Ethylene propylene rubber liquid condensation and devolatilization system and method

Through the optimization of the ratio of multi-kettle coagulation system and dispersant, the problems of low solvent separation rate and difficult control of the particle size of the rubber during the aggregation of ethylene-propylene rubber are solved, and the uniformity and stable operation of the rubber particles are achieved, and the colloid is avoided. , improves solvent recovery efficiency.

CN119075875APending Publication Date: 2024-12-06SHAANXI COAL & CHEM TECH INST
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411199157.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-29
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

In the prior art, the solvent separation rate, the particle size of the rubber is not easy to control, and the rubber particles are prone to agglomeration during the agglomeration process.

Method used

Using a multi-kettle coagulation system, through a thermostat, a glue liquid injector and three condensation kettles connected in series, combined with the principles of water vapor distillation and wet degassing, the process flow of gas-liquid phase full countercurrent is used, and a variety of dispersants are added and Heat desalination water, control the agglomeration conditions to ensure uniformity of the colloid and solvent separation to prevent colloid clumping.

Benefits of technology

The uniformity of the colloid particles, stable moisture content and low volatile content are achieved, the solvent recovery efficiency is improved, the agglomeration equipment is absorbed, and continuous and stable operation is ensured.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119075875A_ABST
    Figure CN119075875A_ABST
Patent Text Reader

Abstract

The invention discloses an ethylene propylene rubber liquid condensation and devolatilization method which comprises the following steps: step 1, after starting, continuously adding a dispersing agent 1 # into a condensation kettle 1 #, a condensation kettle 2 # and a condensation kettle 3 #, mixing a dispersing agent 2 # and thermal desalted water, feeding the mixture into a temperature controller for heating, and feeding the mixture, a dispersing agent 3 # and an ethylene propylene rubber liquid into a glue liquid ejector together after heating, medium-pressure steam is introduced into the glue liquid ejector, and the mixed liquid is heated and pressurized through the medium-pressure steam; and 2, carrying out condensation devolatilization treatment on the heated and pressurized mixed solution obtained in the step 1 to finally obtain the ethylene propylene rubber aqueous colloidal particles. The invention further discloses an ethylene propylene rubber liquid condensation and devolatilization system. The defects that the solvent separation rate is low, the particle size of colloidal particles is not easy to control and the colloidal particles are easy to agglomerate again in a coagulation kettle in the ethylene propylene rubber coagulation in the prior art are overcome.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of polymer production, in particular to an ethylene-propylene rubber glue solution condensation devolatilization system and an ethylene-propylene rubber glue solution condensation devolatilization method. Background Art

[0002] Ethylene propylene rubber is a synthetic rubber with ethylene and propylene as the main monomers. According to the different monomer compositions in the molecular chain, it is divided into EPDM and EPDM. The former is a copolymer of ethylene and propylene, represented by EPM, and the latter is a copolymer of ethylene, propylene and a small amount of non-conjugated diene third monomer, represented by EPDM. The two are collectively referred to as ethylene propylene rubber, namely ethylene propylene rubber (EPR). Ethylene propylene rubber (EPR) is a synthetic rubber with excellent natural aging resistance, ozone resistance, heat aging resistance and electrical insulation. It is widely used in automotive parts, waterproof materials for construction, wire and cable sheaths, heat-resistant hoses, tapes, automotive seals, lubricant additives and other products. The proportion of EPDM in the consumption of synthetic rubber is gradually increasing.

[0003] The EPDM polymerization process usually uses hexane as solvent, V-A1 catalyst system or metallocene catalyst system, the monomer is dissolved in the solvent, and the polymerization reaction is carried out in the solution. The process technology of producing EPDM by solution polymerization is mature and the product quality is stable. Moreover, the wet coagulation process is currently used in the production process of EPDM. This method sprays the polymer glue generated by polymerization into hot water that serves as both a heat transfer medium and a conveying medium, and uses water vapor to strip and recover the solvent (including unreacted monomers) in it to achieve the purpose of separating the two. The solvent is recovered by distillation + refining.

[0004] Research has found that the density of EPDM raw rubber is 0.855-0.90kg / m. The characteristic of this type of rubber is that after the rubber liquid forms rubber particles in the coagulation kettle, the solvent wrapped in it is not easy to diffuse out. In addition, it is easy to have problems such as the phenomenon of rubber particles sandwiching, excessive strength of rubber particles in the coagulation kettle, difficulty in cutting, agglomeration of rubber particles, blockage and rubber particles holding the axis. Therefore, the difficulties in the coagulation of EPDM are: 1. How to separate a large amount of solvent from the rubber liquid. 2. How to control the size of the rubber particles after coagulation to facilitate the transportation of subsequent unit rubber particles. 3. How to prevent the agglomeration of rubber particles in the coagulation unit.

[0005] At present, the EPDM rubber coagulation unit generally has problems such as uneven and difficult to control particle size distribution, low solvent recovery rate, and re-agglomeration of particles. Summary of the invention

[0006] The first purpose of the present invention is to provide an ethylene propylene rubber glue liquid coagulation and devolatilization system, which solves the defects of low solvent separation rate, difficult to control the particle size of the rubber particles and easy re-agglomeration of the rubber particles in the coagulation kettle in the prior art of ethylene propylene rubber coagulation.

[0007] The second object of the present invention is to provide a method for condensation and devolatilization of ethylene-propylene rubber solution, which solves the defects of low solvent separation rate, difficult control of particle size of rubber particles and easy re-agglomeration of rubber particles in the condensation kettle in the prior art of ethylene-propylene rubber condensation.

