiO3 with dichloromethane, and then adding dodecyltrimethylammonium bromide as a dispersant to obtain a BaTiO3 dispersion; wherein the mass ratio of BaTiO3 to the dispersant is 1:60, and the mass fraction of BaTiO3 in the dispersion is 0.5wt%;
[0100] Step S23, preparing spinning solution A and spinning solution B: PDLA and PLLA are mixed in a molar ratio of 1:7 as a matrix polymer, and the mixture is dissolved in a mixed solvent consisting of chloroform and methanol (the volume ratio of chloroform and methanol is 1:3) to prepare a spinning solution A with a concentration of 5wt%; PDLA and PLLA are mixed in a molar ratio of 1:14 as a matrix polymer, and the mixture is dissolved in a mixed solvent consisting of N-methylpyrrolidone and glycerol (the volume ratio of N-methylpyrrolidone and glycerol is 1:6) to prepare a spinning solution B with a concentration of 18wt%;
[0101] Step S24, preparing a polylactic acid fiber filter membrane: according to the mass ratio of the formed first fiber, the second fiber and the barium titanate support of 1:12.5:22.5, the spinning solution A and the spinning solution B of step S23 and the BaTiO3 dispersion obtained in step S22 are subjected to multi-needle electrospinning to obtain a polylactic acid fiber filter membrane with a thickness of 20 μm; wherein the inner diameter of the nozzle used for the spinning solution A is 10 μm, the inner diameter of the nozzle used for the spinning solution B is 65 μm, and the inner diameter of the nozzle used for the BaTiO3 dispersion is 40 μm, the electrospinning voltage is 20 kV, the spinning temperature is 25 ℃, the relative humidity of the environment is 30%, the consumption rate of BaTiO3 dispersion is 0.8 mL / h, the consumption rate of spinning solution A is 1.0 mL / h, the consumption rate of spinning solution B is 0.5 mL / h, the spinning time is 1.2 h, the receiving distance is 15 cm, the diameter of the first fiber formed by spinning solution A is 30 nm, and the average pore size is 5 nm; the diameter of the second fiber formed by spinning solution B is 3 μm, and the average pore size is 25 nm.
[0102] Example 3
[0103] The preparation method of the polylactic acid fiber filter membrane of this embodiment comprises the following steps:
[0104] Step S31, preparing BaTiO3 nanoparticles: titanium dioxide, barium hydroxide and diethylene glycol are mixed to perform microwave-assisted synthesis of BaTiO3, wherein the average diameter of the BaTiO3 nanoparticles is 40 nm; wherein the mass ratio of titanium dioxide to barium hydroxide is 1:6, the amount of diethylene glycol is 10 mL, the output power of the microwave reactor is 1000 W, the reaction temperature is 100° C., and the reaction time is 30 min;
[0105] Step S32, preparing a BaTiO3 dispersion: mixing BaTiO3 with chloroform, and then adding sodium dodecyl sulfate dispersant to obtain a BaTiO3 dispersion; wherein the mass ratio of BaTiO3 to the dispersant is 1:40, and the mass fraction of BaTiO3 in the dispersion is 0.75wt%;
[0106] Step S33, preparing spinning solution A and spinning solution B: PDLA and PLLA are mixed in a molar ratio of 1:6 as a matrix polymer, and dissolved in a mixed solvent consisting of dimethylformamide and isopropanol (the volume ratio of dimethylformamide and isopropanol is 1:4) to prepare a spinning solution A with a concentration of 10wt%; PDLA and PLLA are mixed in a molar ratio of 1:12 as a matrix polymer, and dissolved in a mixed solvent consisting of ethyl acetate and propylene glycol (the volume ratio of ethyl acetate and propylene glycol is 1:7) to prepare a spinning solution B with a concentration of 20wt%;
[0107] Step S34, preparing a polylactic acid fiber filter membrane: according to the mass ratio of the formed first fiber, the second fiber and the barium titanate support of 1:25:26.7, the spinning solution A and the spinning solution B of step S33 and the BaTiO3 dispersion of step S32 are subjected to multi-needle electrospinning to obtain a polylactic acid fiber filter membrane with a thickness of 600 μm; wherein the inner diameter of the nozzle used for the spinning solution A is 19 μm, the inner diameter of the nozzle used for the spinning solution B is 75 μm, and the inner diameter of the nozzle used for the BaTiO3 dispersion is 45 μm; The electrospinning voltage is 25 kV, the spinning temperature is 30°C, the relative humidity of the environment is 37%, the consumption rate of BaTiO3 dispersion is 1.2 mL / h, the consumption rate of spinning solution A is 1.5 mL / h, the consumption rate of spinning solution B is 0.8 mL / h, the spinning time is 1.5 h, the receiving distance is 25 cm, the diameter of the first fiber formed by spinning solution A is 750 nm, and the average pore size is 22 nm; the diameter of the second fiber formed by spinning solution B is 8 μm, and the average pore size is 45 nm.
