Ni-carboxylic acid magnetic cellulose microsphere and preparation method thereof

Through the preparation method of Ni-carboxylic acid magnetic cellulose microspheres, cellulose coated magnetic particles to prevent oxidation and agglomeration, solving the problems of easy oxidation and high cost of existing magnetic particles in the air, and achieving high efficiency and low cost grouping Amine tag protein isolation.

CN119075954APending Publication Date: 2024-12-06GUANGDONG UNIV OF TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411460904.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-18
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

The existing Ni2+-NTA affinity ligand modified magnetic particles are easily oxidized in the air, resulting in a decrease in magnetic properties, high cost, and it is difficult to simultaneously prevent the agglomeration of magnetic particles and effectively separate histidine-tagged proteins.

Method used

The preparation method of Ni-carboxylic acid magnetic cellulose microspheres is adopted to generate carboxylic acid cellulose through esterification reaction, and the cellulose is dissolved in combination with NaOH/urea aqueous solution, and magnetic Fe3O4 particles are dispersed in the emulsification system, and formed by NiSO4 ion exchange reaction. Ni-carboxylic acid magnetic cellulose microspheres, cellulose coated magnetic particles to prevent oxidation and agglomeration.

Benefits of technology

Effectively prevent the oxidation and agglomeration of magnetic particles, improve the stability and separation efficiency of magnetic particles, and achieve low-cost and high-efficiency separation of histidine tag protein without additional modification of magnetic particles.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119075954A_ABST
    Figure CN119075954A_ABST
Patent Text Reader

Abstract

The invention belongs to the field of cellulose carrier protein separation, and particularly relates to Ni-carboxylic acid magnetic cellulose microspheres and a preparation method thereof.The preparation method comprises the steps that S1, cellulose powder with the formula amount is dispersed in distilled water, polybasic carboxylic acid is added for an esterification reaction, and carboxylated cellulose is obtained; s2, dissolving the carboxylated cellulose in a NaOH / urea aqueous solution obtained by mixing NaOH, urea and water to obtain a cellulose solution; s3, dispersing magnetic Fe3O4 in the cellulose solution according to a formula ratio to obtain a mixture; adding the mixture into an emulsification system, continuously stirring uniformly to obtain carboxylic acid magnetic cellulose microspheres, and cleaning the carboxylic acid magnetic cellulose microspheres; s4, the carboxylic acid magnetic cellulose microspheres are added into a NiSO4 solution for a reaction, deionized water is used for washing, and the Ni-carboxylic acid magnetic cellulose microspheres are obtained, the problems of aggregation and oxidation of the magnetic cellulose microspheres can be effectively solved, and the method has the advantages of being good in histidine tag protein separation effect and low in cost.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of separating proteins using cellulose carriers, and in particular relates to Ni-carboxylic acid magnetic cellulose microspheres and a preparation method thereof. Background Art

[0002] Protein analysis and detection is of great significance in the fields of chemistry, life sciences and clinical medicine. Proteins are of various types and complex structures. They often coexist with a large number of interfering components, such as small organic molecules, salts and other proteins, which strongly interfere with the detection of target proteins. Therefore, before detecting the protein structure, the protein needs to be separated and purified.

[0003] At present, protein sample pretreatment methods are mainly divided into protein precipitation, ultrafiltration, liquid-liquid extraction, solid phase extraction (SPE) and magnetic solid phase extraction.

[0004] Protein precipitation is a method of adding specific reagents to change the solution environment to precipitate proteins, which are then separated by centrifugation. The advantages of this method are simple operation and high efficiency, but the disadvantages are poor selectivity, some protein may be lost during the precipitation process, and subsequent purification steps are usually required.

[0005] Ultrafiltration uses the selective filtration of the membrane to concentrate and purify macromolecular proteins under external pressure. This method is simple to operate, but the ultrafiltration membrane may be clogged by contaminants in the sample, affecting its service life and efficiency.

[0006] Liquid-liquid extraction is based on the difference in solubility of substances in two immiscible solvents, transferring proteins from one solvent to another. Although this method is simple, the water-organic phase system may cause protein denaturation.

[0007] Solid phase extraction (SPE) technology uses solid chromatographic fillers to adsorb proteins in the sample, and then elutes with a specific solvent to purify and enrich the sample. SPE technology can be automated, reducing the number of operating steps, and when combined with magnetic materials, it can avoid the use of high-pressure and easily clogged extraction columns, thereby improving separation efficiency. Among them, magnetic solid phase extraction disperses magnetic nanomaterials in the matrix, and the contact area between the adsorbent and the target protein is large. It can complete the adsorption and separation of the target protein under low dosage and short time conditions, thereby improving the adsorption efficiency. For example, Fe3O4@Au / MPA / NTA-Ni2+ magnetic nanoparticles, by surface modification of Ni 2+ -NTA ligand adsorbs His-tagged proteins.

[0008] In magnetic solid phase extraction, Ni 2+-NTA affinity ligand modified magnetic particles have attracted wide attention in the purification of histidine-tagged proteins. These magnetic particles have the advantage of large specific surface area, thus enhancing the binding with proteins.