[0008] The first technical solution adopted by the present invention is that the ethylene propylene rubber glue liquid condensation and devolatilization system includes a temperature controller, a glue liquid injector, a 1# condensation kettle, a 2# condensation kettle and a 3# condensation kettle connected in sequence, a first glue particle water pump and a glue particle filter are arranged on the pipeline connecting the 1# condensation kettle and the 2# condensation kettle, the glue particle filter is arranged at the outlet of the first glue particle water pump, and the glue particle filter is also connected to the top wall of the 1# condensation kettle through a pipeline; a first grinding pump is arranged on the pipeline connecting the 2# condensation kettle and the 3# condensation kettle, and a second grinding pump is arranged on the discharge pipeline of the 3# condensation kettle; it also includes a second glue particle water pump and a third glue particle water pump, the second glue particle water pump is connected to the top and bottom of the 2# condensation kettle respectively through a pipeline, and the third glue particle water pump is connected to the top and bottom of the 3# condensation kettle respectively through a pipeline; the bottom walls of the 1# condensation kettle, the 2# condensation kettle and the 3# condensation kettle are all connected to the low-pressure steam pipeline.

[0009] The present invention is also characterized in that:

[0010] An exhaust pipe is provided on the top of the 1# condensation kettle; agitators are provided inside the 1# condensation kettle, the 2# condensation kettle and the 3# condensation kettle, and the paddle type of the agitators inside the 1# condensation kettle, the 2# condensation kettle and the 3# condensation kettle is consistent; the agitator includes three layers of blades, specifically: the top layer blades are downward pressure paddle type, the middle layer and the lower layer blades are flat push paddles, and an annular distributor is also provided inside the 1# condensation kettle.

[0011] The distributor comprises an annular water distribution pipe which is provided with a plurality of spray nozzles.

[0012] A first glue-water separator is arranged on the pipeline connecting the second glue water pump and the top wall of the 2# coagulation kettle, and the first glue-water separator is also connected to the collecting tank through the pipeline;

[0013] A second glue-water separator is arranged on the pipeline connecting the third glue water pump and the top wall of the 3# coagulation kettle, and the second glue-water separator is also connected to the collecting tank through the pipeline.

[0014] The filter screen used by the particle filter is V-shaped. The V-shaped filter screen is conducive to the separation of particles and condensed water, and the particles are not easy to clog the filter screen.

[0015] The second technical solution adopted by the present invention is a method for condensation devolatilization of ethylene-propylene rubber solution, using the above-mentioned system, comprising the following steps:

[0016] Step 1: After starting, dispersant 1# is continuously added to 1# condensation kettle, 2# condensation kettle and 3# condensation kettle. Dispersant 2# is mixed with hot desalted water and then enters the temperature controller for heating. After heating, it enters the glue liquid injector together with dispersant 3# and EPDM glue liquid. Medium-pressure steam is passed through the glue liquid injector, and the mixed liquid is heated and pressurized by the medium-pressure steam.

[0017] Step 2: The mixed solution obtained in step 1 after heating and pressurizing is subjected to condensation and devolatilization treatment to finally obtain EPDM rubber hydrocolloid particles.

[0018] The present invention is also characterized in that:

[0019] Step 1 is specifically as follows: after starting, dispersant 1# is continuously added to 1# condensation kettle, 2# condensation kettle and 3# condensation kettle, dispersant 2# and hot desalted water are mixed and then enter the temperature controller for heating, the operating temperature is 85°C-87°C, and the pressure is 0.07MPa-0.08MPa; after the heating is completed, it enters the glue liquid injector together with dispersant 3# and EPDM rubber glue, and the glue liquid injector is passed with medium-pressure steam. The mixed liquid is heated and pressurized by the medium-pressure steam, and the operating temperature is 88°C-90°C, and the pressure is 0.3MPa-0.4MPa.

[0020] In step 1, dispersant 1# is an aqueous solution of polycarboxylate with a concentration of 50 g / L; dispersant 2# is an aqueous solution of calcium chloride with a concentration of 50 g / L; dispersant 3# is an aqueous solution of a preparation agent with a concentration of 50 g / L, and the preparation agent is composed of the following raw materials: surfactant, talcum powder, defoamer, zinc stearate and sodium hydroxide; wherein the mass ratio of surfactant, talcum powder, defoamer and zinc stearate is 0.5-0.6:25-30:1.5-2.0:6.5-7.0, and the amount of sodium hydroxide is to adjust the pH value of dispersant 3# to 9-10;

[0021] The volume ratio of hot desalted water and dispersant 2# is: hot desalted water: glue solution = 1-2:10;

[0022] The mass ratios of the three dispersants to the condensed water in the 1# condensation kettle are: dispersant 1#: condensed water = 1-2:500, dispersant 2#: condensed water = 1-2:500, dispersant 3#: condensed water = 1-4:4400;

[0023] The volume ratio of condensed water to EPDM rubber solution in the 1# condensation kettle is 1.0-2:1.

[0024] Step 2 is specifically as follows: the mixed liquid obtained in step 1 after heating and pressure increase is sprayed into the bottom of the 1# coagulation kettle, the operating temperature of the 1# coagulation kettle is 85°C-95°C, and the pressure is 0.05MPa-0.10MPa; finally, uniform particles are formed in the 1# coagulation kettle, the solvent hexane in the EPDM rubber solution is vaporized and discharged from the top of the 1# coagulation kettle, the particles and the particles water are recycled after condensation and enter the first particles water pump, and then separated by the particles filter, part of the particles water is refluxed from the top of the 1# coagulation kettle to the 1# coagulation kettle, and the remaining particles water transports the particles into the 2# coagulation kettle, and the 2# coagulation kettle is operated. The temperature is 95℃-105℃, and the pressure is 0.05MPa-0.08MPa. After the second desolventization of the colloid particles in the 2# condensation kettle, they enter the first grinding pump together with the colloid particle water. After the colloid particles are ground by the first grinding pump, the ground colloid particles and the colloid particle water enter the 3# condensation kettle together. The operating temperature of the 3# condensation kettle is 95℃-100℃, and the pressure is 0.05MPa-0.08MPa, and the third desolventization is carried out. Then the colloid particles and the colloid particle water enter the second grinding pump together, and the ground colloid particles and the colloid particle water are sent to the roller screen together for post-processing.