[0108] Example 4
[0109] The preparation method of the polylactic acid fiber filter membrane of this embodiment comprises the following steps:
[0110] Step S41, preparing BaTiO3 nanoparticles: mixing titanium dioxide, barium peroxide, and isopropanol solvent to perform microwave-assisted synthesis of BaTiO3, wherein the average diameter of the BaTiO3 nanoparticles is 60 nm; wherein the mass ratio of titanium dioxide to barium peroxide is 1:8, the amount of isopropanol is 100 mL, the output power of the microwave reactor is 500 W, the reaction temperature is 120° C., and the reaction time is 120 min;
[0111] Step S42, preparing a BaTiO3 dispersion: mixing BaTiO3 with N-methylpyrrolidone, and then adding sodium dodecylbenzenesulfonate dispersant to obtain a BaTiO3 dispersion; wherein the mass ratio of BaTiO3 to the dispersant is 1:10, and the mass of BaCO3 in the dispersion is 1wt%;
[0112] Step S43, preparing spinning solution A and spinning solution: PDLA and PLLA are mixed in a molar ratio of 1:5 as a matrix polymer, and dissolved in a mixed solvent consisting of chloroform and n-butanol (the volume ratio of chloroform and n-butanol is 1:5) to prepare a spinning solution A with a concentration of 15wt%; PDLA and PLLA are mixed in a molar ratio of 1:10 as a matrix polymer, and dissolved in a mixed solvent consisting of tetrahydrofuran and ethylene glycol (the mass ratio of tetrahydrofuran and ethylene glycol is 1:10) to prepare a spinning solution B with a concentration of 25wt%;
[0113] Step S44, preparing a polylactic acid fiber filter membrane: according to the mass ratio of the formed first fiber, the second fiber and the barium titanate support being 1:1.5:15, the spinning solution A and the spinning solution B of step S43 and the BaTiO3 dispersion of step S42 are subjected to multi-needle electrospinning to obtain a polylactic acid fiber filter membrane with a thickness of 200 μm; wherein the inner diameter of the nozzle used for the spinning solution A is 16 μm, the inner diameter of the nozzle used for the spinning solution B is 70 μm, and the inner diameter of the nozzle used for the BaTiO3 dispersion is 5 0μm, the electrospinning voltage is 22kV, the spinning temperature is 35℃, the relative humidity of the environment is 45%, the consumption rate of BaTiO3 dispersion is 1.mL / h, the consumption rate of spinning solution A is 2mL / h, the consumption rate of spinning solution B is 1.2mL / h, the spinning time is 2h, the receiving distance is 22cm, the diameter of the first fiber formed by spinning solution A is 600nm, and the average pore size is 20nm; the diameter of the second fiber formed by spinning solution B is 7μm, and the average pore size is 35nm.
[0114] Example 5
[0115] The preparation method of the polylactic acid fiber filter membrane of this embodiment comprises the following steps:
[0116] Step S51, preparing BaTiO3 nanoparticles: titanium dioxide, barium chloride dihydrate and methanol are mixed to perform microwave-assisted synthesis of BaTiO3 nanoparticles, wherein the average diameter of the BaTiO3 nanoparticles is 80 nm, wherein the mass ratio of titanium dioxide to barium chloride dihydrate is 1:1, the amount of methanol is 40 mL, the output power of the microwave reactor is 800 W, the reaction temperature is 180° C., and the reaction time is 60 min;
[0117] Step S52, preparing a BaTiO3 dispersion: mixing BaTiO3 with dimethylformamide, and then adding polyvinyl pyrrolidone to obtain a BaTiO3 dispersion; wherein the mass ratio of BaTiO3 to the dispersant is 1:100, and the mass fraction of BaTiO3 in the dispersion is 0.25wt%;
[0118] Step S53, preparing spinning solution A and spinning solution B: dissolving PLLA in a mixed solvent consisting of dichloromethane and ethanol (the volume ratio of dichloromethane to ethanol is 1:2) to prepare spinning solution A with a concentration of 0.4wt% and spinning solution B with a concentration of 15wt% respectively;
[0119] Step S54, preparing a polylactic acid fiber filter membrane: according to the mass ratio of the formed first fiber, the second fiber and the barium titanate support being 1:6.4:150, the spinning solution A and the spinning solution B of step S13 and the BaTiO3 dispersion of step S12 are subjected to multi-needle electrospinning to obtain a polylactic acid fiber filter membrane with a thickness of 500 μm; wherein the inner diameter of the nozzle used for the spinning solution A is 20 μm, the inner diameter of the nozzle used for the spinning solution B is 80 μm, and the inner diameter of the nozzle used for the BaTiO3 dispersion is 60 μm, The electrospinning voltage is 10 kV, the spinning temperature is 20°C, the relative humidity of the environment is 25%, the consumption rate of BaTiO3 dispersion is 0.2 mL / h, the consumption rate of spinning solution A is 0.8 mL / h, the consumption rate of spinning solution B is 0.5 mL / h, the spinning time is 1.5 h, the receiving distance is 17 cm, the diameter of the first fiber formed by spinning solution A is 800 nm, and the average pore size is 25 nm; the diameter of the second fiber formed by spinning solution B is 10 μm, and the average pore size is 50 nm.