[0009] However, currently 2+ -NTA affinity ligand modified magnetic particles still have shortcomings:

[0010] The diameter of magnetic particles is very small. Under the influence of surface energy, these magnetic particles are prone to agglomeration, which affects the magnetic properties and dispersibility of the magnetic particles. In addition, the exposed magnetic particles are easily oxidized in the air, causing the magnetic particles to lose their activity.

[0011] Although the existing technology modifies the surface of magnetic particles by introducing specific functional groups or polymers to reduce direct contact between particles, thereby avoiding agglomeration and oxidation. However, at present, it is mainly modified by silane coupling agents, polymer coating or biomolecules (such as proteins, polysaccharides). Although the above-mentioned magnetic particle modification methods can enhance the stability of magnetic particles in complex environments. However, the current modification methods cannot simultaneously make Ni 2+ It is connected to magnetic particles, and because the surface of the magnetic particles is modified with proteins and polysaccharides, it cannot separate histidine-tagged proteins well and has the problem of high cost. Summary of the invention

[0012] One of the purposes of the present invention is to avoid the shortcomings of the prior art and provide a Ni-carboxylic acid magnetic cellulose microsphere and a preparation method thereof, which can effectively prevent the aggregation and oxidation problems of the magnetic cellulose microspheres and has the advantages of good separation effect of histidine tagged protein and low cost.

[0013] To achieve one of the above purposes, the present invention provides the following technical solutions:

[0014] A method for preparing Ni-carboxylic acid magnetic cellulose microspheres is provided, comprising the following steps:

[0015] S1, dispersing a formula amount of cellulose powder in distilled water, adding polycarboxylic acid to carry out esterification reaction, and obtaining carboxylated cellulose;

[0016] S2, dissolving the carboxylated cellulose in a NaOH / urea aqueous solution obtained by mixing NaOH, urea and water to obtain a cellulose solution;

[0017] S3, dispersing a formula amount of magnetic Fe3O4 in the cellulose solution to obtain a mixture;

[0018] The mixture is put into an emulsified system obtained by mixing Span 80, Tween 80 and liquid paraffin, and the mixture is stirred evenly to obtain carboxylic acid magnetic cellulose microspheres, and the carboxylic acid magnetic cellulose microspheres are washed;

[0019] S4. Adding carboxylic acid magnetic cellulose microspheres into NiSO4 solution to react, and after the reaction is completed, washing with deionized water to remove the remaining NiSO4 to obtain Ni-carboxylic acid magnetic cellulose microspheres.

[0020] In some embodiments, sodium dihydrogen phosphate is further added to the esterification reaction, and the esterification reaction process uses deionized water for ultrasonic reaction, and the esterification is carried out at 110° C. to 130° C. for 80 min to 100 min, and after cooling, it is washed with deionized water for multiple times.

[0021] In some embodiments, the polycarboxylic acid is 1,2,3,4-butanetetracarboxylic acid or citric acid;

[0022] The weight ratio of cellulose powder, polycarboxylic acid and sodium dihydrogen phosphate is 1-1.5:0.1-0.5:0.2.

[0023] In some embodiments, the weight ratio of NaOH, urea and water is (1-8):(6-14):(78-93),

[0024] The weight ratio of the carboxylated cellulose to the NaOH / urea aqueous solution is 1-2:30-60.

[0025] In some embodiments, the weight ratio of the magnetic Fe3O4 to the cellulose solution is 0.5-1:2-4.

[0026] In some embodiments, the concentration of the NiSO4 solution is 0.4M to 0.6M, and the amount of the NiSO4 solution added per gram of carboxylic acid magnetic cellulose microspheres is 35ml to 50ml.

[0027] In some embodiments, during dissolution, the carboxylated cellulose is precooled at -12°C to -15°C for 15 min, then swollen at a stirring speed of 300 to 500 r / min, and dissolved at a stirring speed of 3000 r / min for 15 to 30 min.

[0028] In some embodiments, the ratio of the amount of Span 80, Tween 80 and liquid paraffin is 1-5:1-3:100-200 respectively;

[0029] After the mixture is put into the emulsification system, the stirring temperature is 25° C. to 45° C., the stirring speed is 500 r / min to 1000 r / min, and the stirring time is 120 min to 240 min.

[0030] In some embodiments, the Ni-carboxylate magnetic cellulose microspheres are washed with SDS solution and ethanol in sequence.

[0031] To achieve the second of the above objects, the present invention provides the following technical solutions:

[0032] Also provided are Ni-carboxylic acid magnetic cellulose microspheres, which are prepared by the above-mentioned preparation method.

