Magnesium oxide carbon dioxide adsorbent as well as preparation method and application thereof
Octagonal magnesium oxide powder was prepared through hydrothermal reaction, exposing strong alkaline sites, solving the problem of insufficient adsorption of magnesium oxide, achieving efficient CO2 adsorption effect, and simplifying the process.
Patent Information
- Application Number
- CN202411268719.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-11
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2044-09-11
AI Technical Summary
During the CO2 adsorption process, magnesium oxide has insufficient alkaline sites on the surface, resulting in the actual adsorption amount not reaching the theoretical value. The existing modification methods are costly and complex in the process.
Embroidered spherical powder formed by octagonal magnesium oxide stack is prepared by hydrothermal reaction, exposing the (111) crystal surface, increasing the strong alkaline sites on the surface, simplifying the calcination process, and improving the CO2 adsorption capacity.
The adsorption amount of magnesium oxide to CO2 is significantly increased, reaching 4 times that of commercial magnesium oxide, and the process is simple and the cost is low.
Smart Images

Figure CN119075901A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of adsorption materials, and in particular to a magnesium oxide carbon dioxide adsorbent and a preparation method and application thereof. Background Art
[0002] CO2 adsorption is crucial to reducing greenhouse gas emissions and addressing climate change. At present, common CO2 adsorption methods include: chemical adsorption using adsorbents such as alkali metal carbonates or amine compounds to react with carbon dioxide; using adsorbents such as activated carbon, metal oxides and metal-organic framework materials to adsorb CO2 through physical or chemical interactions; using organisms such as microorganisms or plants to absorb and fix CO2 through their metabolic processes. Among them, the method of using adsorbents to adsorb CO2 has the characteristics of low energy consumption and simple operation, and can quickly adsorb and desorb CO2, which can achieve high-efficiency and low-cost CO2 separation, and has attracted much attention.
[0003] Magnesium oxide can react chemically with CO2, so that CO2 molecules are embedded in the crystal structure of magnesium oxide, thereby achieving CO2 adsorption. Compared with other metal oxides, magnesium oxide is abundant in resources, has a theoretical adsorption capacity of up to 1100 mg CO2 / g adsorbent, requires less energy during regeneration, is low in cost, is non-toxic, and can effectively adsorb CO2 in the room temperature to medium temperature range. Therefore, it is used to adsorb CO2. However, due to the insufficient alkaline sites on the surface of magnesium oxide or the low quality, the contact and diffusion of CO2 molecules are limited, resulting in the actual value of magnesium oxide adsorbing CO2 failing to reach the theoretical value. In order to increase the actual adsorption amount of magnesium oxide for attached CO2, researchers have improved the CO2 adsorption capacity by adding modifiers such as molten salts. For example, using molten salts (such as NaNO3) to form NO on the surface of magnesium oxide, the adsorption of CO2 by magnesium oxide can be improved. 2+ , provides O 2- This process increases the number of basic sites on the surface of magnesium oxide; moreover, the molten salt changes the original reaction path of magnesium oxide and CO2, and promotes the formation of oxygen defects by grabbing the lattice oxygen on the surface of magnesium oxide. 2- The rapid formation of magnesium oxide enhances the basic sites on the surface of magnesium oxide. Another example is the method of amino functionalization of magnesium oxide to improve its CO2 capture ability. Amino groups have strong alkalinity and can form stable chemical bonds with CO2. By introducing amino groups on the surface of magnesium oxide, the number of basic sites on the surface can be increased, the selectivity and adsorption efficiency of the adsorbent can be improved, and CO2 molecules can be more easily captured.
[0004] However, both molten salt-modified and amino-modified magnesium oxide involve high material and production costs, and the preparation process requires complex synthesis methods and precise process control. Otherwise, it is difficult to improve the quantity and quality of magnesium oxide alkaline sites, which leads to a low actual adsorption capacity of CO2 / g by magnesium oxide.
[0005] Therefore, developing a magnesium oxide that can improve the number of basic sites without modification is of great significance for improving the CO2 adsorption capacity of magnesium oxide. Summary of the invention
[0006] The object of the present invention is to provide a magnesium oxide carbon dioxide adsorbent and a preparation method and application thereof. The magnesium oxide carbon dioxide adsorbent provided by the present invention can improve the number of basic sites of magnesium oxide.
