Composite catalyst for synergistically removing NOx and chlorine-containing volatile organic compounds as well as preparation method and application of composite catalyst
By using a composite catalyst composed of Ti elements and non-precious metal elements, combined with precious metal loading and hydrothermal preparation, the problem of synergistic removal of nitrogen oxides and chlorine-containing volatile organic compounds at low temperatures is solved, and efficient flue gas purification effect and suitable effect are achieved. Characteristics of industrial production.
Patent Information
- Application Number
- CN202411111098.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-13
- Publication Date
- 2024-12-06
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
It is difficult for existing catalysts to efficiently remove nitrogen oxides and chlorine-containing volatile organic compounds at low temperatures, and there are problems with poor N2 selectivity and HCl selectivity, which affects the flue gas purification effect.
A composite catalyst is used, which consists of Ti elements and non-precious metal elements, has a one-dimensional tubular nanostructure, and is loaded with precious metal elements on the surface or inside. It is prepared by hydrothermal method, broadening the temperature range of the synergistic reaction and improving catalytic activity.
Efficiently remove NOx and chlorine-containing volatile organic compounds in the temperature range of 100-400°C, improving thermal stability and HCl selectivity, and is suitable for large-scale production and industrial applications.
Smart Images

Figure CN119075969A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a composite catalyst and a preparation method and application thereof, and in particular to a composite catalyst for synergistically and efficiently removing NOx and chlorine-containing volatile organic matter and a preparation method and application thereof, belonging to the field of catalysts. Background Art
[0002] Volatile organic compounds (VOCs) and nitrogen oxides (NOx) are the main precursors of photochemical reactions in the atmosphere, causing atmospheric environmental problems such as smog and ozone pollution. In addition, the two pollutants are often produced by the same pollution sources, such as: municipal solid waste incineration, iron ore sintering, metal smelting and coking, coal-fired power generation in thermal power plants and other processes. The VOCs emitted by these pollution sources involve aromatic organic matter and chlorine-containing organic matter, which pose a serious threat to human health and require strict emission control.
[0003] Flue gas end treatment technology is to install a flue gas denitrification device at the tail end of the flue to convert harmful NOx into harmless substances through chemical or physical reactions. At present, the main technologies used for flue gas denitrification are wet denitrification technology and dry denitrification technology. Wet denitrification mainly uses chemical solutions to absorb nitrogen oxides in flue gas at the tail end of the flue. It is generally divided into oxidation absorption method, alkaline solution absorption method, liquid phase reduction absorption method and liquid phase complex absorption method. However, this technology is prone to secondary pollution and has a low denitrification rate, and has not been widely promoted and applied. Dry denitrification technology mainly includes adsorption method, electron beam method, plasma method, catalytic reduction method and other methods. The reduction method is currently the most widely used due to its high denitrification efficiency and low cost.
[0004] In the denitrification process, the selective catalytic reduction (SCR) low-temperature catalyst can be used to jointly control and reduce the emission of volatile organic pollutants, and this method has high industrial application value. First, the NH3-SCR reaction process has reaction conditions for the simultaneous catalytic combustion of VOCs; second, reducing the emission of multiple pollutants through a single pollutant control unit can save energy and reduce costs, which is conducive to the promotion of technology and the positive cycle of commercialization; third, it has been found that nitrogen oxides and volatile organic compounds can not only affect environmental quality and human health alone, but the two can also react to form haze, ozone and other pollution, which has become increasingly serious in recent years and needs to be solved urgently.
[0005] At present, in the research on catalysts for the synergistic removal of nitrogen oxides and chlorinated volatile organic compounds (CVOCs), the synergistic temperature window of the catalysts is mostly above 300°C, and catalysts with good low-temperature effects often have poor N2 selectivity. Therefore, designing SCR-based synergistic catalysts with good low-temperature synergistic activity and high N2 selectivity is still a research problem. Although CeTi catalysts have good N2 selectivity, they have problems such as high conversion temperature and low mineralization rate for the catalytic oxidation of benzene series. In the synergistic removal of chlorinated volatile organic compounds, in addition to problems such as high synergistic temperature window, there are also problems such as poor HCl selectivity and Cl poisoning.
[0006] Therefore, developing a catalyst that can synergistically and efficiently remove nitrogen oxides and chlorinated volatile organic compounds has become a technical problem that needs to be solved urgently. Summary of the invention
[0007] Problem that the invention aims to solve
[0008] In view of the technical problems existing in the prior art, the present invention first provides a composite catalyst. The composite catalyst of the present invention can efficiently and synergistically remove NOx and chlorinated volatile organic compounds at a temperature of 100 to 400°C, effectively broadening the temperature range of the synergistic reaction of nitrogen oxides and chlorinated volatile organic compounds.
[0009] Furthermore, the present invention also provides a method for preparing a composite catalyst, which is simple and easy to implement, and the raw materials are easy to obtain, and is suitable for mass production.