[0033] Beneficial effects of the method for preparing Ni-carboxylic acid magnetic cellulose microspheres of the present invention:

[0034] The invention discloses a method for preparing Ni-carboxylic acid magnetic cellulose microspheres. The method comprises the following steps: firstly, cellulose powder is reacted into carboxylated cellulose through an esterification reaction, and then a NaOH / urea aqueous solution is used to dissolve the carboxylated cellulose. NaOH hydrate molecules in the NaOH / urea aqueous solution are combined with cellulose molecular chains in the decarboxylated cellulose. The NaOH hydrate molecules form hydrogen bonds with the carboxylated cellulose molecular chains, thereby destroying the original hydrogen bond structures of the carboxylated cellulose molecular chains and dissolving the carboxylated cellulose. Meanwhile, urea in the NaOH / urea aqueous solution inhibits the reaggregation of free carboxylated cellulose molecular chains, thereby improving the dissolution efficiency of the carboxylated cellulose molecular chains, so that the carboxylated cellulose can subsequently wrap magnetic particles.

[0035] An emulsification system composed of Span 80, Tween 80 and liquid paraffin is used to disperse the mixture of magnetic Fe3O4 and cellulose solution. Span 80 and Tween 80 in the emulsification system serve as surfactants, and liquid paraffin is the oil phase. The cellulose solution can be dispersed into microspheres of uniform size and about ten to hundreds of microns in diameter in the emulsification system with opposite polarities. The operation is easy and the cost is low.

[0036] Microspheres of this size can effectively refine the size of magnetic particles, further increase the specific surface area of ​​the magnetic particles, and improve the efficiency of Ni-carboxylic acid magnetic cellulose microspheres in separating proteins.

[0037] In addition, the cellulose solution can effectively prevent the oxidation of the magnetic particles by coating the surface of the magnetic particles, thereby improving the functional stability of the magnetic particles. The cellulose attached to the surface of the magnetic particles also reduces the surface energy and surface activity of each magnetic particle, avoiding the aggregation of the magnetic particles and ensuring the separation function of the magnetic particles.

[0038] Cellulose has a large number of hydroxyl groups. After being modified with polycarboxylic acids, the carboxyl groups of the modified cellulose quickly and stably attach Ni to its surface. The cellulose not only wraps the magnetic particles to prevent the magnetic particles from focusing, but also does not require additional modification of the magnetic particles, effectively improving the performance of the magnetic particles and having the advantage of low cost. BRIEF DESCRIPTION OF THE DRAWINGS

[0039] Figure 1A VSM diagram of Ni-carboxylate magnetic cellulose microspheres of the experimental example.

[0040] Figure 1B This is a diagram showing the effect of collecting Ni-carboxylate magnetic cellulose microspheres from an aqueous solution.

[0041] Figure 2 This is a scanning electron microscope image of the Ni-carboxylate magnetic cellulose microspheres of the experimental example.

[0042] Figure 3 This is the X-ray diffraction pattern of the Ni-carboxylate magnetic cellulose microspheres of the test example.

[0043] Figure 4 This is the infrared image of Ni-carboxylate magnetic cellulose microspheres of the test example.

[0044] Figure 5 This is the particle size distribution diagram of Ni-carboxylate magnetic cellulose microspheres of the test example.

[0045] Figure 6 This is the adsorption kinetic curve of the Ni-carboxylate magnetic cellulose microspheres for separating histidine-tagged proteins in the experimental example.

[0046] Figure 7 This is the adsorption isotherm fitting curve of Ni-carboxylate magnetic cellulose microspheres for separating histidine-tagged proteins in the experimental example.

[0047] Figure 8 This is the repeated use of Ni-carboxylate magnetic cellulose microspheres for separating histidine-tagged proteins in an experimental example.

[0048] Fig. 9 This is the electrophoresis diagram of the Ni-carboxylate magnetic cellulose microspheres used in the test example to separate histidine-tagged proteins. DETAILED DESCRIPTION

[0049] The preferred embodiments of the present invention will be described in more detail below with reference to the accompanying drawings. Although the preferred embodiments of the present invention are shown in the accompanying drawings, it should be understood that the present invention can be implemented in various forms and should not be limited by the embodiments described herein. On the contrary, these embodiments are provided to make the present invention more thorough and complete, and to fully convey the scope of the present invention to those skilled in the art.

[0050] Example 1

[0051] This embodiment discloses a method for preparing Ni-carboxylic acid magnetic cellulose microspheres, comprising the following steps:

[0052] Step S1: Esterification reaction

[0053] Disperse cellulose powder in distilled water, add an appropriate amount of polycarboxylic acid (such as 1,2,3,4-butanetetracarboxylic acid or citric acid), and perform esterification reaction to generate carboxylated cellulose. In the esterification reaction, sodium dihydrogen phosphate can be added as a catalyst to improve the reaction efficiency. Use deionized water for ultrasonic reaction, control the reaction temperature at 110℃~130℃, and the reaction time is 80min to 100min.

[0054] After the reaction is completed, the mixture is washed with deionized water for several times to remove unreacted polycarboxylic acid and sodium dihydrogen phosphate.

[0055] Step S2: Preparation of cellulose solution

[0056] Sodium hydroxide (NaOH), urea and water are mixed in a weight ratio of 1:6-14:78-93 to prepare a NaOH / urea aqueous solution.