[0007] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:
[0008] The invention provides a magnesium oxide carbon dioxide adsorbent. The magnesium oxide carbon dioxide adsorbent is an embroidery ball-shaped powder formed by stacking octagonal pyramid magnesium oxides. The particle size of the embroidery ball-shaped powder is 20-40 μm.
[0009] The present invention also provides a method for preparing the magnesium oxide carbon dioxide adsorbent described in the above technical solution, comprising the following steps:
[0010] (1) mixing a carbon source, a water-soluble magnesium salt, an alkali and water, and performing a hydrothermal reaction to obtain magnesium carbonate;
[0011] (2) calcining the magnesium carbonate obtained in step (1), cooling it to room temperature, and obtaining a magnesium oxide carbon dioxide adsorbent; the cooling rate is 20 to 200° C. / min.
[0012] Preferably, the carbon source in step (1) comprises one or more of ascorbic acid, urea, potassium bicarbonate and sodium bicarbonate.
[0013] Preferably, the water-soluble magnesium salt in step (1) includes one or more of anhydrous magnesium sulfate, anhydrous magnesium chloride and magnesium acetate.
[0014] Preferably, the base in step (1) comprises NaOH and / or KOH.
[0015] Preferably, in step (1), the molar ratio of the carbon element in the carbon source to the magnesium element in the water-soluble magnesium salt is (3-10):1.
[0016] Preferably, the temperature of the hydrothermal reaction in step (1) is 120-200° C.; and the hydrothermal reaction time is 3-10 h.
[0017] Preferably, the calcination temperature in step (2) is 650-900° C. and the calcination time is 1-3 hours.
[0018] Preferably, the heating rate of heating to the calcination temperature in step (2) is 5 to 35° C. / min.
[0019] The present invention also provides the use of the magnesium oxide carbon dioxide adsorbent described in the above technical solution or the magnesium oxide carbon dioxide adsorbent prepared by the preparation method described in the above technical solution as a CO2 adsorbent.
[0020] The present invention provides a magnesium oxide carbon dioxide adsorbent, which is an embroidery ball-shaped powder formed by stacking octagonal pyramidal magnesium oxide, and the particle size of the embroidery ball-shaped powder is 20 to 40 μm. The magnesium oxide carbon dioxide adsorbent provided by the present invention is an embroidery ball-shaped powder formed by stacking octagonal pyramidal magnesium oxide, and the octagonal pyramidal morphology can expose the (111) crystal plane of magnesium oxide, thereby exposing the strong alkaline sites on its surface; and the particle size of the embroidery ball-shaped powder is 20 to 40 μm, with a smaller particle size and a larger specific surface area. Therefore, the magnesium oxide carbon dioxide adsorbent provided by the present invention can expose more alkaline sites, thereby effectively improving the adsorption capacity of magnesium oxide for CO2. The results of the embodiment show that the adsorption amount of CO2 by the magnesium oxide carbon dioxide adsorbent provided by the present invention is 4 times the adsorption amount of CO2 by commercial magnesium oxide. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1 This is a SEM image of anhydrous magnesium carbonate prepared in Example 1 of the present invention;
[0022] Figure 2 This is a SEM image of the magnesium oxide carbon dioxide adsorbent prepared in Example 1 of the present invention;
[0023] Figure 3 TEM image of the magnesium oxide carbon dioxide adsorbent prepared in Example 1 of the present invention;
[0024] Figure 4 The CO2-TPD test result curve of the magnesium oxide carbon dioxide adsorbent prepared in Example 1 of the present invention and commercial magnesium oxide;
[0025] Figure 5 This is a curve of the magnesium oxide carbon dioxide adsorbent prepared in Example 1 of the present invention and commercial magnesium oxide adsorbing 100% CO2 gas at 50°C for 4 hours. DETAILED DESCRIPTION
[0026] The invention provides a magnesium oxide carbon dioxide adsorbent. The magnesium oxide carbon dioxide adsorbent is an embroidery ball-shaped powder formed by stacking octagonal pyramid magnesium oxides. The particle size of the embroidery ball-shaped powder is 20-40 μm.