[0025] The beneficial effects of the present invention are:

[0026] (1) Aiming at the difficulty of preventing the colloid particles from agglomerating in the agglomeration unit, the method adopted by the present invention is that the method for agglomerating EPDM rubber liquid by the present invention utilizes the principles of steam distillation and wet degassing, adopts a multi-reactor agglomeration production process with full countercurrent of gas and liquid phases and unequal pressure and temperature, and sends a variety of dispersants, water and EPDM rubber liquid into the agglomerators of three series-connected agglomeration reactors according to a set method for agglomeration to obtain EPDM water colloid particles; the agglomeration conditions in the three agglomeration reactors are controlled to ensure that the colloid particles will not agglomerate again under the premise that most of the hexane can be separated. The method produces uniform colloid particles, stable water content of colloid particles, low volatile content, low water content of recovered solvent, smooth water transportation of colloid particles, no agglomeration and agglomeration phenomenon in the agglomeration equipment, and stable continuous operation.

[0027] (2) The method of the present invention optimizes the condensation process conditions such as the condensation temperature and the operating pressure that matches it, so that the operating state approaches the gas-liquid equilibrium state, and the steam consumption is greatly reduced, which is conducive to further reducing energy consumption.

[0028] (3) In order to solve the difficulty of how to control the size of the rubber particles after coagulation and facilitate the subsequent transportation of the unit rubber particles, the method of the present invention changes the order and method of adding the dispersant and the rubber solution in the ethylene-propylene rubber solution coagulation process, mixes the dispersant, desalted water and the rubber solution in advance, and then sprays them into the first coagulation kettle after preheating. Controlling the ratio of the dispersant, hot desalted water and the rubber solution can accurately and effectively control the particle size of the rubber particles, thereby facilitating the subsequent transportation of the unit rubber particles. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] Figure 1 It is a process flow chart of the method for condensation and devolatilization of ethylene-propylene rubber solution of the present invention;

[0030] Figure 2 is a photograph of the initial state of the glue solution in Example 1 of the present invention;

[0031] Figure 3 This is a photo of the state inside the 1# condensation reactor in an embodiment of the present invention;

[0032] Figure 4 is a photograph of the state inside the colloidal particle filter in Example 1 of the present invention;

[0033] Figure 5 This is a photograph of the state of the colloidal particles (particle size 5mm-10mm) in the 3# coagulation reactor in Example 1 of the present invention;

[0034] In the figure, 1. 1# coagulation kettle, 2. 2# coagulation kettle, 3. 3# coagulation kettle, 4. first colloid particle water pump, 5. colloid particle filter, 6. second colloid particle water pump, 7. third colloid particle water pump, 8. first grinding pump, 9. second grinding pump, 10. first glue-water separator, 11. second glue-water separator, 12. agitator, 13. temperature controller, 14. glue liquid injector, 15. distributor, 15-1. annular water distribution pipe, 15-2. nozzle, 16. exhaust pipe. DETAILED DESCRIPTION

[0035] The present invention is described in detail below with reference to the accompanying drawings and specific embodiments.

[0036] The present invention provides a condensation and devolatilization system for ethylene-propylene rubber liquid, such as Figure 1 As shown, it includes a temperature controller 13, a glue liquid injector 14, a 1# condensation kettle 1, a 2# condensation kettle 2 and a 3# condensation kettle 3 connected in sequence, a first glue particle water pump 4 and a glue particle filter 5 are arranged on the pipeline connecting the 1# condensation kettle 1 and the 2# condensation kettle 2, the glue particle filter 5 is arranged at the outlet of the first glue particle water pump 4, and the glue particle filter 5 is also connected to the top of the 1# condensation kettle 1 through a pipeline; a first grinding pump 8 is arranged on the pipeline connecting the 2# condensation kettle 2 and the 3# condensation kettle 3, and a second grinding pump 9 is arranged on the discharge pipeline of the 3# condensation kettle 3; it also includes a second glue particle water pump 6 and a third glue particle water pump 7, the second glue particle water pump 6 is connected to the top and bottom of the 2# condensation kettle 2 through a pipeline respectively, and the third glue particle water pump 7 is connected to the top and bottom of the 3# condensation kettle 3 through a pipeline respectively; the bottom walls of the 1# condensation kettle 1, the 2# condensation kettle 2 and the 3# condensation kettle 3 are all connected to the low-pressure steam pipeline.

[0037] An exhaust pipe 16 is provided on the top of the 1# condensation kettle 1, which is used to discharge the solvent hexane in the EPDM rubber solution after vaporization; a stirrer 12 is provided inside the 1# condensation kettle 1, the 2# condensation kettle 2 and the 3# condensation kettle 3, and the paddle-type consistent stirrer of the stirrer 12 inside the 1# condensation kettle 1, the 2# condensation kettle 2 and the 3# condensation kettle 3 includes three layers of blades, specifically: the top layer blades are downward pressure paddle type, the middle layer and the lower layer blades are flat push paddles, and an annular distributor is also provided inside the 1# condensation kettle 1, which is located above the liquid surface of the condensation kettle, and the reflux rubber particle water is distributed by the distributor.