[0120] Example 6
[0121] The difference from Example 2 is that in step S24, the inner diameter of the nozzle used for the spinning solution B is 160 μm, the diameter of the second fiber formed by the spinning solution B is 15 μm, and the average pore size is 80 nm.
[0122] Comparative Example 1
[0123] The preparation method of the polylactic acid fiber filter membrane of this comparative example comprises the following steps:
[0124] Step S1, PDLA and PLLA are mixed as a matrix polymer in a molar ratio of 1:8, and dissolved in a mixed solvent consisting of dichloromethane and glycerol (the volume ratio of dichloromethane and glycerol is 1:4) to prepare a spinning solution A with a concentration of 6wt%; PDLA and PLLA are mixed as a matrix polymer in a molar ratio of 1:13, and dissolved in a mixed solvent consisting of N-methylpyrrolidone and n-butanol (the volume ratio of N-methylpyrrolidone and n-butanol is 1:8) to prepare a spinning solution B with a concentration of 16wt%;
[0125] Step S2, according to the mass ratio of the first fiber to the second fiber of 3:4, the spinning solution A and the spinning solution B are subjected to multi-needle electrospinning to obtain a polylactic acid fiber filter membrane with a thickness of 350 μm; wherein, the inner diameter of the nozzle used for spinning solution A is 22 μm, the inner diameter of the nozzle used for spinning solution B is 83 μm, 4 mL of spinning solution A and spinning solution B are taken, the electrospinning voltage is 18 kV, the spinning temperature is 40°C, the relative humidity of the environment is 33%, the consumption rate of spinning solution A is 0.6 mL / h, the consumption rate of spinning solution B is 0.3 mL / h, the receiving distance is 19 cm, the spinning time is 1.5 h, the diameter of the first fiber obtained from spinning solution A is 850 nm, and the average pore size is 30 nm; the average diameter of the second fiber obtained from spinning solution B is 12 μm, and the average pore size is 60 nm.
[0126] Comparative Example 2
[0127] The preparation method of the polylactic acid fiber filter membrane of this comparative example comprises the following steps:
[0128] Step S1, mixing titanium dioxide, barium nitrate and propanol to prepare BaTiO3; wherein the mass ratio of titanium dioxide to barium nitrate is 1:10, and the propanol solvent is 90 mL; mixing BaTiO3 with dichloromethane, and then adding dodecyltrimethylammonium bromide dispersant to obtain a BaTiO3 dispersion; wherein the mass ratio of BaTiO3 to the dispersant is 1:60, the mass fraction of BaTiO3 in the dispersion is 0.3wt%, and the average diameter of BaTiO3 nanoparticles is 85nm;
[0129] Step S2, PDLA and PLLA are mixed in a molar ratio of 1:9 as a matrix polymer, and the mixture is dissolved in a mixed solvent consisting of dimethylformamide and butanol (the volume ratio of dimethylformamide and butanol is 1:5) to prepare a spinning solution A with a concentration of 6 wt%; PDLA and PLLA are mixed in a molar ratio of 1:11 as a matrix polymer, and the mixture is dissolved in a mixed solvent consisting of dichloromethane and ethanol (the volume ratio of dichloromethane and ethanol is 1:9) to prepare a spinning solution B with a concentration of 22 wt%;
[0130] Adding BaTiO3 dispersion to spinning solution A and spinning solution B respectively to obtain spinning solution C and spinning solution D;
[0131] Step S3, according to the mass ratio of PDLA+PLLA in the first fiber, PDLA+PLLA in the second fiber, and the total mass of BaTiO3 in the first fiber and the second fiber of 1:1.6:11.7, the spinning solution C and the spinning solution D are subjected to multi-needle electrospinning to obtain a polylactic acid fiber filter membrane with a thickness of 80 μm; wherein the inner diameter of the spinning nozzle used for the spinning solution C is 25 μm, the inner diameter of the spinning nozzle used for the spinning solution D is 85 μm, the electrospinning voltage is 12 kV, the spinning temperature is 45°C, the relative humidity of the environment is 42%, the spinning solution C consumption rate is 0.4 mL / h, the spinning solution D consumption rate is 0.8 mL / h, the spinning time is 2 h, the receiving distance is 14 cm, the diameter of the first fiber obtained from the spinning solution C is 900 nm, the average pore size is 50 nm, the diameter of the second fiber obtained from the spinning solution D is 15 μm, and the average pore size is 80 nm.