[0027] In the present invention, the magnesium oxide carbon dioxide adsorbent is an embroidery ball-shaped powder formed by stacking octagonal pyramids of magnesium oxide. The octagonal pyramid morphology can expose the (111) crystal plane of magnesium oxide, thereby exposing the strong alkaline sites on its surface.
[0028] In the present invention, the particle size of the octagonal pyramidal magnesium oxide is preferably 0.3-1 μm, more preferably 0.5-0.8 μm. In the magnesium oxide carbon dioxide adsorbent provided by the present invention, the particle size of the octagonal pyramidal magnesium oxide is within the above range, which can expose more basic sites.
[0029] In the present invention, the particle size of the embroidery ball-shaped powder is 20 to 40 μm, preferably 25 to 35 μm. The embroidery ball-shaped powder of the magnesium oxide carbon dioxide adsorbent provided by the present invention has a smaller particle size and a larger specific surface area. Therefore, the magnesium oxide carbon dioxide adsorbent provided by the present invention can expose more alkaline sites, thereby effectively improving the adsorption capacity and removal rate of magnesium oxide for CO2.
[0030] The present invention also provides a method for preparing the magnesium oxide carbon dioxide adsorbent described in the above technical solution, comprising the following steps:
[0031] (1) mixing a carbon source, a water-soluble magnesium salt, an alkali and water, and performing a hydrothermal reaction to obtain magnesium carbonate;
[0032] (2) calcining the magnesium carbonate obtained in step (1), cooling it to room temperature, and obtaining a magnesium oxide carbon dioxide adsorbent; the cooling rate is 20 to 200° C. / min.
[0033] The invention mixes a carbon source, a water-soluble magnesium salt, an alkali and water, and performs a hydrothermal reaction to obtain magnesium carbonate.
[0034] In the present invention, the carbon source preferably includes one or more of ascorbic acid, urea, potassium bicarbonate and sodium bicarbonate, more preferably ascorbic acid or urea. The present invention utilizes a carbon source to provide CO2, which can combine with hydroxide to form carbonate ions, and carbonate ions combine with magnesium ions in the solution to form magnesium carbonate. The present invention uses the above-mentioned carbon source, which is rich in source and easy to produce CO2.
[0035] In the present invention, the water-soluble magnesium salt preferably includes one or more of anhydrous magnesium sulfate, anhydrous magnesium chloride and magnesium acetate, and more preferably anhydrous magnesium sulfate. The present invention uses a water-soluble magnesium salt to provide magnesium ions to form magnesium carbonate with carbonate ions.
[0036] In the present invention, the molar ratio of the carbon element of the carbon source to the magnesium element of the water-soluble magnesium salt is preferably (3-10): 1, and more preferably (5-8): 1. The present invention controls the molar ratio of the carbon element to the magnesium element within the above range, which can not only fully convert the magnesium salt into magnesium carbonate, but also affect the crystallization process of magnesium carbonate, so that the magnesium carbonate is embroidered ball-shaped magnesium carbonate.
[0037] In the present invention, the base is preferably NaOH and / or KOH. In the present invention, the base is added to provide hydroxide to the reaction system, which is combined with carbon dioxide produced by the carbon source to form carbonate, and then the carbonate reacts with the water-soluble magnesium salt to form magnesium carbonate. In the present invention, the base is preferably alkali solution, and the concentration of the alkali solution is preferably 3 to 10 moL / L, more preferably 5 moL / L.
[0038] The present invention has no special limitation on the amount of the alkali, as long as the pH value of the mixed solution formed by the carbon source, the water-soluble magnesium salt, the alkali and water is 8 to 12.5. The present invention limits the pH value of the above system to the above range, so that the system can be alkaline, which is more conducive to fully converting the carbon dioxide generated by the carbon source into carbonate.
[0039] In the present invention, the water is used as a reaction solvent. The present invention has no particular limitation on the amount of the water, as long as it can fully dissolve the carbon source, the water-soluble magnesium salt and the alkali, and can smoothly carry out the hydrothermal reaction. In one embodiment of the present invention, when the anhydrous magnesium sulfate is 3.6110 g and the ascorbic acid is 7.0448 g, the volume of the water is 30 mL.