[0038] The distributor 15 includes an annular water distribution pipe 15-1, which is provided with a plurality of spray nozzles 15-2. The plurality of nozzles 15-2 can effectively prevent the colloid particles from agglomerating on the liquid surface and also have a defoaming effect.

[0039] A first glue-water separator 10 is provided on the pipeline connecting the second glue water pump 6 with the top wall of the 2# coagulation kettle 2, and the first glue-water separator 10 is also connected with the collecting tank through a pipeline;

[0040] A second glue-water separator 11 is arranged on the pipeline connecting the third glue water pump 7 with the top wall of the 3# coagulation kettle 3, and the second glue-water separator 11 is also connected with the collecting tank through the pipeline.

[0041] The outlet of the colloid water pump-1 is provided with an inclined filter, and a cap is provided above the filter screen, which can effectively reduce the possibility of colloid particles blocking the filter screen. The filter screen used by the colloid filter 5 is V-shaped.

[0042] The present invention also provides a method for condensation devolatilization of ethylene-propylene rubber solution, using the condensation devolatilization system of ethylene-propylene rubber solution, comprising the following steps:

[0043] Step 1: After starting, dispersant 1# is continuously added to 1# condensation kettle 1, 2# condensation kettle 2 and 3# condensation kettle 3, dispersant 2# is mixed with hot desalted water and enters temperature controller 13 for heating, and after heating, dispersant 3# and EPDM rubber glue enter glue liquid injector 14 together, and glue liquid injector 14 is passed with medium-pressure steam, and the mixed liquid is heated and pressurized by the medium-pressure steam;

[0044] Step 1 is specifically as follows: after starting, dispersant 1# is continuously added to 1# condensation kettle 1, 2# condensation kettle 2 and 3# condensation kettle 3. Dispersant 2# and hot desalted water are directly provided by the boundary area, that is, desalted water with a temperature of 90±1°C is mixed in proportion and enters the temperature controller 13 for heating. The operating temperature is 85°C-87°C and the pressure is 0.07MPa-0.08MPa. After the heating is completed, it enters the glue liquid injector 14 together with dispersant 3# and EPDM rubber glue. Medium-pressure steam is passed through the glue liquid injector 14. The mixed liquid is heated and pressurized by the medium-pressure steam. The operating temperature is 88°C-90°C and the pressure is 0.3MPa-0.4MPa.

[0045] In step 1, dispersant 1# is an aqueous solution of polycarboxylate with a concentration of 50 g / L;

[0046] Polycarboxylate (Polyoxyethylene-polyoxypropylene ethercarboxylic acid, referred to as APEG) is a nonionic surfactant. This compound has the following characteristics:

[0047] (1) APEG molecules contain both hydrophilic and hydrophobic groups and have good dispersibility and emulsification properties.

[0048] (2) APEG has a complex molecular structure and can adjust its affinity and hydrophobicity. When used in combination with different hydrophobic surfactants, it can produce a synergistic effect.

[0049] (3) The length of the oxyethylene and oxypropylene groups in the APEG molecule can be adjusted. ) It is used as an emulsifier. After the dispersant 1# condensation is started, it is continuously added to the 1#, 2#, and 3# condensation kettles;

[0050] Dispersant 2# is a 50g / L calcium chloride aqueous solution, which plays a dispersing role;

[0051] Dispersant 3# is an aqueous solution of the preparation agent with a concentration of 50g / L. Its main functions are to prevent the colloid particles from agglomerating and to prevent the rubber from forming a wall, which is beneficial to the transportation of the colloid particles.

[0052] The prepared agent is composed of the following raw materials: surfactant, talcum powder, defoamer, zinc stearate and sodium hydroxide; wherein the mass ratio of surfactant, talcum powder, defoamer and zinc stearate is 0.5-0.6:25-30:1.5-2.0:6.5-7.0, and the amount of sodium hydroxide is to adjust the pH value of dispersant 3# to 9-10;

[0053] The hot desalted water is directly provided by the boundary area, i.e., desalted water with a temperature of 90±1°C; the volume ratio of the hot desalted water and dispersant 2# is: hot desalted water: glue solution = 1-2:10;

[0054] The mass concentration of the dispersant in the condensation kettle (the concentration here is the total concentration of the solution, and the amount of all reagents added must be considered when calculating); the mass ratios of the three dispersants to the condensation water in the 1# condensation kettle 1 are: dispersant 1#: condensation water = 1~2:500, dispersant 2#: condensation water = 1~2:500, dispersant 3#: condensation water = 1~4:4400; where the condensation water comes from: the desalted water contained in the solutions of dispersant 1#, dispersant 2#, and dispersant 3#, the added hot desalted water, the amount of medium-pressure steam used at the glue liquid injector 14, and the amount of low-pressure steam introduced into the bottom of the three condensation kettles to maintain the kettle temperature;

[0055] #The volume ratio of condensed water to EPDM glue in the condensation kettle 1 is 1.0-2:1 (the specific ratio is determined by the solid content of the glue).

[0056] The composition of the glue liquid is solvent hexane, rubber dissolved in the solvent and a small amount of olefin dissolved in the solvent, and the solid content of the glue liquid is 5%-10%;

[0057] Step 2: The mixed solution obtained in step 1 after the temperature and pressure are raised is subjected to condensation and devolatilization treatment.