[0057] The cellulose solution is pre-cooled at -12°C to -15°C for 15 minutes, then the carboxylated cellulose is swollen at a stirring speed of 300 to 500 rpm, and dissolved at a stirring speed of 3000 rpm for 15 to 30 minutes to obtain a cellulose solution.

[0058] Step S3: Preparation of carboxylated magnetic cellulose microspheres

[0059] A formulated amount of magnetic Fe3O4 powder is dispersed in a cellulose solution to obtain a mixture.

[0060] The mixture is added into an emulsified system obtained by mixing Span 80, Tween 80 and liquid paraffin in a dosage ratio of 1-5:1-3:100-200, and the stirring temperature is controlled at 25°C-45°C, the stirring speed is 500-1000 rpm, and the stirring time is 120-240 min to obtain carboxylic acid magnetic cellulose microspheres.

[0061] The carboxylated magnetic cellulose microspheres are washed to remove unreacted emulsifier and impurities.

[0062] Step S4: Ni ion exchange reaction

[0063] The carboxylate magnetic cellulose microspheres are added into a 0.4M to 0.6M NiSO4 solution to allow the microspheres to undergo an ion exchange reaction with NiSO4.

[0064] After the reaction was completed, the microspheres were washed with deionized water to remove the residual NiSO4.

[0065] Cleaning steps

[0066] The Ni-carboxylate magnetic cellulose microspheres were washed with SDS solution and ethanol in sequence to further remove surface impurities and unreacted chemicals.

[0067] The weight ratio of cellulose powder, polycarboxylic acid and sodium dihydrogen phosphate is controlled within the range of 1-1.5:0.1-0.5:0.2.

[0068] The weight ratio of carboxylated cellulose to NaOH / urea aqueous solution is controlled at 1-2:30-60.

[0069] The weight ratio of magnetic Fe3O4 to cellulose solution is controlled at 0.5-1:2-4.

[0070] The amount of NiSO4 solution added to each gram of carboxylic acid magnetic cellulose microspheres is controlled to be 35ml-50ml.

[0071] Through the above steps, Ni-carboxylate magnetic cellulose microspheres are prepared.

[0072] Ni-carboxylic acid magnetic cellulose microspheres encapsulate magnetic nanoparticles through cellulose. The cellulose surface is rich in hydroxyl groups and has the characteristics of biodegradability, low price, and good biocompatibility. Based on these excellent properties, cellulose can be used to coat magnetic nanoparticles to improve the stability of magnetic nanoparticles to prevent magnetic particles from aggregating and oxidizing. The rich hydroxyl groups on the surface of carboxylic acid cellulose can be modified to introduce new functional groups to give it more properties. Therefore, the magnetic cellulose microspheres modified by Ni-polycarboxylic acid groups and the polycarboxylated microspheres chelated with nickel ions can be combined with the histidine residues on the surface of recombinant proteins in a coordinated manner, thereby achieving highly selective and efficient separation of histidine-tagged proteins.

[0073] Example 2

[0074] This embodiment discloses a method for preparing Ni-carboxylic acid magnetic cellulose microspheres, comprising the following steps:

[0075] Step S1: Esterification reaction

[0076] Disperse cellulose powder in distilled water, add an appropriate amount of polycarboxylic acid (such as 1,2,3,4-butanetetracarboxylic acid or citric acid), and perform esterification reaction to generate carboxylated cellulose. In the esterification reaction, sodium dihydrogen phosphate can be added as a catalyst to improve the reaction efficiency. Use deionized water for ultrasonic reaction, control the reaction temperature at 110°C, and the reaction time is 80 minutes.

[0077] After the reaction is completed, the mixture is washed with deionized water for several times to remove unreacted polycarboxylic acid and sodium dihydrogen phosphate.

[0078] Step S2: Preparation of cellulose solution

[0079] Sodium hydroxide (NaOH), urea and water were mixed in a weight ratio of 1:6:78 to prepare a NaOH / urea aqueous solution.

[0080] The mixture was precooled at -12°C for 15 minutes, and then the carboxylated cellulose was swollen at a stirring speed of 300 rpm and dissolved at a stirring speed of 3000 rpm for 15 minutes to obtain a cellulose solution.

[0081] Step S3: Preparation of carboxylated magnetic cellulose microspheres

[0082] A formulated amount of magnetic Fe3O4 powder is dispersed in a cellulose solution to obtain a mixture.

[0083] The mixture was added into an emulsified system obtained by mixing Span 80, Tween 80 and liquid paraffin in a dosage ratio of 1:1:100, and the stirring temperature was controlled at 25°C, the stirring speed was 500 rpm, and the stirring time was 120 min to obtain carboxylate magnetic cellulose microspheres.

[0084] The carboxylated magnetic cellulose microspheres are washed to remove unreacted emulsifier and impurities.

[0085] Step S4: Ni ion exchange reaction

[0086] The carboxylated magnetic cellulose microspheres were added into a 0.4 M NiSO4 solution to allow the microspheres to undergo an ion exchange reaction with NiSO4.

[0087] After the reaction was completed, the microspheres were washed with deionized water to remove the residual NiSO4.