[0040] The present invention has no particular limitation on the method for mixing the carbon source, water-soluble magnesium salt, alkali and water. Conventional mixing methods can be used to completely dissolve the carbon source, water-soluble magnesium salt and alkali in water to form a mixed solution.
[0041] In the present invention, the temperature of the hydrothermal reaction is preferably 120-200°C, more preferably 150-180°C; the hydrothermal reaction time is preferably 3-10h, more preferably 3-6h. The present invention has no special limitation on the device for the hydrothermal reaction, and any conventional hydrothermal reaction device can be used. In the present invention, the device for the hydrothermal reaction is preferably a polytetrafluoroethylene-lined reactor. In the present invention, the device for the hydrothermal reaction is preferably placed in a homogeneous reactor for hydrothermal reaction. In the present invention, the homogeneous reactor can promote mass transfer and make each material react evenly. In one embodiment of the present invention, the power of the homogeneous reactor is preferably 5Hz.
[0042] In the present invention, after the hydrothermal reaction, the system after the reaction is preferably cooled to room temperature, and then the solid product obtained by the hydrothermal reaction is washed, filtered and dried in sequence to obtain magnesium carbonate. The present invention has no particular limitation on the operation methods of the washing, filtering and drying, as long as the impurities on the surface of the magnesium carbonate can be fully removed and dried.
[0043] After obtaining magnesium carbonate, the present invention calcines the magnesium carbonate and cools it to room temperature to obtain a magnesium oxide carbon dioxide adsorbent; the cooling rate is 20 to 200° C. / min.
[0044] In the present invention, the calcination temperature is preferably 650-900°C, more preferably 650-800°C; the calcination time is preferably 1-3h, more preferably 2-3h. The present invention performs calcination at the above temperature and time, which can make magnesium carbonate lose weight and generate magnesium oxide and CO2. The present invention has no special limitation on the calcination device, and any conventional calcination device can be used. In one embodiment of the present invention, the calcination device is a muffle furnace.
[0045] The present invention preferably grinds the magnesium carbonate into powder before calcining. The present invention can disperse the agglomerated magnesium carbonate by grinding, which is more conducive to fully converting the magnesium carbonate into magnesium oxide. The present invention does not specifically limit the particle size of the ground magnesium carbonate powder, as long as the agglomerated magnesium carbonate particles can be dispersed.
[0046] In the present invention, the heating rate to the calcination temperature is preferably 5-35°C / min, more preferably 20-25°C / min. In the present invention, heating at the above heating rate is more conducive to the transformation of the morphology of magnesium oxide into an octagonal pyramid.
[0047] In the present invention, the cooling rate is 20-200°C / min, preferably 100-150°C / min. The present invention cools at the above rate, has a faster cooling rate, and can fully expose the (111) crystal plane of magnesium oxide.
[0048] The method provided by the present invention does not require the addition of molten salt or ionic liquid, and is directly calcined in the air. The required equipment is simple and easy to operate. In addition, the present invention greatly exposes the (111) crystal plane of magnesium oxide through a simple calcination method, thereby exposing the strong alkaline sites on its surface, thereby effectively improving the adsorption capacity and removal rate of magnesium oxide for carbon dioxide.
[0049] The present invention also provides the use of the magnesium oxide carbon dioxide adsorbent described in the above technical solution as a CO2 adsorbent.
[0050] The present invention does not specifically limit the application method of the magnesium oxide carbon dioxide adsorbent as a CO2 adsorbent, and a conventional method of adsorbing CO2 by an adsorbent may be used.
[0051] The magnesium oxide carbon dioxide adsorbent provided by the present invention greatly exposes the (111) crystal plane of magnesium oxide and the strong alkaline sites on its surface, so that it can be used as a CO2 adsorbent and effectively improve the adsorption capacity and removal rate of magnesium oxide for carbon dioxide.
[0052] The technical solutions in the present invention will be described clearly and completely below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only a part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0053] Example 1
[0054] A magnesium oxide carbon dioxide adsorbent is an embroidery ball-shaped powder formed by stacking octagonal pyramid magnesium oxides, the particle size of the octagonal pyramid magnesium oxide is 0.5-0.8 μm, and the particle size of the embroidery ball-shaped powder is 30 μm.