[0010] Solutions for solving problems
[0011] [1] A composite catalyst, comprising a composite carrier, wherein the composite carrier comprises a Ti element and a first active element, wherein:
[0012] The first active element includes a non-noble metal element of a transition group, and the non-noble metal element does not include Ti element.
[0013] [2] The composite catalyst according to [1] above, wherein the composite catalyst has a one-dimensional tubular nanostructure, and the one-dimensional tubular nanostructure is obtained by composite molding of the Ti element and the first active element;
[0014] Preferably, the molar ratio of the first active element to the Ti element is 0.05-0.25:1.
[0015] [3] The composite catalyst according to [1] or [2] above, wherein the non-precious metal element comprises one or a combination of two or more of cerium, vanadium, manganese, iron and copper.
[0016] [4] The composite catalyst according to any one of [1] to [3] above, wherein the composite catalyst further comprises a second active element supported on the surface and / or inside of the composite carrier, wherein:
[0017] The second active element includes a noble metal element. Preferably, the noble metal element includes one or a combination of two or more of ruthenium, rhodium, palladium and platinum.
[0018] [5] The composite catalyst according to [4] above, wherein the loading amount of the second active element is 5 wt% or less, preferably greater than 0 and less than 2 wt%, based on the total mass of the composite carrier; and / or
[0019] The specific surface area of the composite catalyst is 200 to 400 m 2 / g, pore volume is 0.2~0.6cm 3 / g, and the average pore size is 3 to 8 nm.
[0020] [6] A method for preparing a composite catalyst according to any one of [1] to [5] above, comprising the step of using a hydrothermal method to composite-form the Ti element and the first active element to obtain a composite carrier;
[0021] Preferably, the method for preparing the composite carrier comprises the following steps:
[0022] Dissolving a precursor of the Ti element and a first active element to obtain a precursor solution;
[0023] causing the precursor solution to precipitate and subjecting it to aging treatment to obtain a precipitate;
[0024] calcining the precipitate once to obtain a carrier precursor;
[0025] Under alkaline conditions, the carrier precursor is subjected to a hydrothermal reaction to obtain a hydrothermal reaction product;
[0026] Acidifying the hydrothermal reaction product with an acidic substance to obtain an acidified product;
[0027] The acidified product is subjected to secondary calcination to obtain a composite carrier.
[0028] [7] The preparation method according to [6] above, wherein the preparation process of the composite carrier includes at least one of the following conditions:
[0029] Adjusting the pH value of the precursor solution to 9-11 to cause the precursor solution to precipitate;
[0030] The aging time is 12 to 24 hours;
[0031] The temperature of the first calcination is 400-500°C, and the time of the first calcination is 3-5h;
[0032] The temperature of the hydrothermal reaction is 140 to 180° C., and the time of the hydrothermal reaction is 24 to 48 hours;
[0033] The pH value of the acidified product is 1 to 2;
[0034] The temperature of the secondary calcination is 400-500° C., and the time of the secondary calcination is 3-5 hours.
[0035] [8] The preparation method according to [6] or [7] above, wherein the preparation method further comprises the step of loading the precious metal on the surface and / or inside of the composite carrier by an impregnation method; preferably, the loading comprises the following steps:
[0036] mixing the composite carrier with a solvent to obtain a suspension;
[0037] impregnating a noble metal precursor into the suspension to obtain an impregnation product;
[0038] The solvent in the impregnated product is removed to obtain a composite catalyst.
[0039] [9] The preparation method according to [8] above, wherein the immersion time is 12 to 48 hours; and / or,
[0040] The solvent in the impregnated product is removed by drying. Preferably, the drying temperature is 60-100°C.
[0041]
[10] A use of the composite catalyst according to any one of [1] to [5] above for the simultaneous removal of chlorine-containing volatile organic pollutants and nitrogen oxides; preferably, the removal temperature is 100 to 400°C.
[0042] Effects of the Invention
[0043] The composite catalyst of the present invention can efficiently and synergistically remove NOx and chlorine-containing volatile organic matter at a temperature of 100 to 400° C., effectively broadening the temperature range of the synergistic reaction of NOx and chlorine-containing volatile organic matter. In addition, the composite catalyst of the present invention has the advantages of high thermal stability, high mineralization rate, high HCl selectivity, etc.
[0044] The preparation method of the composite catalyst of the invention is simple and easy, the raw materials are easy to obtain, and it is suitable for mass production.