[0088] Cleaning steps

[0089] The Ni-carboxylate magnetic cellulose microspheres were washed with SDS solution and ethanol in sequence to further remove surface impurities and unreacted chemicals.

[0090] The weight ratio of cellulose powder, polycarboxylic acid and sodium dihydrogen phosphate is controlled at 1:0.1:0.2.

[0091] The weight ratio of carboxylated cellulose to NaOH / urea aqueous solution was controlled at 1:30.

[0092] The weight ratio of magnetic Fe3O4 to cellulose solution is controlled at 0.5:2.

[0093] The amount of NiSO4 solution added per gram of carboxylic acid magnetic cellulose microspheres is controlled at 35 ml.

[0094] Through the above steps, Ni-carboxylate magnetic cellulose microspheres are prepared.

[0095] Ni-carboxylic acid magnetic cellulose microspheres encapsulate magnetic nanoparticles through cellulose. The cellulose surface is rich in hydroxyl groups and has the characteristics of biodegradability, low price, and good biocompatibility. Based on these excellent properties, cellulose can be used to coat magnetic nanoparticles to improve the stability of magnetic nanoparticles to prevent magnetic particles from aggregating and oxidizing. The rich hydroxyl groups on the surface of carboxylic acid cellulose can be modified to introduce new functional groups to give it more properties. Therefore, the magnetic cellulose microspheres modified by Ni-polycarboxylic acid groups and the polycarboxylated microspheres chelated with nickel ions can be combined with the histidine residues on the surface of recombinant proteins in a coordinated manner, thereby achieving highly selective and efficient separation of histidine-tagged proteins.

[0096] Example 3

[0097] This embodiment discloses a method for preparing Ni-carboxylic acid magnetic cellulose microspheres, comprising the following steps:

[0098] Step S1: Esterification reaction

[0099] Disperse cellulose powder in distilled water, add an appropriate amount of polycarboxylic acid (such as 1,2,3,4-butanetetracarboxylic acid or citric acid), and perform esterification reaction to generate carboxylated cellulose. In the esterification reaction, sodium dihydrogen phosphate can be added as a catalyst to improve the reaction efficiency. Use deionized water for ultrasonic reaction, control the reaction temperature at 130°C, and the reaction time is 100 minutes.

[0100] After the reaction is completed, the mixture is washed with deionized water for several times to remove unreacted polycarboxylic acid and sodium dihydrogen phosphate.

[0101] Step S2: Preparation of cellulose solution

[0102] Sodium hydroxide (NaOH), urea, and water were mixed in a weight ratio of 1:14:93 to prepare a NaOH / urea aqueous solution.

[0103] The mixture was precooled at -15°C for 15 minutes, and then the carboxylated cellulose was swollen at a stirring speed of 500 rpm and dissolved at a stirring speed of 3000 rpm for 30 minutes to obtain a cellulose solution.

[0104] Step S3: Preparation of carboxylated magnetic cellulose microspheres

[0105] A formulated amount of magnetic Fe3O4 powder is dispersed in a cellulose solution to obtain a mixture.

[0106] The mixture was added into an emulsified system obtained by mixing Span 80, Tween 80 and liquid paraffin in a dosage ratio of 5:3:200, and the stirring temperature was controlled at 45° C., the stirring speed was 1000 rpm, and the stirring time was 240 min to obtain carboxylate magnetic cellulose microspheres.

[0107] The carboxylated magnetic cellulose microspheres are washed to remove unreacted emulsifier and impurities.

[0108] Step S4: Ni ion exchange reaction

[0109] The carboxylated magnetic cellulose microspheres were added into a 0.6 M NiSO4 solution to allow the microspheres to undergo an ion exchange reaction with NiSO4.

[0110] After the reaction was completed, the microspheres were washed with deionized water to remove the residual NiSO4.

[0111] Cleaning steps

[0112] The Ni-carboxylate magnetic cellulose microspheres were washed with SDS solution and ethanol in sequence to further remove surface impurities and unreacted chemicals.

[0113] The weight ratio of cellulose powder, polycarboxylic acid and sodium dihydrogen phosphate is controlled at 1.2:0.4:0.2.

[0114] The weight ratio of carboxylated cellulose to NaOH / urea aqueous solution is controlled at 1.5:30-60.

[0115] The weight ratio of magnetic Fe3O4 to cellulose solution is controlled at 0.8:2.5.

[0116] The amount of NiSO4 solution added per gram of carboxylic acid magnetic cellulose microspheres is controlled at 40 ml.

[0117] Through the above steps, Ni-carboxylate magnetic cellulose microspheres are prepared.

[0118] Ni-carboxylic acid magnetic cellulose microspheres encapsulate magnetic nanoparticles through cellulose. The cellulose surface is rich in hydroxyl groups and has the characteristics of biodegradability, low price, and good biocompatibility. Based on these excellent properties, cellulose can be used to coat magnetic nanoparticles to improve the stability of magnetic nanoparticles to prevent magnetic particles from aggregating and oxidizing. The rich hydroxyl groups on the surface of carboxylic acid cellulose can be modified to introduce new functional groups to give it more properties. Therefore, the magnetic cellulose microspheres modified by Ni-polycarboxylic acid groups and the polycarboxylated microspheres chelated with nickel ions can be combined with the histidine residues on the surface of recombinant proteins in a coordinated manner, thereby achieving highly selective and efficient separation of histidine-tagged proteins.