[0055] The preparation method of the above-mentioned magnesium oxide carbon dioxide adsorbent is:
[0056] (1) Ascorbic acid is used as a carbon source, anhydrous magnesium sulfate is used as a water-soluble magnesium salt, and a NaOH solution with a concentration of 5 mol / L is used as an alkali solution; wherein the molar ratio of the carbon element of the carbon source to the magnesium element of the water-soluble magnesium salt is 8:1, which is recorded as n(C):n(Mg)=8:1;
[0057] 7.0448 g of carbon source, 3.6110 g of water-soluble magnesium salt and alkali solution were dissolved in 30 mL of water to obtain a mixed solution, the pH value of the mixed solution was 12.5, the mixed solution was placed in a 100 mL polytetrafluoroethylene liner, loaded into a reactor, and then placed in a homogeneous reactor, the frequency of the homogeneous reactor was adjusted to 5 Hz, and the temperature was kept at 180° C. for 3 h for hydrothermal reaction; after the hydrothermal reaction, the system was cooled to room temperature, washed and filtered, and the obtained solid powder was placed in a drying oven for 24 h to obtain anhydrous magnesium carbonate;
[0058] (2) Grinding the anhydrous magnesium carbonate obtained in step (1) into powder and placing it in a boron nitride crucible, calcining it in a muffle furnace, setting the initial temperature to 20°C, heating it to 650°C at a heating rate of 25°C / min, and calcining it for 2h. After the calcination, placing the crucible in cold water and cooling it to room temperature at a cooling rate of 150°C / min to obtain a magnesium oxide carbon dioxide adsorbent.
[0059] Example 2
[0060] A magnesium oxide carbon dioxide adsorbent is an embroidery ball-shaped powder formed by stacking octagonal pyramid magnesium oxides, the particle size of the octagonal pyramid magnesium oxide is 0.3-1 μm, and the particle size of the embroidery ball-shaped powder is 30 μm.
[0061] The preparation method of the above-mentioned magnesium oxide carbon dioxide adsorbent is:
[0062] (1) Ascorbic acid is used as a carbon source, anhydrous magnesium sulfate is used as a water-soluble magnesium salt, and a 5 mol / L NaOH solution is used as an alkali solution; wherein n(C):n(Mg)=8:1;
[0063] 7.0448 g of carbon source, 3.6110 g of water-soluble magnesium salt and alkali solution were dissolved in 30 mL of water to obtain a mixed solution, wherein the pH value of the mixed solution was 12.5; the mixed solution was placed in a 100 mL polytetrafluoroethylene liner, loaded into a reaction kettle, and then placed in a homogeneous reactor, the frequency of the homogeneous reactor was adjusted to 5 Hz, and the temperature was kept at 180° C. for 3 h for hydrothermal reaction; after the hydrothermal reaction, the system was cooled to room temperature, washed, filtered, and the obtained solid powder was placed in a drying oven for 24 h to obtain anhydrous magnesium carbonate;
[0064] (2) Grinding the anhydrous magnesium carbonate obtained in step (1) into powder and placing it in a boron nitride crucible, calcining it in a muffle furnace, setting the initial temperature to 20° C., heating it to 800° C. at a heating rate of 25° C. / min, and calcining it for 2 hours. After the calcination, placing the crucible in cold water and cooling it to room temperature at a cooling rate of 150° C. / min to obtain a magnesium oxide carbon dioxide adsorbent.
[0065] Test Example 1
[0066] The SEM image of anhydrous magnesium carbonate prepared in Example 1 is as follows Figure 1 As shown, Figure 1 The upper right corner is a SEM image at high magnification. Figure 1 It can be seen that the surface of the anhydrous magnesium carbonate prepared in Example 1 is a spherical embroidery ball with an average diameter of about 0.05nm, and the diameter of the embroidery ball powder is about 30μm. This shows that the anhydrous magnesium carbonate prepared in Example 1 is an embroidery ball-shaped magnesium carbonate powder with a particle size of , and combined with the results of multiple SEM images, it can be seen that the particle size of the embroidery ball-shaped magnesium carbonate powder is 20-40μm.