[0132] Comparative Example 3
[0133] Step S1, preparing Zr-MOFs nanocrystals: dissolving 2 mol / L zirconium tetrachloride solution and 1,4-benzenedicarboxylic acid (the volume ratio of zirconium tetrachloride solution to 1,4-benzenedicarboxylic acid is 1:1) in dimethylformamide (the volume ratio of zirconium tetrachloride solution to dimethylformamide is 1:10), and then placing in a microwave reactor (500 W, 120° C., 30 min), obtaining a Zr-MOFs dispersion after reaction, extracting and drying (drying temperature is 60° C., time 24 h) to obtain Zr-MOFs nanocrystals (crystal size is 200 nm, pore size is 1.2 nm);
[0134] Step S2, preparing a stable Zr-MOFs dispersion: dispersing Zr-MOFs nanocrystals in dimethylformamide (the mass ratio of Zr-MOFs to dimethylformamide is 1:20), adding polyvinyl pyrrolidone (the mass ratio of Zr-MOFs to polyvinyl pyrrolidone is 20:1), and obtaining a stable Zr-MOFs dispersion after ultrasonic dispersion for 3 hours;
[0135] Step S3, adding L-polylactic acid to dimethylformamide and magnetically stirring for 6 hours to obtain a first polylactic acid solution with a relatively high concentration (concentration of 120 g / L) and a second polylactic acid solution with a relatively low concentration (concentration of 60 g / L);
[0136] Step S4, the first polylactic acid solution is loaded into a syringe pump with a metal needle inner diameter of 0.33mm (take 1mL, electrospinning positive voltage is 10kV, negative voltage is 5kV, receiving distance is 10cm, solution consumption rate is 3mL / h, roller speed is 500rpm), the second polylactic acid solution is loaded into a syringe pump with a metal needle inner diameter of 0.86mm (take 1mL, electrospinning positive voltage is 30kV, negative voltage is 1kV, receiving distance is 30cm, solution consumption rate is 1mL / h, Zr-MOF s dispersion used in the nozzle inner diameter of 43μm, the consumption rate of Zr-MOFs dispersion was 0.8mL / h, the spinning time was 1h, the roller speed was 500rpm), and multi-needle electrospinning (ambient temperature was 20°C, relative humidity was 45%) was carried out to prepare polylactic acid fiber filter membrane. The diameter of the first fiber obtained from the first polylactic acid solution was 1.5μm, and the average pore size was 100nm. The diameter of the second fiber obtained from the second polylactic acid solution was 20μm, and the average pore size was 150nm. The thickness of the obtained fiber membrane was 300μm.
[0137] Comparative Example 4
[0138] The preparation method of the polylactic acid fiber filter membrane of this comparative example comprises the following steps:
[0139] Step S1, mixing titanium dioxide, barium nitrate and propanol to prepare BaTiO3; wherein the mass ratio of titanium dioxide to barium nitrate is 1:10, and the propanol solvent is 85 mL; mixing BaTiO3 with dichloromethane, and then adding dodecyltrimethylammonium bromide dispersant to obtain a BaTiO3 dispersion; wherein the mass ratio of BaTiO3 to the dispersant is 1:68, the mass fraction of BaTiO3 in the dispersion is 1.5wt%, and the average diameter of BaTiO3 nanoparticles is 90nm;
[0140] Step S2, PDLA and PLLA are mixed as a matrix polymer in a molar ratio of 1:8, and dissolved in a mixed solvent consisting of dichloromethane and glycerol (the volume ratio of dichloromethane and glycerol is 1:4) to prepare a spinning solution A with a concentration of 16wt%; PDLA and PLLA are mixed as a matrix polymer in a molar ratio of 1:13, and dissolved in a mixed solvent consisting of N-methylpyrrolidone and n-butanol (the volume ratio of N-methylpyrrolidone and n-butanol is 1:8) to prepare a spinning solution B with a concentration of 28wt%;
[0141] Step S3, according to the mass ratio of the formed first fiber, the second fiber and the barium titanate support being 1:12.8:11.2, the spinning solution A and the spinning solution B obtained in S2 and the BaTiO3 dispersion obtained in S1 are subjected to multi-needle electrospinning to obtain a polylactic acid fiber filter membrane with a thickness of 450 μm; wherein the inner diameter of the nozzle used for the spinning solution A is 26 μm, the inner diameter of the nozzle used for the spinning solution B is 90 μm, 4 mL of the spinning solution A and the spinning solution B are taken, the electrospinning voltage is 18 kV, and the spinning temperature is The temperature was 40°C, the relative humidity was 33%, the inner diameter of the nozzle used for the BaTiO3 dispersion was 75 μm, the consumption rate of the BaTiO3 dispersion was 0.5 mL / h, the consumption rate of spinning solution A was 0.6 mL / h, the consumption rate of spinning solution B was 0.3 mL / h, the spinning time was 1.5 h, the receiving distance was 19 cm, the diameter of the first fiber obtained from spinning solution A was 960 nm, and the average pore size was 80 nm; the diameter of the second fiber obtained from spinning solution B was 18 μm, and the average pore size was 100 nm.