[0058] Step 2 is specifically as follows: the mixed liquid after temperature and pressure increase obtained in step 1 is sprayed into the bottom of the 1# condensation kettle 1, the operating temperature of the 1# condensation kettle is 85℃-95℃, and the pressure is 0.05MPa-0.10MPa; finally, uniform particles are formed in the 1# condensation kettle 1, the solvent hexane in the EPDM rubber solution is vaporized and discharged from the top of the 1# condensation kettle, and the particles and particles water are recycled after condensation and enter the first particle water pump 4, and then separated by the particle filter 5, and part of the separated particles water is refluxed from the top of the 1# condensation kettle 1 to the 1# condensation kettle 1. The reflux particles water is sprayed to the liquid surface of the 1# condensation kettle by the distributor 15, which effectively prevents the particles from agglomerating and sticking to the wall at the liquid surface, and the remaining particles water transports the particles into the 2# condensation kettle 2, and the operating temperature of the 2# condensation kettle is 95℃-105℃ , the pressure is 0.05MPa-0.08MPa; after the second desolventization of the colloid particles in the 2# condensation kettle, they enter the first grinding pump 8 together with the colloid water. After the grinding action of the first grinding pump 8, the particle size range of the colloid particles is narrowed and the solvent wrapped in the colloid particles is released. The ground colloid particles and the colloid water enter the 3# condensation kettle 3 together. The operating temperature of the 3# condensation kettle is 95℃-100℃, and the pressure is 0.05MPa-0.08MPa, and the third desolventization is carried out; after three desolventizations, most of the solvent is removed, and then the colloid particles and the colloid water enter the second grinding pump 9 together. The main purpose of the second grinding is to make the particle size of the colloid particles uniform, which is convenient for subsequent processing. The ground colloid particles and the colloid water are sent to the rolling screen together for post-processing. The three condensation kettles are maintained at a temperature in the kettle by low-pressure steam at the bottom of the kettle. The non-condensable steam at the top of the kettle is mainly solvent hexane and water vapor. After condensation, hexane and water are separated and reused after separation.

[0059] The coagulator of the present invention is a device including three series-connected coagulation kettles. In the method for coagulation of ethylene-propylene rubber glue liquid of the present invention, dispersant 2#, dispersant 3#, hot desalted water and glue liquid are mixed in advance, and then sprayed into 1# coagulation kettle 1 after preheating. Controlling the ratio of dispersant, hot desalted water and glue liquid can accurately and effectively control the particle size of glue particles. Before being sprayed into 1# coagulation kettle 1, the glue liquid is mixed with dispersant and hot desalted water, which is conducive to forming particles in the coagulation kettle. The dispersant effectively prevents adhesion between the glue particles. The preheating and heating with medium-pressure steam make the mixed liquid have vaporization conditions at the nozzle. When the liquid is sprayed into the 1# condensation kettle, the solvent can be quickly volatilized to form rubber particles. Here, the temperature of the mixed liquid at the nozzle should be controlled. If the temperature of the mixed liquid is too low, the solvent cannot be quickly vaporized, so that the rubber particles are in a state of solid rubber wrapped in rubber liquid. After stirring or collision with the kettle wall, the wrapping layer breaks, causing the rubber liquid to flow out and form large pieces of adhesion. If the temperature of the mixed liquid is too high, after being sprayed into the 1# condensation kettle 1, the solvent inside the rubber particles absorbs enough heat and will quickly vaporize, causing the rubber particles to burst, forming fine rubber particles or rubber powder, which may cause a large amount of fine powder to be entrained in the non-condensable steam, and also cause the rubber particles and the rubber water to be unable to be separated, seriously affecting the subsequent treatment. In the method of ethylene-propylene rubber glue liquid coagulation, due to the small density of ethylene-propylene rubber, the water-gel mixture in the condensation kettle belongs to a highly self-suspended particle system. In order to prevent adhesion or wall hanging at the liquid surface of the 1# condensation kettle, the top paddle of the first condensation kettle adopts a downward pressure paddle type; the reflux rubber water is distributed by a distributor to flush the liquid surface. Since the flow direction of the rubber particles is from bottom to top, the middle and lower paddles are flat push paddles, which are used to quickly disperse the initial rubber particles formed by the rubber liquid sprayed out of the nozzle. The rubber particle filter at the outlet of the first rubber particle water pump 4 has a V-shaped filter screen, and the rubber particle water outlet is located at the bottom of the V-shaped filter screen. Since the density of EPDM is less than the density of water, the rubber particles will float to the top of the V-shaped filter screen and be sent to the 2# condensation kettle 2 by the rubber particle water, which effectively prevents the rubber particles from clogging the filter screen. Since the rubber particles will float in the condensation kettle, the inlets of the second rubber particle water pump 6 and the third rubber particle water pump 7 of the 2# condensation kettle 2 and the 3# condensation kettle 3 are respectively located at the bottom of the 2# condensation kettle 2 and the 3# condensation kettle 3, which can effectively reduce the rubber particles from entering the second rubber particle water pump 6 and the third rubber particle water pump 7. The main function of the first grinding pump 8 is to grind the large-size rubber particles into small-size particles, release the solvent wrapped in the rubber particles, and remove them; the main function of the second grinding pump 9 is to grind the rubber particles into rubber particles with uniform particle size, which is conducive to the transportation and subsequent treatment of the rubber particles. The paddle type of the agitator of the 2# and 3# coagulation kettles is the same as that of the 1# coagulation kettle. The three coagulation kettles all maintain the temperature in the kettle by introducing low-pressure steam into the kettle. The steam introduced into the coagulation kettle eventually turns into condensed water. The coagulation kettle needs to control the liquid level to be stable. The condensed water exceeding the control liquid level is separated by the first glue-water separator 10 and the second glue-water separator 11. The condensed water is discharged from the bottom of the separator to the separation water collection tank. The colloid-containing water in the 2# and 3# coagulation kettles flows back to the corresponding coagulation kettles from the top of the corresponding glue-water separators.