[0067] The SEM image of the magnesium oxide carbon dioxide adsorbent prepared in Example 1 is as follows: Figure 2 As shown, Figure 2 The upper right corner is a SEM image at high magnification. Figure 2It can be seen that the magnesium oxide carbon dioxide adsorbent prepared in Example 1 is an embroidery ball-shaped powder formed by stacking octagonal pyramid magnesium oxide, the particle size of the octagonal pyramid magnesium oxide is about 0.3-1 μm, and the particle size of the embroidery ball-shaped powder is about 20-40 μm.
[0068] The TEM image of the magnesium oxide carbon dioxide adsorbent prepared in Example 1 is as follows: Figure 3 As shown, (a) is the transmission image, (b) is the high-resolution image, and (c) is the selected area electron diffraction pattern (SAED). Figure 3 In which Figure (a) confirms that the magnesium oxide in the magnesium oxide carbon dioxide adsorbent prepared in Example 1 is in an octahedral form. Figure 3 As can be seen from (b) and (c), the quadrilateral outline of the properly arranged isolated particles and the related selected area electron diffraction (SAED) pattern indicate that the (111) crystal plane is exposed on the surface of the magnesium oxide particles. Conventional commercially available magnesium oxide particles often appear as polydispersed aggregates rather than isolated octahedral crystals. This indicates that the magnesium oxide carbon dioxide adsorbent provided by the present invention has a different crystal structure from conventional commercially available magnesium oxide.
[0069] Test Example 2
[0070] In order to verify the distribution of basic sites on the surface of the magnesium oxide carbon dioxide adsorbent prepared in Example 1, the material was tested by temperature-programmed desorption of CO2 (CO2-TPD). The test instrument used was a Micromeritics ChemiSorb 2750 reactor from Micromeritics Instruments. 70 mg of MgO was weighed and stirred at a flow rate of 50 mL min -1 In argon atmosphere, at 10℃·min -1 The flow rate was raised from room temperature to 300 °C and then maintained at this temperature for 2 h to remove impurities adsorbed on the surface. -1 After the temperature was lowered to 50 °C under argon atmosphere, the -1 CO2 was introduced at a flow rate of 1.50 mL / min and maintained for 3.5 h. -1 After purging the sample with argon at a flow rate of 1.5 h, the sample was heated at 10 °C·min -1 The temperature is raised to 850°C at a flow rate of , so that the corresponding CO2 temperature-programmed desorption curve can be obtained.
[0071] Figure 4 The CO2-TPD test result curves of commercial magnesium oxide (Adamas Beta Chemical Reagent Co., Ltd.) and the magnesium oxide carbon dioxide adsorbent prepared in Example 1. Figure 4The characteristic peak at the desorption temperature indicates the basic strength of the adsorbent, and the area under the distribution curve indicates the number of basic sites in the adsorbent. Figure 4 It can be seen that three main peaks appear at temperatures below 200°C, 300-500°C and 700-900°C, respectively, indicating weak alkaline sites, medium alkaline sites and strong alkaline sites of magnesium oxide. However, commercial magnesium oxide only exposes some medium alkaline sites, and their number is much smaller than that of the magnesium oxide carbon dioxide adsorbent prepared in this experiment. This shows that the magnesium oxide carbon dioxide adsorbent provided by the present invention can improve the number of alkaline sites of magnesium oxide.
[0072] Test Example 3
[0073] In order to verify the actual CO2 adsorption capacity of the octahedral MgO adsorbent, the MgO carbon dioxide adsorbent prepared in Example 1 and the commercial MgO carbon dioxide adsorbent were tested using a thermogravimetric analyzer (TGA). The mass change of the MgO adsorbent before and after the introduction of high-purity CO2 gas was calculated, and then the difference was calculated to obtain the saturated CO2 adsorption capacity of the MgO adsorbent material. About 10 mg of the sample was weighed and placed in a 100% high-purity nitrogen gas flow (gas flow rate 20 mL min -1 ) to 600℃ (heating rate is 20℃·min -1 ) and keep it for 1 hour to avoid the influence of moisture and carbon dioxide in the air on the sample. After pretreatment, the temperature was lowered to 150℃ and kept for 1 hour. During the cooling process, high-purity N2 was continuously introduced as a protective gas. After the system was stable, high-purity CO2 gas (gas flow rate 60mL·min -1 ), the adsorption test process was maintained for 4 hours. The CO2 adsorption amount of the adsorbent material is calculated as shown in formula (I):
[0074] CO2 adsorption capacity (mmol·g -1 )=(m t -m0)×1000 / (m0×M (CO2) ) Formula (I)
[0075] In formula (I), m t is the mass of the sample at time t, m0 is the initial mass of the sample before adsorption, M (CO2) is the molar molecular weight of CO2 (44 g·mol -1 ).