[0119] Example 4

[0120] This embodiment discloses a method for preparing Ni-carboxylic acid magnetic cellulose microspheres, comprising the following steps:

[0121] Step S1: Esterification reaction

[0122] Disperse cellulose powder in distilled water, add an appropriate amount of polycarboxylic acid (such as 1,2,3,4-butanetetracarboxylic acid or citric acid), and perform esterification reaction to generate carboxylated cellulose. In the esterification reaction, sodium dihydrogen phosphate can be added as a catalyst to improve the reaction efficiency. Use deionized water for ultrasonic reaction, control the reaction temperature at 120°C, and the reaction time is 90 minutes.

[0123] After the reaction is completed, the mixture is washed with deionized water for several times to remove unreacted polycarboxylic acid and sodium dihydrogen phosphate.

[0124] Step S2: Preparation of cellulose solution

[0125] Sodium hydroxide (NaOH), urea and water were mixed in a weight ratio of 1:10:80 to prepare a NaOH / urea aqueous solution.

[0126] The mixture was precooled at -13°C for 15 minutes, and then the carboxylated cellulose was swollen at a stirring speed of 400 rpm and dissolved at a stirring speed of 3000 rpm for 18 minutes to obtain a cellulose solution.

[0127] Step S3: Preparation of carboxylated magnetic cellulose microspheres

[0128] A formulated amount of magnetic Fe3O4 powder is dispersed in a cellulose solution to obtain a mixture.

[0129] The mixture was added into an emulsified system obtained by mixing Span 80, Tween 80 and liquid paraffin in a dosage ratio of 4:2:150, and the stirring temperature was controlled at 30°C, the stirring speed was 800 rpm, and the stirring time was 150 min to obtain carboxylate magnetic cellulose microspheres.

[0130] The carboxylated magnetic cellulose microspheres are washed to remove unreacted emulsifier and impurities.

[0131] Step S4: Ni ion exchange reaction

[0132] The carboxylated magnetic cellulose microspheres were added into a 0.55 M NiSO4 solution to allow the microspheres to undergo an ion exchange reaction with NiSO4.

[0133] After the reaction was completed, the microspheres were washed with deionized water to remove the residual NiSO4.

[0134] Cleaning steps

[0135] The Ni-carboxylate magnetic cellulose microspheres were washed with SDS solution and ethanol in sequence to further remove surface impurities and unreacted chemicals.

[0136] The weight ratio of cellulose powder, polycarboxylic acid and sodium dihydrogen phosphate is controlled at 1.1:0.3:0.2.

[0137] The weight ratio of carboxylated cellulose to NaOH / urea aqueous solution was controlled at 1.5:40.

[0138] The weight ratio of magnetic Fe3O4 to cellulose solution is controlled at 0.8:2.5.

[0139] The amount of NiSO4 solution added per gram of carboxylic acid magnetic cellulose microspheres is controlled at 40 ml.

[0140] Through the above steps, Ni-carboxylate magnetic cellulose microspheres are prepared.

[0141] Ni-carboxylic acid magnetic cellulose microspheres encapsulate magnetic nanoparticles through cellulose. The cellulose surface is rich in hydroxyl groups and has the characteristics of biodegradability, low price, and good biocompatibility. Based on these excellent properties, cellulose can be used to coat magnetic nanoparticles to improve the stability of magnetic nanoparticles to prevent magnetic particles from aggregating and oxidizing. The rich hydroxyl groups on the surface of carboxylic acid cellulose can be modified to introduce new functional groups to give it more properties. Therefore, the magnetic cellulose microspheres modified by Ni-polycarboxylic acid groups and the polycarboxylated microspheres chelated with nickel ions can be combined with the histidine residues on the surface of recombinant proteins in a coordinated manner, thereby achieving highly selective and efficient separation of histidine-tagged proteins.

[0142] Test example

[0143] In order to verify the performance of the Ni-carboxylate magnetic cellulose microspheres of the present invention, a sample was prepared by the following test, the steps of which include:

[0144] 1.5 g of cellulose powder and 0.1 g of 1,2,3,4-butanetetracarboxylic acid were added into a flask, and 0.15 g of sodium dihydrogen phosphate was added as a catalyst. The mixture was ultrasonically dissolved with deionized water, esterified at 130° C. for 90 min, and washed with deionized water several times to obtain carboxylated cellulose.