[0060] Example 1

[0061] The system of the present invention is used in a pilot coagulation unit, the coagulation kettle volume is 500L, three kettles are used for coagulation, the nozzle aperture of the 1# coagulation kettle is 3mm, the operating temperature is 90±2°C, the operating pressure is 50kpa, the amount of glue added is 80L / h-100L / h, the solid content of the glue is 9%, the amount of hot desalted water added is 8L / h, the 1# dispersant and the 2# dispersant are both 1.0L / h, i.e. 50g / h, the 3# dispersant is 2L / h, i.e. 100g / h, (the operating conditions of the 2# and 3# coagulation kettles are consistent, the operating temperature is 95±5°C, the operating pressure is 50kpa, the 1# dispersant is 1.0L / h, i.e. 50g / h), the three kettles can operate continuously for up to 720h, the cumulative operation is more than 1500h, and the glue is treated for more than 150m 3 The colloid particles obtained in the experimental coagulation test are uniform, the water content of the colloid particles is 35±2%, the volatile matter is less than 1%, and the water content of the recovered n-hexane is 80-100ppm;

[0062] The specific process is as follows:

[0063] The method for condensation devolatilization of ethylene-propylene rubber liquid uses the above-mentioned condensation devolatilization system of ethylene-propylene rubber liquid, comprising the following steps:

[0064] Step 1: After starting, dispersant 1# (1.0L / h, i.e., 50g / h) is continuously added to 1# condensation kettle 1, 2# condensation kettle 2, and 3# condensation kettle 3. Dispersant 2# (1.0L / h, i.e., 50g / h) and hot desalted water (8L / h) are mixed and enter the temperature controller 13 to be heated to 85-87°C. After the heating is completed, it enters the glue liquid injector 14 together with dispersant 3# (2L / h, i.e., 100g / h) and EPDM glue liquid (80L / h). The glue liquid injector 14 is connected with medium-pressure steam, and the mixed liquid is heated and pressurized by the medium-pressure steam (the operating temperature is 88°C-90°C, and the pressure is 0.3MPa-0.4MPa);

[0065] Step 1 is specifically as follows: after starting, dispersant 1# is continuously added to 1# condensation kettle 1, 2# condensation kettle 2 and 3# condensation kettle 3. Dispersant 2# and hot desalted water are directly provided by the boundary area, that is, desalted water with a temperature of 90±1°C is mixed in proportion and enters the temperature controller 13 for heating. The operating temperature is 85°C-87°C and the pressure is 0.07MPa-0.08MPa. After the heating is completed, it enters the glue liquid injector 14 together with dispersant 3# and EPDM rubber glue. Medium-pressure steam is passed through the glue liquid injector 14. The mixed liquid is heated and pressurized by the medium-pressure steam. The operating temperature is 88°C-90°C and the pressure is 0.3MPa-0.4MPa.

[0066] In step 1, dispersant 1# is an aqueous solution of polycarboxylate with a concentration of 50 g / L;

[0067] Dispersant 2# is a 50g / L calcium chloride aqueous solution, which plays a dispersing role;

[0068] Dispersant 3# is a 50g / L aqueous solution of the preparation agent. Its main function is to prevent the agglomeration of the rubber particles and the wall formation of the rubber material, which is conducive to the transportation of the rubber particles. The preparation agent is composed of the following raw materials: surfactant, talcum powder, defoamer, zinc stearate and sodium hydroxide; among which, the mass ratio of surfactant, talcum powder, defoamer and zinc stearate is 0.5:25:1.5:6.5, and the amount of sodium hydroxide is to adjust the pH value of dispersant 3# to 9-10;

[0069] The hot desalted water is directly provided by the boundary area, i.e., desalted water with a temperature of 90±1°C; the volume ratio of the hot desalted water and dispersant 2# is: hot desalted water: glue solution = 1:10;

[0070] The mass ratios of the three dispersants to the condensed water in the 1# condensation kettle 1 are as follows: dispersant 1#: condensed water = 1:500, dispersant 2#: condensed water = 1:500, dispersant 3#: condensed water = 1:250; the condensed water comes from: the desalted water contained in the dispersant 1#, dispersant 2#, and dispersant 3# solutions, the added hot desalted water, the amount of medium-pressure steam used at the glue liquid ejector 14, and the amount of low-pressure steam introduced into the bottom of the three condensation kettles to maintain the kettle temperature; the solid content of the glue liquid is 9%;

[0071] Step 2: The mixed solution obtained in step 1 after the temperature and pressure are raised is subjected to condensation and devolatilization treatment.

[0072] Step 2 is specifically as follows: the mixed liquid after temperature and pressure increase obtained in step 1 is sprayed into the bottom of the 1# condensation kettle 1, the operating temperature of the 1# condensation kettle is 85℃-95℃, and the pressure is 0.05MPa-0.10MPa; finally, uniform particles are formed in the 1# condensation kettle 1, the solvent hexane in the EPDM rubber solution is vaporized and discharged from the top of the 1# condensation kettle, and the particles and particles water are recycled after condensation and enter the first particle water pump 4, and then separated by the particle filter 5, and part of the separated particles water is refluxed from the top of the 1# condensation kettle 1 to the 1# condensation kettle 1. The reflux particles water is sprayed to the liquid surface of the 1# condensation kettle by the distributor 15, which effectively prevents the particles from agglomerating and sticking to the wall at the liquid surface, and the remaining particles water transports the particles into the 2# condensation kettle 2, and the operating temperature of the 2# condensation kettle is 95℃-105℃ , the pressure is 0.05MPa-0.08MPa; after the second desolventization of the colloid particles in the 2# condensation kettle, they enter the first grinding pump 8 together with the colloid water. After the grinding action of the first grinding pump 8, the particle size range of the colloid particles is narrowed and the solvent wrapped in the colloid particles is released. The ground colloid particles and the colloid water enter the 3# condensation kettle 3 together. The operating temperature of the 3# condensation kettle is 95℃-100℃, and the pressure is 0.05MPa-0.08MPa, and the third desolventization is carried out; after three desolventizations, most of the solvent is removed, and then the colloid particles and the colloid water enter the second grinding pump 9 together. The main purpose of the second grinding is to make the particle size of the colloid particles uniform, which is convenient for subsequent processing. The ground colloid particles and the colloid water are sent to the rolling screen together for post-processing. The three condensation kettles are maintained at a temperature in the kettle by low-pressure steam at the bottom of the kettle. The non-condensable steam at the top of the kettle is mainly solvent hexane and water vapor. After condensation, hexane and water are separated and reused after separation.