[0142] Comparative Example 5
[0143] The difference from Example 2 is that the inner diameter of the nozzle used for spinning solution A is 12 μm, the inner diameter of the nozzle used for spinning solution B is 400 μm, the diameter of the first fiber formed by spinning solution A is 50 nm, and the average pore size is 7 nm; the diameter of the second fiber formed by spinning solution B is 30 μm, and the average pore size is 200 nm.
[0144] Test example
[0145] 1. Tensile performance test
[0146] The polylactic acid fiber filter membrane was cut to obtain tensile specimens, and its tensile properties were tested using a universal tensile machine (model 4403, sensor 100N) according to the ASTM D638-2003 plastic tensile properties test standard of the American Society for Testing and Materials. At least 3 parallel test samples were guaranteed for each group, and the results were averaged.
[0147] 2. Surface potential test
[0148] The surface potential of the polylactic acid fiber filter membrane was tested using a non-contact electrostatic meter (VM54XQS, Quatek, USA) at a test height of 2 cm. The temperature and humidity were constant at 25°C and 45%. 20 data points were randomly collected for each sample and the average value was taken.
[0149] 3. Filtration performance test
[0150] The polylactic acid fiber filter membrane (area 113.04cm 2) air filtration performance, the gas flow rate was set to 85L / min, and the particle size range of NaCl atomized particles produced by the aerosol generator was 0.1-10μm. At least 3 different positions of each group of fiber membranes were tested, and the results were averaged.
[0151] 4. Air resistance test
[0152] Respiratory resistance test: A micromanometer (AIRPRO AP800, TSI, USA), anthropomorphic respirator and simulated human head were used to measure respiratory resistance. The gas flow rate was set to 10, 32, 65, and 85 L / min. The filter membrane was encapsulated on a simulated human head, and the air pressure of the cavity composed of the filter material and the human head and the atmosphere were measured and subtracted. The experiment was repeated three times and the average value was taken to calculate the respiratory resistance (i.e., air resistance) of the filter membrane.
[0153] 5. Antibacterial performance test
[0154] The selected strains were Escherichia coli and Staphylococcus aureus, and the strains were cultured in lysate broth (LB) medium at 37°C for 16 h. After incubation, 0.5 mL of Escherichia coli and 0.5 mL of Staphylococcus aureus were washed, combined, and suspended in 0.85% NaCl solution to obtain 1 mL of cell mixture with a cell density of 10 9 CFU / mL. Then dilute 10 times with the above NaCl solution to a cell density of 10 8 CFU / mL. The polylactic acid fiber filter membrane was cut into discs with a diameter of 10 cm and immersed in 100 μL of bacterial suspension. The polylactic acid fiber filter membrane was treated with light irradiation using a solar simulator (HSX-F300, NBeT). The optical density was measured using a solar power meter (VLP-2000, NBeT). The sample was kept at 25 cm from the light and irradiated for 30 minutes under light with a wavelength of 600 nm. The temperature was detected using a thermal imaging camera (HT-18, HTI). A control group was also set up (without antibacterial effect under sunlight). The bacterial suspension was serially diluted and the CFU counted until the cell density was approximately 10 2 CFU / mL, the plates were cultured overnight (37°C, RH75%), and the antibacterial efficiency was calculated by counting CFU. Three experiments were performed in each group, and the results were averaged.
[0155] The morphological and structural parameters of the polylactic acid fiber filtration membranes of the embodiments and comparative examples are shown in Table 1, and the test results are shown in Table 2 and Table 3.
[0156] Table 1
[0157]
[0158]
[0159] Table 2
[0160]
[0161] Table 3
[0162]
[0163] according to Figure 1 and Figure 2 It can be seen that the fiber surface of the polylactic acid fiber filter membrane provided by the present invention is uniformly loaded with barium titanate particles, while the fiber surface of the polylactic acid fiber filter membrane of comparative example 2 is basically free of particles, and the barium titanate is embedded in the fiber.