[0045] The composite catalyst of the present invention can be used for the coordinated removal of multiple pollutants in flue gas, and specifically can be used for the efficient coordinated removal of NOx and chlorine-containing volatile organic compounds. BRIEF DESCRIPTION OF THE DRAWINGS
[0046] Figure 1 This is a SEM analysis image of the composite catalyst prepared in Example 1;
[0047] Figure 2 This is a SEM analysis image of the composite catalyst prepared in Example 3;
[0048] Figure 3 This is a SEM analysis image of the composite catalyst prepared in Example 5;
[0049] Figure 4 TEM analysis diagrams of the composite catalysts prepared in Example 1 and Example 3; wherein the left diagram is Example 1 and the right diagram is Example 3;
[0050] Figure 5 This is a graph showing the activity of the composite catalyst prepared in Example 1 for simultaneously removing nitrogen oxides and chlorine-containing volatile organic compounds;
[0051] Figure 6 This is the activity data diagram of the composite catalyst prepared in Example 2 for simultaneously removing nitrogen oxides and chlorine-containing volatile organic compounds;
[0052] Figure 7 This is a graph showing the activity of the composite catalyst prepared in Example 3 for simultaneously removing nitrogen oxides and chlorine-containing volatile organic compounds;
[0053] Figure 8 This is the activity data diagram of the composite catalyst prepared in Example 4 for simultaneously removing nitrogen oxides and chlorine-containing volatile organic compounds;
[0054] Fig. 9 This is a graph showing the activity of the composite catalyst prepared in Example 5 for simultaneously removing nitrogen oxides and chlorine-containing volatile organic compounds;
[0055] Fig.10 This is a stability data diagram of the composite catalyst prepared in Example 1;
[0056] Fig.11 This is a stability data diagram of the composite catalyst prepared in Example 3;
[0057] Fig.12 The N2 selectivity diagram of the composite catalyst prepared in Example 1, Example 3 and Example 5 for simultaneously removing nitrogen oxides and chlorine-containing volatile organic compounds;
[0058] Fig.13 HCl selectivity diagram for simultaneous removal of nitrogen oxides and chlorine-containing volatile organic compounds by the composite catalysts prepared in Example 1, Example 3 and Example 5. DETAILED DESCRIPTION
[0059] Various exemplary embodiments, features and aspects of the present invention will be described in detail below. The word "exemplary" used here means "used as an example, embodiment or illustrative". Any embodiment described here as "exemplary" is not necessarily interpreted as being superior or better than other embodiments.
[0060] In addition, in order to better illustrate the present invention, numerous specific details are provided in the following specific embodiments. It should be understood by those skilled in the art that the present invention can be implemented without certain specific details. In other examples, methods, means, equipment and steps well known to those skilled in the art are not described in detail in order to highlight the subject matter of the present invention.
[0061] Unless otherwise stated, the units used in this specification are all international standard units, and the numerical values and numerical ranges appearing in the present invention should be understood to include the inevitable systematic errors in industrial production.
[0062] In this specification, the word "may" includes both performing a certain process and not performing a certain process.
[0063] In this specification, the references to "some specific / preferred embodiments", "other specific / preferred embodiments", "embodiments", etc., mean that the specific elements (e.g., features, structures, properties and / or characteristics) described in connection with the embodiments are included in at least one embodiment described herein, and may or may not exist in other embodiments. In addition, it should be understood that the elements may be combined in various embodiments in any suitable manner.
[0064] In this specification, the numerical range expressed using "a numerical value A to a numerical value B" means a range including the endpoints A and B.
[0065] <First aspect>
[0066] The first aspect of the present invention provides a composite catalyst, wherein the composite catalyst comprises a composite carrier, the composite carrier comprises a Ti element and a first active element, wherein:
[0067] The first active element includes a non-noble metal element of a transition group, and the non-noble metal element does not include Ti element.
[0068] The composite catalyst of the present invention can synergistically remove nitrogen oxides and chlorine-containing volatile organic compounds, effectively broadening the synergistic reaction temperature range of nitrogen oxides and chlorine-containing volatile organic compounds. In addition, the composite catalyst of the present invention has the advantages of high thermal stability, high mineralization rate, high HCl selectivity, etc.
[0069] In some specific embodiments, the composite catalyst has a one-dimensional tubular nanostructure. The one-dimensional tubular nanostructure is obtained by composite molding of the Ti element and the first active element. That is, the composite carrier exists in the form of a composite metal oxide and is a one-dimensional tubular nanostructure. The one-dimensional tubular nanostructure further increases the specific surface area of the catalyst, can provide more active sites, enhance the adsorption of reactant molecules, and help improve the conversion rate and selectivity of the catalytic reaction. Due to the advantages of the above structure and performance, the one-dimensional tubular nanostructure has a wide range of application prospects in the treatment of various industrial processes requiring high temperature and high-efficiency catalysis.
[0070] In some specific embodiments, the non-precious metal element includes one or a combination of two or more of cerium, vanadium, manganese, iron, and copper; preferably, the non-precious metal element includes one or a combination of two or more of cerium, vanadium, and manganese.
[0071] In some specific embodiments, the molar ratio of the first active element to the Ti element is 0.05 to 0.25:1, for example, 0.08:1, 0.1:1, 0.12:1, 0.15:1, 0.18:1, 0.2:1, 0.22:1, etc. When the molar ratio of the first active element to the Ti element is too high, the one-dimensional tubular nanostructure is difficult to form.