[0145] Dissolving carboxylated cellulose in a NaOH / urea aqueous solution, wherein the amount of carboxylated cellulose is 3%, and mixing uniformly to obtain a mixed solution; wherein the weight ratio of the sodium hydroxide, urea and water in the NaOH / urea aqueous solution is 7:12:81, during the dissolution process, washing the microspheres with a low-temperature reverse S solution, absorbing the residual oil phase mixture, and then washing the carboxylated magnetic cellulose microspheres with ethanol;

[0146] Carboxylate magnetic cellulose microspheres were added into NiSO4 solution for reaction, and then washed with deionized water to remove excess NiSO4, wherein the amount of NiSO4 used was 0.1M 50mL, to obtain Ni-carboxylate magnetic cellulose microspheres (CAM / MCMs-Ni), which were freeze-dried and stored.

[0147] The performance of the Ni-carboxylate magnetic cellulose microspheres obtained above was tested, and the results were as follows:

[0148] Figure 1A The VSM diagram of Ni-carboxylic acid magnetic cellulose microspheres (CAM / MCMs-Ni) shows an S-shaped hysteresis loop with no hysteresis and coercivity, showing good magnetic response performance. It can be considered that the microspheres may have superparamagnetism. The saturation magnetization of CAM / MCMs-Ni and Fe3O4 are 13.69emu / g and 49.14emu / g, respectively. Figure 1B It is shown that the external magnet can collect CAM / MCMs-Ni from the aqueous solution, which shows that the Ni-carboxylate magnetic cellulose microspheres of the present invention can still achieve the separation effect after being wrapped by fibers.

[0149] Figure 2 The figure is a scanning electron microscope image of the prepared Ni-carboxylic acid magnetic cellulose microspheres. The material is in a relatively regular spherical shape, which shows that the Ni-carboxylic acid magnetic cellulose microspheres prepared in the present invention can better control the size of the magnetic particles.

[0150] Figure 3 This is the X-ray diffraction pattern of the prepared Ni-carboxylic acid magnetic cellulose microspheres. It can be seen from the figure that at 2θ at 22°, a crystalline diffraction peak belonging to cellulose type I can be observed, indicating that the crystal structure of cellulose has not changed when it becomes a microsphere; the corresponding diffraction peaks at 30.1°, 35.5°, 43.1°, 53.4°, 57.0°, and 63.1° correspond to the (220), (311), (400), (422), (511), and (440) diffraction planes of Fe3O4 face-centered cubic, respectively, indicating that the crystal form of the magnetic particles can be found at the corresponding diffraction angles.

[0151] Figure 4 The infrared image of the prepared Ni-carboxylic acid magnetic cellulose microspheres shows that at the wave number of 569 cm -1 The absorption peaks on the left and right are caused by the vibration of Fe-O bonds and are the characteristic absorption peaks of Fe3O4; 3350cm -1 The broad absorption peak is the stretching vibration absorption peak of -OH, 1369cm -1 is the bending vibration of CO; at 1718cm -1 The absorption peaks of C=O carboxylic acid groups are at 3442 cm due to the chelation of metal ions. -1 The OH absorption peaks on the left and right become broader and shift toward higher wavenumbers, and the peak intensity changes significantly, which proves that the material has been successfully modified and chelated with nickel ions.

[0152] Figure 5This is the particle size distribution diagram of the prepared Ni-carboxylate magnetic cellulose microspheres. The microsphere size is about 1-2μm and the dispersion is good.

[0153] To further illustrate the performance of Ni-carboxylate magnetic cellulose microspheres in separating histidine-tagged proteins, the following operations were performed:

[0154] S1. Weigh 0.5 g of Ni-carboxylate magnetic cellulose microspheres and add 10 mL of buffer A to prepare a 50 mg / mL Ni-carboxylate magnetic cellulose microsphere solution.

[0155] S2, ultrasonically disperse the microsphere solution in S1 for 5 min and equilibrate the magnetic beads;

[0156] S3, add 1 mL of the target protein solution to the microspheres in S2, shake and combine for 20 min, and then separate by magnetic separation. The target protein has been magnetically adsorbed;

[0157] S4, wash the microspheres adsorbed with protein in S3 with 2 mL bufferA1 for 2 min to rinse impurities

[0158] S5, wash again with bufferA1 buffer for 2 min to rinse impurities;

[0159] S6, add 0.8mL buffer B to the microspheres in S5, shake and elute for 4 minutes, and the supernatant after magnetic separation is the separated and purified histidine-tagged recombinant protein. The above buffer A, buffer A1, and buffer B are the binding solution, rinsing solution, and elution solution of the histidine-tagged protein, respectively.

[0160] The following results are obtained:

[0161] Figure 6 The adsorption kinetic curve of the prepared Ni-carboxylic acid magnetic cellulose microspheres for separating histidine-tagged proteins. The adsorption amount of BSA at CAM / MCMs-Ni at 30°C was 55.49 mg / g. The correlation coefficient R obtained by fitting the pseudo-second-order kinetic model 2 The theoretical equilibrium adsorption capacity is 65.09 mg / g between 0.9 and 0.95, which is quite different from the actual value. 2 In the range of 0.95 to 0.99, the calculated theoretical equilibrium adsorption capacity is 56.69 mg / g, which is closer to the actual measured equilibrium adsorption capacity. Therefore, the pseudo-first-order kinetic model can better describe the adsorption process of CAM / MCMs-Ni on histidine protein.