[0073] from Figure 2 It can be seen that in the initial state of the rubber liquid, the rubber is completely dissolved in the solvent hexane, the viscosity is 500-600cp, the solid content of the rubber liquid is 9%, and the color of the rubber liquid is light red because it contains trace amounts of catalysts. After coagulation, the catalyst is washed away with water, and the rubber particles are white.

[0074] from Figure 3 It can be seen that in the running state, the particles in the 1# condensation kettle 1 are evenly distributed without agglomeration or wall adhesion, there are only a few bubbles on the liquid surface, no large amount of foaming, no glue sticking to the stirring shaft, and the overall operation is normal and stable. Because more than 93% of the solvent hexane is separated in the 1# condensation kettle, the stable operation of the 1# condensation kettle 1 is the key to the condensation system.

[0075] from Figure 4 It can be seen that inside the filter at the outlet of the first colloid water pump 4, the particle size of the separated colloid particles is uniform and meets the requirements, and there is no clogging of the filter screen.

[0076] from Figure 5It can be seen that the sampling of the colloid particles at the outlet of 3# condensation reactor 3 shows that the particle size distribution of the colloid particles is uniform and meets the requirements, the colloid particles are white, the catalyst water washing effect is significant, and the volatile matter content and water content of the colloid particles meet the process requirements.

[0077] Example 2

[0078] Other conditions are consistent with those in Example 1. When the outlet pressure of the first colloid pump 4 is 0.15 MPa and the aperture of the nozzle of the 1# condensation kettle is 2 mm, the particle size of the condensed colloid particles is 3-6 mm.

[0079] Example 3

[0080] Other conditions are consistent with those in Example 2. When the nozzle aperture of the 1# coagulation reactor is 3 mm, the particle size of the coagulated colloid particles is 5-8 mm.

[0081] Example 4

[0082] The other conditions are consistent with those in Example 2. When the nozzle aperture of the 1# coagulation reactor is 5 mm, the particle size of the coagulated colloid particles is 10-14 mm.

[0083] Example 5

[0084] The other conditions are the same as those in Example 1, except that the prepared agent is composed of the following raw materials: surfactant, talcum powder, defoamer, zinc stearate and sodium hydroxide; wherein the mass ratio of surfactant, talcum powder, defoamer and zinc stearate is 0.6:30:2.0:7.0, and the amount of sodium hydroxide is to adjust the pH value of dispersant 3# to 10;

[0085] The volume ratio of hot desalted water and dispersant 2# is: hot desalted water: glue solution = 2:10;

[0086] The mass ratios of the three dispersants to the condensed water in the 1# condensation kettle are: dispersant 1#: condensed water = 2:500, dispersant 2#: condensed water = 2:500, dispersant 3#: condensed water = 4:4400;

[0087] The solid content of the glue is 5%.

[0088] Example 6

[0089] The other conditions are the same as those in Example 1, except that the prepared agent is composed of the following raw materials: surfactant, talcum powder, defoamer, zinc stearate and sodium hydroxide; wherein the mass ratio of surfactant, talcum powder, defoamer and zinc stearate is 0.55:26:1.6:6.6, and the amount of sodium hydroxide is to adjust the pH value of dispersant 3# to 9.5;

[0090] The volume ratio of hot desalted water and dispersant 2# is: hot desalted water: glue solution = 1.5:10;

[0091] The mass ratios of the three dispersants to the condensed water in the 1# condensation kettle are: dispersant 1#: condensed water = 1.5:500, dispersant 2#: condensed water = 1.5:500, dispersant 3#: condensed water = 2:4400;

[0092] The solid content of the glue is 10%.

Claims

1. Ethylene propylene rubber liquid coagulation and devolatilization system, characterized in that: The invention comprises a temperature controller (13), a glue liquid ejector (14), a 1# condensation kettle (1), a 2# condensation kettle (2) and a 3# condensation kettle (3) which are connected in sequence. A first colloid water pump (4) and a colloid filter (5) are provided on the pipeline connecting the 1# condensation kettle (1) and the 2# condensation kettle (2). The colloid filter (5) is provided at the outlet of the first colloid water pump (4). The colloid filter (5) is also connected to the top wall of the 1# condensation kettle (1) through the pipeline. The pipeline connecting the 2# condensation kettle (2) and the 3# condensation kettle (3) is provided. A first grinding pump (8) is provided on the pipeline between the first and second condensation kettles (1), and a second grinding pump (9) is provided on the discharge pipeline of the third condensation kettle (3); a second colloid water pump (6) and a third colloid water pump (7) are also provided, the second colloid water pump (6) being connected to the top and bottom of the second condensation kettle (2) through pipelines, and the third colloid water pump (7) being connected to the top and bottom of the third condensation kettle (3) through pipelines; the bottom walls of the first condensation kettle (1), the second condensation kettle (2) and the third condensation kettle (3) are all connected to the low-pressure steam pipeline.