[0076] Figure 5 The curves of commercial magnesium oxide (Adamas Beta Chemical Reagent Co., Ltd.) and magnesium oxide carbon dioxide adsorbent prepared in Example 1 adsorbing 100% CO2 gas for 4 hours at 50°C. Figure 5 It can be seen that the CO2 adsorption performance of commercial magnesium oxide is about 0.1mmol g -1The CO2 adsorption performance of the magnesium oxide carbon dioxide adsorbent prepared in this experiment is about 0.4mmol g -1 , which is 4 times that of commercial magnesium oxide.
[0077] It can be seen from the above experimental results that the CO2 adsorption performance of the magnesium oxide carbon dioxide adsorbent prepared by the present invention is much higher than the CO2 adsorption performance of commercial magnesium oxide. This is because the magnesium oxide carbon dioxide adsorbent prepared by the present invention is an embroidery ball-shaped powder formed by stacking octagonal pyramidal magnesium oxide, and has a smaller particle size. The octagonal pyramidal morphology can expose the (111) crystal plane of magnesium oxide, thereby exposing the strong alkaline sites on its surface. Therefore, the magnesium oxide carbon dioxide adsorbent provided by the present invention can expose more alkaline sites, thereby effectively improving the adsorption capacity of magnesium oxide for CO2.
[0078] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A magnesium oxide carbon dioxide adsorbent, wherein the magnesium oxide carbon dioxide adsorbent is an embroidery ball-shaped powder formed by stacking octagonal pyramid magnesium oxides, and the particle size of the embroidery ball-shaped powder is 20 to 40 μm.
2. The method for preparing the magnesium oxide carbon dioxide adsorbent according to claim 1, comprising the following steps: (1) mixing a carbon source, a water-soluble magnesium salt, an alkali and water, and performing a hydrothermal reaction to obtain magnesium carbonate; (2) calcining the magnesium carbonate obtained in step (1), cooling it to room temperature, and obtaining a magnesium oxide carbon dioxide adsorbent; the cooling rate is 20 to 200° C. / min.
3. The preparation method according to claim 2, characterized in that: The carbon source in step (1) includes one or more of ascorbic acid, urea, potassium bicarbonate and sodium bicarbonate.
4. The preparation method according to claim 2, characterized in that: The water-soluble magnesium salt in step (1) includes one or more of anhydrous magnesium sulfate, anhydrous magnesium chloride and magnesium acetate.
5. The preparation method according to claim 2, characterized in that: The base in step (1) includes NaOH and / or KOH.
6. The preparation method according to claim 2, characterized in that: In the step (1), the molar ratio of the carbon element of the carbon source to the magnesium element of the water-soluble magnesium salt is (3-10):
1.
7. The preparation method according to claim 2, characterized in that: The temperature of the hydrothermal reaction in step (1) is 120-200° C.; the hydrothermal reaction time is 3-10 hours.
8. The preparation method according to claim 2, characterized in that: The calcination temperature in step (2) is 650-900° C. and the calcination time is 1-3 hours.
9. The preparation method according to claim 8, characterized in that: The heating rate of heating to the calcination temperature in the step (2) is 5 to 35° C. / min.
10. Use of the magnesium oxide carbon dioxide adsorbent according to claim 1 or the magnesium oxide carbon dioxide adsorbent prepared by the preparation method according to any one of claims 2 to 9 as a CO2 adsorbent.
Citation Information
Patent Citations
Synthetic method of {111} crystal face preferred magnesium oxide material
CN103265058A
Magnesium oxide and preparation method thereof
CN104310808A
Preparation method of mesoporous magnesium oxide of flower-like morphology composed of nanoparticles
CN109052437A
Preparation method of porous pompon-shaped magnesium oxide
CN111943238A
Preparation method of nano magnesium oxide
CN112645366A