[0162] Figure 7The adsorption isotherm fitting curve of Ni-carboxylated magnetic cellulose microspheres for separating histidine-tagged proteins was obtained. The correlation coefficient R of CAM / MCMs-Ni adsorbing histidine-tagged proteins fitted by Langmuir isotherm adsorption model at 30 °C was 2 The correlation coefficient R of the Freundlich isotherm adsorption model was 0.952. 2 is 0.838, so the Langmuir isotherm adsorption model can better describe the adsorption behavior of CAM / MCMs-Ni.

[0163] Figure 8 In order to reuse the prepared Ni-carboxylate magnetic cellulose microspheres for separating histidine-tagged proteins, 0.02 mol / L PBS acetate buffer (pH=9, containing 0.5 M NaCl and 0.5 M imidazole) was selected as the eluent. After desorption, the regenerated CAM / MCMs-Ni was used to extract the proteins again.

[0164] Fig. 9 This is the electrophoresis diagram of the prepared Ni-carboxylic acid magnetic cellulose microspheres for separating histidine-tagged proteins. From lanes L and S, it can be seen that compared with the initial protein cell lysate (lane L), the protein band after material treatment (lane S) is weakened, indicating that part of the target protein is bound to the material; from the eluate band (lane 1), it can be seen that the target recombinant protein is enriched and purified, and the material selectivity is good.

[0165] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A method for preparing Ni-carboxylic acid magnetic cellulose microspheres, characterized in that: The following steps are included: S1, dispersing a formula amount of cellulose powder in distilled water, adding polycarboxylic acid to carry out esterification reaction, and obtaining carboxylated cellulose; S2, dissolving the carboxylated cellulose in a NaOH / urea aqueous solution obtained by mixing NaOH, urea and water to obtain a cellulose solution; S3, dispersing a formula amount of magnetic Fe3O4 in the cellulose solution to obtain a mixture; The mixture is put into an emulsified system obtained by mixing Span 80, Tween 80 and liquid paraffin, and the mixture is stirred evenly to obtain carboxylic acid magnetic cellulose microspheres and the carboxylic acid magnetic cellulose microspheres are washed; S4, adding carboxylic acid magnetic cellulose microspheres into NiSO4 solution for reaction, and after the reaction, washing with deionized water to remove the remaining NiSO4 to obtain Ni-carboxylic acid magnetic cellulose microspheres.

2. The method for preparing Ni-carboxylate magnetic cellulose microspheres according to claim 1, characterized in that: Sodium dihydrogen phosphate is also added in the esterification reaction. The esterification process uses deionized water for ultrasonic reaction, and the esterification is carried out at 110° C. to 130° C. for 80 min to 100 min. After cooling, the product is washed with deionized water for multiple times.

3. The method for preparing Ni-carboxylate magnetic cellulose microspheres according to claim 2, characterized in that: The polycarboxylic acid is 1,2,3,4-butanetetracarboxylic acid or citric acid; The weight ratio of the cellulose powder, the polycarboxylic acid and the sodium dihydrogen phosphate is 1-1.5:0.1-0.5:0.

2.

4. The method for preparing Ni-carboxylate magnetic cellulose microspheres according to claim 1, characterized in that: The weight ratio of NaOH, urea and water is (1-8):(6-14):(78-93), The weight ratio of the carboxylated cellulose to the NaOH / urea aqueous solution is 1-2:30-60.

5. The method for preparing Ni-carboxylate magnetic cellulose microspheres according to claim 1, characterized in that: The weight ratio of the magnetic Fe3O4 to the cellulose solution is 0.5-1:2-4.

6. The method for preparing Ni-carboxylate magnetic cellulose microspheres according to claim 1, characterized in that: The concentration of the NiSO4 solution is 0.4M-0.6M, and the amount of the NiSO4 solution added per gram of carboxylic acid magnetic cellulose microspheres is 35ml-50ml.

7. The method for preparing Ni-carboxylate magnetic cellulose microspheres according to claim 1, characterized in that: When dissolving, precool at -12°C to -15°C for 15 minutes, then swell the carboxylated cellulose at a stirring speed of 300 to 500 r / min, and dissolve at a stirring speed of 3000 r / min for 15 to 30 minutes.

8. The method for preparing Ni-carboxylate magnetic cellulose microspheres according to claim 1, characterized in that: The ratio of the amount of Span80, Tween 80 and liquid paraffin is 1-5:1-3:100-200 respectively; After the mixture is put into the emulsification system, the stirring temperature is 25° C. to 45° C., the stirring speed is 500 r / min to 1000 r / min, and the stirring time is 120 min to 240 min.

9. The method for preparing Ni-carboxylate magnetic cellulose microspheres according to claim 1, characterized in that: The Ni-carboxylate magnetic cellulose microspheres were washed with SDS solution and ethanol in sequence.

10. A Ni-carboxylate magnetic cellulose microsphere, characterized in that: The Ni-carboxylate magnetic cellulose microspheres are prepared by the preparation method according to any one of claims 1 to 9.