[0072] In some specific embodiments, in order to make the effect of synergistically removing NOx and chlorine-containing volatile organic compounds more effective, the composite catalyst also includes a second active element loaded on the surface and / or inside of the composite carrier, wherein the second active element includes a noble metal element, preferably, the noble metal element includes one or a combination of two or more of ruthenium, rhodium, palladium, and platinum. The inventors of the present invention have found that the CO2 selectivity and HCl selectivity can be more effectively improved by loading noble metals.
[0073] In some specific embodiments, based on the total mass of the composite support, the loading amount of the second active element is 5wt% or less, preferably greater than 0 and less than 2wt%, for example: 0.1wt%, 0.3wt%, 0.5wt%, 0.7wt%, 0.9wt%, 1wt%, 1.3wt%, 1.5wt%, 1.7wt%, 1.9wt%, 2wt%, 3wt%, 4wt%, etc. In the present invention, the effect of the composite catalyst can be most effectively exerted by introducing extremely low content of precious metal elements.
[0074] In the present invention, the specific surface area of the composite catalyst is 200 to 400 m 2 / g, pore volume is 0.2~0.6cm 3 / g, and the average pore size is 3 to 8 nm.
[0075] <Second Aspect>
[0076] The second aspect of the present invention provides a method for preparing the composite catalyst according to the first aspect of the present invention, which comprises the step of using a hydrothermal method to composite-form the Ti element and the first active element to obtain a composite carrier. In addition, the composite carrier exists in the form of a composite metal oxide and presents a one-dimensional tubular nanostructure. By using the hydrothermal method, the composite catalyst can have a one-dimensional tubular nanostructure.
[0077] In some specific embodiments, the method for preparing the composite carrier comprises the following steps:
[0078] Dissolving a precursor of the Ti element and a precursor of the first active element to obtain a precursor solution;
[0079] Precipitating the precursor solution and performing an aging treatment to obtain a precipitate;
[0080] calcining the precipitate once to obtain a carrier precursor;
[0081] Under alkaline conditions, the carrier precursor is subjected to a hydrothermal reaction to obtain a hydrothermal reaction product;
[0082] Acidifying the hydrothermal reaction product with an acidic substance to obtain an acidified product;
[0083] The acidified product is subjected to secondary calcination to obtain a composite carrier.
[0084] In the present invention, a precursor solution is obtained by dissolving a precursor of the Ti element and a precursor of the first active element. The present invention does not specifically limit the dissolution method, and generally, the precursor of the Ti element and the precursor of the first active element are mixed and dissolved in a solvent. The present invention does not specifically limit the solvent, and it can be any feasible solvent in the art, such as polar solvents such as water. The present invention does not specifically limit the concentration of the precursor of the Ti element and the precursor of the first active element in the precursor solution, as long as they can be dissolved.
[0085] The precursor of the Ti element may generally be a Ti salt, for example, any feasible salt such as titanium sulfate and / or titanium tetrachloride. The precursor of the first active element may generally be a salt containing the first active element.
[0086] Taking the first active element as Ce as an example, the precursor of Ce may be a cerium salt, such as one or a combination of two or more of cerium nitrate, cerium sulfate, cerium chloride, etc. Taking the first element as V as an example, the precursor of V may be a vanadium salt, such as one or a combination of two or more of ammonium metavanadate, vanadyl oxalate, and vanadyl sulfate, etc. For other feasible first active elements, their precursors may be any feasible salts, which will not be described in detail in the present invention.
[0087] Further, the precursor solution is precipitated and aged to obtain a precipitate; specifically, the precursor solution is precipitated using an alkaline substance and aged to obtain a precipitate. The alkaline substance is generally a weak alkaline substance, such as ammonia water.
[0088] Specifically, by using an alkaline substance to adjust the pH value of the precursor solution to 9 to 11, for example, 9.5, 10, 10.5, etc., the precursor solution will produce a precipitate, and then continue to perform an aging treatment to obtain a precipitate. Preferably, the aging treatment time is 12 to 24 hours, for example, 14 hours, 16 hours, 18 hours, 20 hours, 22 hours, etc.
[0089] Further, the precipitate is calcined once to obtain a carrier precursor; specifically, before the precipitate is calcined once, the precipitate may be subjected to at least one of related treatments such as washing, drying, rolling and screening. Specifically, the washing may be performed using any feasible polar solvent, such as water. The drying may be performed at a temperature of 80 to 120°C.
[0090] Furthermore, in the present invention, the primary calcination temperature is 400-500° C., such as 420° C., 450° C., 480° C., etc., and the primary calcination time is 3-5 h, such as 3.5 h, 4 h, 4.5 h, etc. A carrier precursor can be obtained by primary calcination.