[0164] Table 1 lists the thickness of the polylactic acid fiber filter membrane, the diameter of the first fiber, the second fiber, the pore size, and their diameter ratio. Table 2 lists the test results of the mechanical properties, surface potential, and filtration performance of the polylactic acid fiber filter membrane in the embodiments and comparative examples. Table 3 lists the test results of the antibacterial efficiency of the polylactic acid fiber filter membrane in the embodiments and comparative examples.
[0165] According to Table 2, in Examples 1 to 6 and Comparative Examples 4 to 5, the breaking strength of the fiber membrane is between 17.7 and 35.5 MP. As the content of barium titanate increases, the breaking strength of the fiber membrane first increases and then decreases. This is mainly because when the content of barium titanate (BaTiO3) is low, the addition of the dispersant can make it evenly dispersed in the solution. The dispersed BaTiO3 plays a role in crystallization and forming crystal nuclei in the polymer, which helps to increase the crystallinity of the fiber and increase the physical cross-linking points in the molecule, thereby playing a reinforcing role. However, as the crystallinity increases to a certain extent, the toughness of the fiber membrane will decrease accordingly. When the content of BaTiO3 is too large, it cannot be evenly dispersed, resulting in local agglomeration, which increases the stress concentration points of the fiber. At the same time, the crystallization effect is weakened, resulting in a decrease in breaking strength. Therefore, the present invention helps to improve the mechanical strength of the fiber filtration membrane by adding an appropriate amount of BaTiO3.
[0166] According to Table 2, the fiber filter membranes in Examples 1 to 6 and Comparative Examples 4 to 5 all exhibit extremely high surface potentials (10.6 to 18.3 kV). The addition of BaTiO3 enhances the piezoelectric properties of the fiber filter membrane, enhances the electrostatic adsorption force and hardly decays over time, proving to have extremely high long-term stability. The ultra-high surface potential and enhanced fiber constraint properties make the fiber an ideal platform for molecular sieving and adsorption separation, usually showing stronger load capacity and lower mass transfer resistance. Specifically, the surface potential drop rate of the fiber filter membrane in Examples 1 to 6 is ≤8.33% in 7 days and ≤12.14% in 30 days, while the surface potential drop rate of the fiber filter membrane in Comparative Examples 1 to 5 is ≥22.22% in 7 days and ≥32.08% in 30 days. This shows that the fiber filter membrane provided by the present invention has extremely high long-term stability and can achieve a long service cycle.
[0167] The fiber filtration membranes in Examples 1 to 6 have a significant effect on PM 0.3 and PM 2.5 The filtration efficiency of the fiber filtration membrane of Comparative Example 1 is lower than that of PM. 0.3 and PM 2.5 The filtration efficiency is low for PM 0.3 The filtration efficiency is 68.3% for PM 2.5 The filtration efficiency is 70.4%.
[0168] According to Table 3, the fiber filter membranes in Examples 1 to 6 and Comparative Examples 1 to 5 show the antibacterial efficiency of the fiber filter membranes against Escherichia coli and Staphylococcus aureus under the conditions of illumination and no illumination. The fiber filter membrane in Comparative Example 1 has no obvious antibacterial effect on Escherichia coli and Staphylococcus aureus, with an antibacterial rate of 21.9% for Escherichia coli and 23.6% for Staphylococcus aureus. However, with the increase of BaTiO3 content, the antibacterial rate of Escherichia coli and Staphylococcus aureus increased. The fiber filter membrane in Example 1 has an inhibition rate of 33.2% and 30.1% against Escherichia coli and Staphylococcus aureus under no light conditions, respectively. After photocatalysis, the inhibition rates against Escherichia coli and Staphylococcus aureus reach 88.8% and 86.4%, respectively. The fiber filter membrane in Example 2 has an inhibition rate of 34.5% and 31.7% against Escherichia coli and Staphylococcus aureus under no light conditions, respectively. After photocatalysis, the inhibition rates against Escherichia coli and Staphylococcus aureus reach 92.7% and 93.4%, respectively. The fiber filter membrane in Example 3 has an antibacterial rate of 38.3% and 35.9% against Escherichia coli and Staphylococcus aureus under no light conditions, and after photocatalysis, the antibacterial rates against Escherichia coli and Staphylococcus aureus reach 99.8% and 96.7% respectively; the fiber filter membrane in Example 4 has an antibacterial rate of 40.2% and 39.1% against Escherichia coli and Staphylococcus aureus under no light conditions, and after photocatalysis, the antibacterial rates against Escherichia coli and Staphylococcus aureus reach 98.8% and 98.9% respectively. The fiber filter membrane in Example 5 has an antibacterial rate of 41.1% and 39.5% against Escherichia coli and Staphylococcus aureus under no light conditions, and after photocatalysis, the antibacterial rates against Escherichia coli and Staphylococcus aureus reach 98.2% and 98.7% respectively. The fiber filtration membrane in Example 6 has an inhibition rate of 41.2% and 39.3% against Escherichia coli and Staphylococcus aureus respectively under no light conditions. After photocatalysis, the inhibition rate against Escherichia coli and Staphylococcus aureus reaches 98.4% and 98.8% respectively.