2. The ethylene propylene rubber solution coagulation and devolatilization system according to claim 1, characterized in that: The top of the No. 1 condensation kettle (1) is provided with an exhaust pipe (16); the interiors of the No. 1 condensation kettle (1), the No. 2 condensation kettle (2) and the No. 3 condensation kettle (3) are all provided with agitators (12), and the paddle types of the agitators (12) inside the No. 1 condensation kettle (1), the No. 2 condensation kettle (2) and the No. 3 condensation kettle (3) are consistent; the agitators include three layers of blades, specifically: the top layer blades are downward pressure blades, the middle layer and the lower layer blades are flat push blades, and an annular distributor is also provided inside the No. 1 condensation kettle (1).

3. The ethylene propylene rubber solution coagulation and devolatilization system according to claim 2, characterized in that: The distributor (15) comprises an annular water distribution pipe (15-1), which is provided with a plurality of spray nozzles (15-2).

4. The ethylene propylene rubber solution coagulation and devolatilization system according to claim 3, characterized in that: A first glue-water separator (10) is provided on the pipeline connecting the second glue water pump (6) and the top wall of the second condensation kettle (2), and the first glue-water separator (10) is also connected to the collection tank through a pipeline; A second glue-water separator (11) is provided on the pipeline connecting the third glue water pump (7) and the top wall of the 3# coagulation kettle (3), and the second glue-water separator (11) is also connected to the collecting tank through a pipeline.

5. The ethylene propylene rubber solution coagulation and devolatilization system according to claim 4, characterized in that: The filter screen used by the colloidal filter (5) is V-shaped.

6. A method for condensation devolatilization of ethylene propylene rubber solution, using the system as claimed in claim 5, characterized in that: The following steps are involved: Step 1: After the start-up, dispersant 1# is continuously added to the 1# condensation kettle (1), the 2# condensation kettle (2) and the 3# condensation kettle (3). Dispersant 2# is mixed with hot desalted water and then enters the temperature controller (13) for heating. After the heating is completed, it enters the glue liquid injector (14) together with dispersant 3# and EPDM glue liquid. The glue liquid injector (14) is passed through medium-pressure steam, and the mixed liquid is heated and pressurized by the medium-pressure steam. Step 2: The mixed solution obtained in step 1 after heating and pressurizing is subjected to condensation and devolatilization treatment to finally obtain EPDM rubber hydrocolloid particles.

7. The method for coagulation devolatilization of EPDM rubber according to claim 6, characterized in that: Step 1 is specifically as follows: after starting, dispersant 1# is continuously added to 1# condensation kettle (1), 2# condensation kettle (2) and 3# condensation kettle (3); dispersant 2# is mixed with hot desalted water and then enters the temperature controller (13) for heating, with the operating temperature being 85°C-87°C and the pressure being 0.07MPa-0.08MPa; after the heating is completed, it enters the glue liquid injector (14) together with dispersant 3# and EPDM glue liquid, and the glue liquid injector (14) is passed with medium-pressure steam. The mixed liquid is heated and pressurized by the medium-pressure steam, with the operating temperature being 88°C-90°C and the pressure being 0.3MPa-0.4MPa.

8. The method for coagulation devolatilization of EPDM rubber solution according to claim 6, characterized in that: In step 1, dispersant 1# is an aqueous solution of polycarboxylate with a concentration of 50 g / L; dispersant 2# is an aqueous solution of calcium chloride with a concentration of 50 g / L; dispersant 3# is an aqueous solution of a preparation agent with a concentration of 50 g / L, and the preparation agent is composed of the following raw materials: surfactant, talc, defoamer, zinc stearate and sodium hydroxide; wherein the mass ratio of surfactant, talc, defoamer and zinc stearate is 0.5-0.6:25-30:1.5-2.0:6.5-7.0, and the amount of sodium hydroxide is to adjust the pH value of dispersant 3# to 9-10; The volume ratio of hot desalted water and dispersant 2# is: hot desalted water: glue solution = 1-2:10; The mass ratios of the three dispersants to the condensed water in the 1# condensation kettle (1) are as follows: dispersant 1#: condensed water = 1-2:500, dispersant 2#: condensed water = 1-2:500, dispersant 3#: condensed water = 1-4:4400; #The volume ratio of condensed water to EPDM rubber solution in the condensation kettle (1) is 1.0-2:

1.

9. The method for coagulation devolatilization of EPDM rubber according to claim 6, characterized in that: Step 2 is specifically as follows: the mixed liquid obtained in step 1 after being heated and pressurized is sprayed into the bottom of the 1# coagulation kettle (1), the operating temperature of the 1# coagulation kettle is 85℃-95℃, and the pressure is 0.05MPa-0.10MPa; finally, uniform particles are formed in the 1# coagulation kettle (1), the solvent hexane in the EPDM rubber solution is vaporized and discharged from the top of the 1# coagulation kettle, and the particles and particle water are recycled after condensation and enter the first particle water pump (4), and then separated by the particle filter (5), part of the particle water is refluxed from the top of the 1# coagulation kettle (1) to the 1# coagulation kettle (1), and the remaining particle water transports the particles into the 2# coagulation kettle (2), and the 2# The operating temperature of the coagulation kettle is 95°C-105°C and the pressure is 0.05MPa-0.08MPa; after the second desolvation of the colloid particles in the 2# coagulation kettle, the colloid particles enter the first grinding pump (8) together with the colloid water. After the colloid particles are ground by the first grinding pump (8), the ground colloid particles and the colloid water enter the 3# coagulation kettle (3). The operating temperature of the 3# coagulation kettle is 95°C-100°C and the pressure is 0.05MPa-0.08MPa, and the third desolvation is carried out; then the colloid particles and the colloid water enter the second grinding pump (9) together, and the ground colloid particles and the colloid water are sent to the roller screen together for post-processing.