[0091] Further, under alkaline conditions, the carrier precursor is subjected to a hydrothermal reaction to obtain a hydrothermal reaction product. The carrier precursor is subjected to a hydrothermal reaction by using an alkaline substance, preferably a strong alkaline substance. The invention does not specifically limit the strong alkaline substance, and it may be NaOH, KOH, etc.
[0092] Furthermore, some surfactants may be added to the hydrothermal reaction system to play a certain dispersing role, such as hexadecyltrimethylammonium bromide (CTAB).
[0093] Specifically, the carrier precursor and the alkaline substance are mixed evenly in a polytetrafluoroethylene liner and placed in a reactor for hydrothermal reaction. The mixing method can be ultrasonic and / or stirring. Preferably, ultrasonic treatment can be performed for 10 to 60 minutes, and then stirring can be performed for 0.5 to 1.5 hours. It should be noted that during the hydrothermal treatment, a certain amount of autogenous pressure will be generated during the reaction process. There is no need to vent the pressure, and the hydrothermal reaction can be directly performed.
[0094] Specifically, the temperature of the hydrothermal reaction is 140-180°C, for example, 150°C, 160°C, 170°C, etc.; the time of the hydrothermal reaction is 24-48h, for example, 28h, 32h, 36h, 40h, 44h, etc.
[0095] In addition, in the hydrothermal reaction system, the concentration of the surfactant can be 0.01-0.1 mol / L, for example: 0.02 mol / L, 0.05 mol / L, 0.08 mol / L, etc.; the alkaline substance used can be added to the hydrothermal reaction system in the form of an alkaline substance solution, wherein the concentration of the alkaline substance solution is 6-12 mol / L, for example: 7 mol / L, 8 mol / L, 9 mol / L, 10 mol / L, 11 mol / L, etc.; the added amount can be 20-70 mL, for example: 30 mL, 40 mL, 50 mL, 60 mL, etc.
[0096] Further, the hydrothermal reaction product is subjected to an acidification treatment using an acidic substance to obtain an acidified product; specifically, the hydrothermal reaction product can be washed using a strong acidic substance to adjust the pH value of the hydrothermal reaction product to 1 to 2, thereby obtaining an acidified product. In the present invention, the acidification process is a process for forming a one-dimensional tubular nanostructure, and the acid sites of the one-dimensional tubular nanostructure can be increased by adjusting the pH value using a strong acidic substance. The present invention does not specifically limit the strong acidic substance, and specifically it can be nitric acid, sulfuric acid, hydrochloric acid, etc.
[0097] Further, the acidified product is subjected to secondary calcination to obtain a composite carrier. Specifically, the temperature of the secondary calcination is 400-500°C, for example: 420°C, 450°C, 480°C, etc.; the time of the secondary calcination is 3-5h, for example: 3.5h, 4h, 4.5h, etc. Preferably, before the secondary calcination, the acidic product can be subjected to relevant treatments such as washing and / or drying. Specifically, the washing can be carried out using any feasible polar solvent, and the acidic product can be made neutral by washing. The polar solvent can be water, an alcohol solvent, etc. Drying can be carried out at a temperature of 60-100°C.
[0098] In some specific embodiments, the preparation method further comprises the step of loading the noble metal on the surface and / or inside of the composite support by impregnation. The present invention can load a small amount of noble metal on the surface and / or inside of the composite support by impregnation.
[0099] Specifically, the loading may include the following steps:
[0100] mixing the composite carrier with a solvent to obtain a suspension;
[0101] impregnating a noble metal precursor into the suspension to obtain an impregnation product;
[0102] The solvent in the impregnated product is removed to obtain a composite catalyst.
[0103] Specifically, the composite carrier and the solvent are mixed evenly to obtain a suspension; the mixing method can be ultrasonic and / or stirring. Preferably, the ultrasonic treatment can be performed for 1 to 30 minutes, and then stirring can be performed for 1 to 30 minutes. The present invention does not specifically limit the solvent, and it can be any feasible solvent in the art, such as polar solvents such as water.
[0104] Further, the noble metal precursor is impregnated in the suspension to obtain an impregnated product. Specifically, the impregnation time is 12 to 48 hours, for example: 18 hours, 24 hours, 30 hours, 36 hours, 42 hours, etc.
[0105] The present invention does not specifically limit the precious metal precursor. In the present invention, the precious metal precursor can be selected from one or more of platinum nitrate, platinum tetrachloride, chloroplatinic acid, platinum acetate, platinum oxalate, platinum bromide, palladium nitrate, palladium chloride, palladium sulfate, palladium acetate, palladium oxalate, palladium dibromide, ruthenium nitrosyl nitrate, ruthenium trichloride, ruthenium sulfate, ruthenium acetate, ruthenium oxalate, ruthenium bromide, rhodium nitrate, rhodium chloride, rhodium sulfate, rhodium acetate, potassium trioxalate rhodium, rhodium bromide and their hydrates.