[0169] Comparing Example 3 with Example 5, it can be seen that the introduction of PDLA can further improve the filtration efficiency and the antibacterial rate of Escherichia coli. Comparing Examples 1 to 6 with Comparative Examples 2, 4, and 5, it can be seen that the introduction of BaTiO3 and the limitation of the first fiber, the second fiber, and the barium titanate support in a specific mass ratio can help the polylactic acid fiber filtration membrane to have high breaking strength, high surface potential, high antibacterial efficiency, and high filtration efficiency.
[0170] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A polylactic acid fiber filter membrane, characterized in that: The polylactic acid fiber filtration membrane comprises a first fiber, a second fiber and a barium titanate support, the first fiber and the second fiber are randomly stacked, and the barium titanate support is supported on the surface of the first fiber and the second fiber; Among them, the diameter ratio of the first fiber to the second fiber is 1:(10-500); the first fiber and the second fiber both include polylactic acid; the mass ratio of the first fiber, the second fiber and the barium titanate support is 1:(1.5-25):(15-150).
2. The polylactic acid fiber filtration membrane according to claim 1, characterized in that: The diameter of the first fiber is 30-800 nm, and the average pore size is 1-25 nm; and / or, the diameter of the second fiber is 1-10 μm, and the average pore size is 2-50 nm; and / or, the barium titanate support is granular, and the average diameter of the barium titanate support is 10-80 nm.
3. The polylactic acid fiber filtration membrane according to claim 1, characterized in that: The first fiber and the second fiber both include left-handed polylactic acid and right-handed polylactic acid; Preferably, the first fiber comprises a first left-handed polylactic acid and a first right-handed polylactic acid, and the second fiber comprises a second left-handed polylactic acid and a second right-handed polylactic acid; Wherein, the molar ratio of the second L-polylactic acid to the second D-polylactic acid is greater than the molar ratio of the first L-polylactic acid to the first D-polylactic acid; Preferably, the molar ratio of the first L-polylactic acid to the first D-polylactic acid is (5-10):1; Preferably, the molar ratio of the second L-polylactic acid to the second D-polylactic acid is (10-15):
1.
4. The polylactic acid fiber filtration membrane according to claim 3, characterized in that: The weight average molecular weight of the first L-polylactic acid is 10KDa to 150KDa; and / or, the weight average molecular weight of the first D-polylactic acid is 200KDa to 350KDa; and / or, the weight average molecular weight of the second L-polylactic acid is 50KDa to 200KDa; and / or, the weight average molecular weight of the second D-polylactic acid is 300KDa to 450KDa.
5. The polylactic acid fiber filtration membrane according to any one of claims 1 to 4, characterized in that: The thickness of the polylactic acid fiber filter membrane is 20 to 600 μm; and / or, the breaking strength of the polylactic acid fiber filter membrane is 17 to 36 MPa, preferably 25.6 to 36 MPa; and / or, at a temperature of 25°C and a humidity of 45%, the surface potential of the polylactic acid fiber filter membrane is 12 to 20 kV; and / or, the polylactic acid fiber filter membrane has a PM 0.3 and PM 2.5 The filtration efficiency is ≥98%; and / or, at a gas flow rate of 10 to 85 L / min, the air resistance of the polylactic acid fiber filter membrane is ≤80 Pa; and / or, under light with a wavelength of 600 nm, the antibacterial rate of the polylactic acid fiber filter membrane against Escherichia coli and Staphylococcus aureus is ≥86%.
6. A method for preparing a polylactic acid fiber filtration membrane according to any one of claims 1 to 5, characterized in that: The following steps are involved: Performing multi-needle electrospinning on the first spinning solution, the second spinning solution, and the barium titanate dispersion to obtain the polylactic acid fiber filter membrane; Wherein, the first spinning solution and the second spinning solution both contain polylactic acid.