[0106] In the present invention, the solvent in the impregnated product may be removed by drying, and preferably, the drying temperature is 60-100° C. Finally, after rolling and screening, a composite catalyst is obtained.
[0107] <Third Aspect>
[0108] The third aspect of the present invention provides a use of the composite catalyst according to the first aspect of the present invention for simultaneously removing chlorine-containing volatile organic pollutants and nitrogen oxides; preferably, the removal temperature is 100-400°C, preferably 275-350°C, and more preferably 300-350°C.
[0109] Specifically, the composite catalyst is placed in the exhaust gas pipeline after dust removal, and a reducing agent is sprayed upstream of the composite catalyst to mix with the exhaust gas; the catalytic removal reaction gas hourly velocity is 30000-120000 ml / (g·h). The exhaust gas is a gas containing NOx and chlorine-containing volatile organic matter discharged from a fixed source or a mobile source. Preferably, the reducing agent is ammonia, and the amount of the reducing agent is 1.0-1.2 times the NOx in the exhaust gas.
[0110] Example
[0111] The embodiments of the present invention will be described in detail below in conjunction with the examples, but those skilled in the art will appreciate that the following examples are only used to illustrate the present invention and should not be considered to limit the scope of the present invention. If no specific conditions are specified in the examples, they are carried out according to normal conditions or the conditions recommended by the manufacturer. If the manufacturer is not specified for the reagents or instruments used, they are all conventional products that can be obtained commercially.
[0112] Example 1
[0113] (1) Preparation of carrier precursor
[0114] According to the molar ratio of n(Ce):n(Ti) in the final sample of 0.125:1, cerium nitrate (Ce(NO3)3) and titanium sulfate (Ti(SO4)2) were weighed and added to deionized water, and stirred continuously for 1 hour at room temperature using a magnetic stirrer until fully dissolved to form a precursor solution. Ammonia water was slowly added dropwise to the precursor solution and stirred continuously until the pH value of the solution reached 10 and a precipitate appeared. After aging at room temperature for 12 hours, the obtained precipitate was washed with deionized water until neutral, and then dried at 100°C for 12 hours, rolled and sieved, and calcined at 400°C for 5 hours to obtain a dark yellow powder, which is the carrier precursor.
[0115] (2) Preparation of composite carrier
[0116] 2g of carrier precursor, 0.5832g of hexadecyltrimethylammonium bromide (CTAB), and 40ml of NaOH solution (10mol / L) were transferred to a polytetrafluoroethylene liner, and after ultrasonic treatment for 30min, they were transferred to a magnetic stirrer and stirred for 1h to mix evenly, and then placed in a stainless steel reactor and allowed to stand at 150°C for 24h to form crystals to obtain a hydrothermal treatment product. After the hydrothermal reaction is completed, the hydrothermal treatment product is taken out and cooled at room temperature, first washed with dilute nitric acid to a pH of about 1.6, then repeatedly washed with deionized water and anhydrous ethanol to neutrality, then dried at 80°C for 12h, and finally calcined at 400°C for 3h to obtain a composite carrier, which is the composite catalyst of this embodiment, recorded as CeTiNTs.
[0117] Example 2
[0118] (1) Preparation of carrier precursor
[0119] According to the molar ratio of n(Ce):n(Ti) in the final sample of 0.125:1, cerium nitrate (Ce(NO3)3) and titanium sulfate (Ti(SO4)2) were weighed and added to deionized water, and stirred continuously for 1 hour at room temperature using a magnetic stirrer until fully dissolved to form a precursor solution. Ammonia water was slowly added dropwise to the precursor solution and stirred continuously until the pH value of the solution reached 10 and a precipitate appeared. After aging at room temperature for 12 hours, the obtained precipitate was washed with deionized water until neutral, and then dried at 100°C for 12 hours, rolled and sieved, and calcined at 400°C for 5 hours to obtain a dark yellow powder, that is, a carrier precursor.
[0120] (2) Preparation of composite carrier
[0121] 2g of carrier precursor, 0.5832g of CTAB, and 40ml of NaOH solution (10mol / L) were transferred to a polytetrafluoroethylene liner, and after ultrasonic treatment for 30min, they were transferred to a magnetic stirrer and stirred for 1h to mix evenly, and then placed in a stainless steel reactor and allowed to stand at 150°C for 24h to form crystals to obtain a hydrothermal treatment product. After the hydrothermal reaction was completed, the hydrothermal treatment product was taken out and cooled at room temperature, first washed with dilute nitric acid to a pH of about 1.6, then repeatedly washed with deionized water and anhydrous ethanol to neutrality, then dried at 80°C for 12h, and finally calcined at 400°C for 3h to obtain a bright yellow powder, i.e., a composite carrier.
[0122] (3) Loading of precious metals
[0123] 1 g of the composite carrier was added to deionized water, and after ultrasonic treatment for 15 min, it was transferred to a magnetic stirrer and stirred for 15 min until uniform. 0.033 mL of trinitronitrosylruthenium (III) solution (ruthenium 1.5% W / V) was added dropwise to the above suspension to make the Ru loading amount 0.05 wt% based on the total mass of the composite carrier. The mixture was stirred at room temperature for 24 h, and then placed in an electric oven at 80°C to evaporate the liquid. The composite catalyst loaded with precious metals was crushed and sieved to obtain 0.05% Ru / CeTiNTs.
[0124] Example 3
[0125] The loading amount of Ru in Example 2 was adjusted to 0.1 wt %, and the rest was exactly the same as in Example 2, to prepare a composite catalyst loaded with precious metals, which was recorded as 0.1% Ru / CeTiNTs.
[0126] Example 4
[0127] The loading amount of Ru in Example 2 was adjusted to 0.2 wt %, and the rest was exactly the same as Example 2, to prepare a composite catalyst loaded with precious metals, which was recorded as 0.2% Ru / CeTiNTs.
[0128] Example 5
[0129] The loading amount of Ru in Example 2 was adjusted to 0.5 wt %, and the rest was exactly the same as Example 2, to prepare a composite catalyst loaded with precious metals, which was recorded as 0.5% Ru / CeTiNTs.
[0130] Performance Testing
[0131] 1. ICP detection
[0132] The metal element contents of the composite catalysts of Example 1 and Example 3 were detected by ICP. The results are shown in Table 1 below.
[0133] Table 1
[0134]
[0135] It can be seen from Table 1 that the composite catalyst of Example 1 of the present invention contains Ce and Ti elements, and the composite catalyst of Example 3 contains Ce, Ti and Ru elements.
[0136] 2. Tests on specific surface area, pore volume, average pore diameter, etc.
[0137] The specific surface area, pore volume and average pore size of the composite catalyst were tested using a physical adsorption instrument (Michiko Baier, Japan). The specific surface area was calculated by the Brunauer-Emmett-Teller (BET) method, the pore volume was calculated by the non-local density functional theory (NLDFT) method, and the average pore size was calculated by pore size distribution (BJH).
[0138] Table 2
[0139]
[0140] It can be seen from Table 2 that by loading precious metals, its specific surface area, pore volume and average pore diameter are reduced, but its catalytic performance is not affected, and the CO2 selectivity is greatly improved.
[0141] 3. Simultaneous removal activity test of NOx and chlorobenzene
[0142] The composite catalysts of Examples 1-5 were crushed and sieved to 40-60 meshes, and 0.1 g was weighed and placed in a fixed-bed quartz tube reactor. The conversion and selectivity of the corresponding substances of the samples were tested at 200-350° C. using Gasmet DX4000 in a simulated flue gas atmosphere (NOx: 500 ppm, NH3: 500 ppm, chlorobenzene: 50 ppm, O2: 5 vol%, and the rest was N2). The total gas flow rate was 100 mL / min (space velocity SV=60000 mL g -1 h -1 ), the result is as follows Figure 5-9 shown.
[0143] Figure 5-9 The degradation and denitration performance test diagrams of the composite catalysts for the synergistic and efficient removal of NOx and chlorine-containing volatile organic compounds prepared in Examples 1-5 are shown in Figure 1. It can be seen from the figure that at 60000 mL g -1 h -1 At a space velocity of 1.5 ℃, the catalysts prepared in Examples 1-5 all showed excellent performance in simultaneously removing NOx and chlorobenzene, and their effective degradation temperature range was 300-350° C. Example 1 had good catalytic activity, but poor CO2 selectivity. The CO2 selectivity of the catalyst was greatly improved after Ru loading.
[0144] In addition, by Fig.12 and Fig.13 It can be seen that only a small amount of N2O is generated in the test process of Example 1, Example 3 and Example 5, which have excellent N2 selectivity. After the composite carrier is loaded with Ru, the selectivity of HCl is improved to varying degrees.
[0145] 4. Stability test of simultaneous removal of NOx and chlorobenzene
[0146] The catalysts of Example 1 and Example 3 were crushed and sieved to 40-60 meshes, and 0.1 g was weighed and placed in a fixed-bed quartz tube reactor. The samples were continuously reacted at 300° C. for 10 h to determine the conversion and selectivity of the corresponding substances using Gasmet DX4000 in a simulated flue gas atmosphere (NOx: 500 ppm, NH3: 500 ppm, chlorobenzene: 50 ppm, O2: 5 vol%, and the rest was N2). The total gas flow rate was 100 mL / min (space velocity SV=60000 mL g -1 h -1 ), the result is as follows Fig.10 and Fig.11 shown.
[0147] Fig.10 The stability test results of the composite catalyst of Example 1 under the condition of continuous reaction at 300°C for 10 hours. Fig.11The stability test results of the composite catalyst of Example 3 under the condition of continuous reaction at 300°C for 10 hours are as follows: Fig.10 and 11 It can be seen that the catalyst prepared by the present invention can still maintain long-term stability under complex flue gas conditions and has good industrial application prospects.