7. The preparation method according to claim 6, characterized in that: The preparation method of the first spinning solution comprises: dissolving the first polylactic acid in a first solvent to obtain the first spinning solution; The preparation method of the second spinning solution comprises: dissolving the second polylactic acid in a second solvent to obtain the second spinning solution; Preferably, the first polylactic acid and the second polylactic acid both include left-handed polylactic acid and right-handed polylactic acid; Preferably, the first polylactic acid comprises a first left-handed polylactic acid and a first right-handed polylactic acid, and the second polylactic acid comprises a second left-handed polylactic acid and a second right-handed polylactic acid; wherein the molar ratio of the second left-handed polylactic acid to the second right-handed polylactic acid is greater than the molar ratio of the first left-handed polylactic acid to the first right-handed polylactic acid; Preferably, the molar ratio of the first L-polylactic acid to the first D-polylactic acid is (5-10):1; Preferably, the sum of the mass fractions of the first L-polylactic acid and the first D-polylactic acid in the first spinning solution is 0.4% to 15%; Preferably, the first solvent includes a first good solvent and a first non-good solvent, and the volume ratio of the first good solvent to the first non-good solvent is 1:(2-5); Preferably, the molar ratio of the second L-polylactic acid to the second D-polylactic acid is (10-15):1; Preferably, the sum of the mass fractions of the second right-handed polylactic acid and the second left-handed polylactic acid in the second spinning solution is 15% to 25%; Preferably, the second solvent includes a second good solvent and a second non-good solvent, and the volume ratio of the second good solvent to the second non-good solvent is 1:(5-10); Preferably, the first good solvent and the second good solvent each independently include at least one of dichloromethane, chloroform, dimethylformamide, N-methylpyrrolidone, tetrahydrofuran, and ethyl acetate, and the first non-good solvent and the second non-good solvent each independently include at least one of methanol, ethanol, isopropanol, glycerol, butanol, ethylene glycol, and propylene glycol; More preferably, the first good solvent includes at least one of dichloromethane, chloroform, and dimethylformamide, the second good solvent includes at least one of dimethylformamide, N-methylpyrrolidone, ethyl acetate, and tetrahydrofuran, the first non-good solvent includes at least one of ethanol, methanol, isopropanol, and n-butanol, and the second non-good solvent includes at least one of butanol, glycerol, propylene glycol, and ethylene glycol.
8. The preparation method according to claim 6, characterized in that: The preparation method of the barium titanate dispersion comprises: Mixing barium titanate, a dispersant and a third solvent to obtain the barium titanate dispersion; Preferably, the preparation method of barium titanate comprises: Mixing titanium dioxide, a barium compound and a fourth solvent, and subjecting the mixture to microwave treatment to obtain the barium titanate; Preferably, the dispersant includes at least one of polyvinyl pyrrolidone, dodecyltrimethylammonium bromide, sodium dodecyl sulfate, and sodium dodecylbenzene sulfonate; Preferably, the third solvent includes at least one of dimethylformamide, dichloromethane, chloroform, and N-methylpyrrolidone; Preferably, the mass ratio of the barium titanate to the dispersant is 1:(10-100); Preferably, the mass fraction of the barium titanate in the barium titanate dispersion is 0.25% to 1%; Preferably, the mass ratio of the titanium dioxide to the barium compound is 1:(1-10); Preferably, the microwave treatment has a power of 500-1500 W, a temperature of 100-200° C., and a time of 20-120 min; Preferably, the barium compound includes at least one of barium hydroxide, barium chloride dihydrate, barium acetate, barium nitrate, and barium peroxide; Preferably, the fourth solvent comprises at least one of diethylene glycol, hexafluoroisopropanol, methanol, ethanol, isopropanol, glycerol, and water; More preferably, the fourth solvent includes at least one of diethylene glycol, methanol, ethanol and isopropanol.
9. The preparation method according to claim 6, characterized in that: In the multi-needle electrospinning process, the metal nozzles loaded with the first spinning solution, the second spinning solution and the barium titanate dispersion are respectively the first nozzle, the second nozzle and the third nozzle; Preferably, the inner diameter of the first nozzle is 10-20 μm, the inner diameter of the second nozzle is 60-80 μm, and the inner diameter of the third nozzle is 30-60 μm; Preferably, the voltages of the first nozzle, the second nozzle and the third nozzle are all 10-30 kV; Preferably, the consumption rate of the first spinning solution is 0.8 to 2 mL / h, the consumption rate of the second spinning solution is 0.2 to 1.2 mL / h, and the consumption rate of the barium titanate dispersion is 0.2 to 1.5 mL / h; Preferably, the receiving distances of the first nozzle, the second nozzle and the third nozzle are all 10-25 cm.
10. An air filter, characterized in that: It comprises the polylactic acid fiber filter membrane described in any one of claims 1 to 5 or the polylactic acid fiber filter membrane prepared by the preparation method described in any one of claims 6 to 9.