[0148] It should be noted that, although the technical solution of the present invention is introduced with specific examples, those skilled in the art will appreciate that the present invention should not be limited thereto.
[0149] The embodiments of the present invention have been described above, and the above description is exemplary, not exhaustive, and is not limited to the disclosed embodiments. Many modifications and variations will be apparent to those of ordinary skill in the art without departing from the scope and spirit of the described embodiments. The selection of terms used herein is intended to best explain the principles of the embodiments, practical applications, or technical improvements in the market, or to enable other persons of ordinary skill in the art to understand the embodiments disclosed herein.
Claims
1. A composite catalyst, characterized in that: The composite catalyst comprises a composite carrier, wherein the composite carrier comprises a Ti element and a first active element, wherein: The first active element includes a non-noble metal element of a transition group, and the non-noble metal element does not include Ti element.
2. The composite catalyst according to claim 1, characterized in that The composite catalyst has a one-dimensional tubular nanostructure, and the one-dimensional tubular nanostructure is obtained by composite molding of the Ti element and the first active element; Preferably, the molar ratio of the first active element to the Ti element is 0.05-0.25:
1.
3. The composite catalyst according to claim 1 or 2, characterized in that The non-precious metal elements include one or a combination of two or more of cerium, vanadium, manganese, iron and copper.
4. The composite catalyst according to any one of claims 1 to 3, characterized in that The composite catalyst further includes a second active element supported on the surface and / or inside of the composite carrier, wherein: The second active element includes a noble metal element. Preferably, the noble metal element includes one or a combination of two or more of ruthenium, rhodium, palladium and platinum.
5. The composite catalyst according to claim 4, characterized in that Based on the total mass of the composite carrier, the loading amount of the second active element is 5 wt% or less, preferably greater than 0 and less than 2 wt%; and / or, The specific surface area of the composite catalyst is 200 to 400 m 2 / g, pore volume is 0.2~0.6cm 3 / g, and the average pore size is 3 to 8 nm.
6. A method for preparing a composite catalyst according to any one of claims 1 to 5, characterized in that: The method comprises the steps of using a hydrothermal method to composite the Ti element and the first active element to obtain a composite carrier; Preferably, the method for preparing the composite carrier comprises the following steps: Dissolving a precursor of the Ti element and a first active element to obtain a precursor solution; causing the precursor solution to precipitate and subjecting it to aging treatment to obtain a precipitate; calcining the precipitate once to obtain a carrier precursor; Under alkaline conditions, the carrier precursor is subjected to a hydrothermal reaction to obtain a hydrothermal reaction product; Acidifying the hydrothermal reaction product with an acidic substance to obtain an acidified product; The acidified product is subjected to secondary calcination to obtain a composite carrier.
7. The preparation method according to claim 6, characterized in that: The preparation process of the composite carrier includes at least one of the following conditions: Adjusting the pH value of the precursor solution to 9-11 to cause the precursor solution to precipitate; The aging time is 12 to 24 hours; The temperature of the first calcination is 400-500°C, and the time of the first calcination is 3-5h; The temperature of the hydrothermal reaction is 140 to 180° C., and the time of the hydrothermal reaction is 24 to 48 hours; The pH value of the acidified product is 1 to 2; The temperature of the secondary calcination is 400-500° C., and the time of the secondary calcination is 3-5 hours.
8. The preparation method according to claim 6 or 7, characterized in that: The preparation method further comprises the step of loading the noble metal on the surface and / or inside of the composite carrier by an impregnation method; preferably, the loading comprises the following steps: mixing the composite carrier with a solvent to obtain a suspension; impregnating a noble metal precursor into the suspension to obtain an impregnation product; The solvent in the impregnated product is removed to obtain a composite catalyst.
9. The preparation method according to claim 8, characterized in that: The immersion time is 12 to 48 hours; and / or, The solvent in the impregnated product is removed by drying. Preferably, the drying temperature is 60-100°C.
10. Use of the composite catalyst according to any one of claims 1 to 5 for simultaneously removing chlorine-containing volatile organic pollutants and nitrogen oxides; preferably, the removal temperature is 100-400°C.
Citation Information
Patent Citations
Preparation method of Ru / CeTiOX catalyst for low-temperature SCR (selective catalytic reduction) reaction
CN106732581A
Catalyst for low-temperature catalytic burning of chlorobenzene and preparation method and application thereof
CN107670658A
Catalyst for low temperature high efficient catalytic VOCs exhaust gas degradation and preparation method thereof
CN108671917A
Catalyst for synergistically removing NOx and CVOCs as well as preparation method and application of catalyst
CN113786828A
Catalyst for concerted catalytic purification of NOx and CVOCs as well as preparation method and application of catalyst
CN117258816A
Cited By
Catalytic combustion catalyst for treating CVOCs as well as preparation method and application of catalytic combustion catalyst
CN119702025A