Supported metal catalyst as well as preparation method and application thereof

By impregnating active metals such as Cu, Zn and Ni on the mesoporous carbon support, a supported metal catalyst was prepared, which solved the complex and costly catalyst preparation problems in the prior art, and significantly improved the acquisition of N-methylmorpholine and raw material utilization rate, suitable for industrial production.

CN119075996APending Publication Date: 2024-12-06MEISIDE (JILIN) NEW MATERIAL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411225278.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-03
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

In the prior art, the catalyst preparation process used for the methylation reaction of morpholine and methanol is complicated and expensive, resulting in high production cost of N-methylmorpholine and low yield, and the raw materials cannot be fully utilized.

Method used

Using mesoporous carbon as a support, the active metals such as Cu, Zn and Ni were loaded through the impregnation method to prepare a supported metal catalyst, which simplifies the preparation process and reduces the cost.

Benefits of technology

The yield of N-methylmorpholine and the conversion rate of morpholine raw materials are improved, and the production cost is reduced. It is suitable for the industrial production of N-methylmorpholine.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005024307240000161
    Figure BDA0005024307240000161
Patent Text Reader

Abstract

The invention discloses a supported metal catalyst as well as a preparation method and application thereof, and relates to the technical field of organic synthesis. The supported metal catalyst comprises a mesoporous carbon carrier and active metal supported on the mesoporous carbon carrier. The preparation method of the supported metal catalyst is simple, and raw materials are cheap and easily available. The supported metal catalyst has good catalytic activity and stability, and can significantly improve the conversion rate of the raw material morpholine and the yield of the product N-methylmorpholine.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of organic synthesis, and in particular to a supported metal catalyst and a preparation method and application thereof. Background Art

[0002] At present, the most common production method of N-methylmorpholine is to carry out methylation reaction with morpholine and methanol as raw materials. The catalyst used in the methylation reaction of morpholine and methanol in the prior art is usually a supported metal catalyst, the carrier of this type of catalyst is generally a metal oxide, and the active metal content of the load is higher, the preparation process of the catalyst is complicated, expensive, resulting in the overall production cost of N-methylmorpholine is higher. In addition, the yield of N-methylmorpholine obtained by this type of catalyst is low, and the raw material fails to be fully utilized.

[0003] In view of this, the present invention is proposed. Summary of the invention

[0004] The purpose of the present invention is to provide a supported metal catalyst and a preparation method and application thereof to solve the above technical problems.

[0005] The present invention is achieved in that:

[0006] In a first aspect, an embodiment of the present invention provides a supported metal catalyst, which includes a carrier and an active metal supported on the carrier; the carrier includes mesoporous carbon, and the active metal includes at least one of Cu element, Zn element, Ni element and Cr element.

[0007] In a second aspect, an embodiment of the present invention provides a method for preparing a supported metal catalyst as described above, the method comprising: using an impregnation method to load an active metal on mesoporous carbon to prepare a supported metal catalyst.

[0008] In a third aspect, an embodiment of the present invention provides a use of the aforementioned supported metal catalyst or the supported metal catalyst prepared by the aforementioned preparation method in the preparation of N-methylmorpholine.

[0009] The present invention has the following beneficial effects:

[0010] The supported metal catalyst provided by the embodiment of the present invention is based on mesoporous carbon as a carrier, and the mesoporous carbon material has dense and evenly distributed pores, and has the characteristics of large specific surface area; the active metal in the supported metal catalyst has good dispersibility on the carrier, and the preparation process of the supported metal catalyst is simple, the raw materials are cheap and easy to obtain, and the production cost is low. The supported metal catalyst of the present invention has excellent catalytic activity and stability, can significantly improve the yield of N-methylmorpholine and the conversion rate of morpholine raw materials, and is conducive to the industrial production of N-methylmorpholine. DETAILED DESCRIPTION

[0011] In order to make the purpose, technical scheme and advantages of the embodiments of the present invention clearer, the technical scheme in the embodiments of the present invention will be described clearly and completely below. If the specific conditions are not specified in the embodiments, they are carried out according to conventional conditions or conditions recommended by the manufacturer. If the manufacturer of the reagents or instruments used is not specified, they are all conventional products that can be purchased commercially.

[0012] N-methylmorpholine is an important fine chemical raw material, mainly used as a catalyst, corrosion inhibitor, extractant and rubber accelerator for polyurethane foam materials. It is also an important intermediate for the synthesis of emulsifiers, medicines, fiber treatment agents and surfactants.

[0013] According to the classification of raw materials in the synthesis route, the preparation methods of N-methylmorpholine mainly include: methylation method of morpholine, formaldehyde and formic acid; N-methyldiethanolamine method; methylation method of morpholine and methyl chloride. These methods are not conducive to the industrial production of N-methylmorpholine, and the reaction process is complicated, the by-products are difficult to control, the production efficiency is low, and the production cost is high.

[0014] The catalyst used in the methylation reaction of morpholine and methanol in the prior art has a complicated preparation process and is expensive, resulting in a high overall production cost of N-methylmorpholine. The present invention provides a process with a simple preparation process and low cost, and the catalyst prepared by the process is conducive to the industrial production of N-methylmorpholine, and improves the yield of N-methylmorpholine while improving the utilization rate of raw materials, so as to solve the above technical problems.

[0015] In a first aspect, an embodiment of the present invention provides a supported metal catalyst, which includes a carrier and an active metal supported on the carrier; the carrier includes mesoporous carbon, and the active metal includes at least one of Cu element, Zn element, Ni element and Cr element.

[0016] It should be noted that mesoporous carbon, as a new type of non-silicon-based mesoporous material, has dense and evenly distributed pores and a large specific surface area. It has broad application potential and value as a carrier.

[0017] Metal active ions have a specific electronic structure, which can adjust the electronic distribution state of reactant molecules, change the reactivity of reactant molecules, and reduce the activation energy of the reaction. In addition, metal active ions can adsorb reactant molecules and strengthen the interaction between reactants and supported metal catalysts, reduce the repulsion between reactant molecules, and increase the effective collision rate of reactants, thereby increasing the reaction rate.

[0018] In an optional embodiment of the present invention, the active metal includes at least one of Cu element, Zn element and Ni element.

[0019] In a preferred embodiment of the present invention, the active metal comprises Cu, Zn and Ni elements at the same time. The use of the above specific active metals can ensure that the supported metal catalyst has good catalytic performance under relatively low active metal loading.

[0020] Specifically, by mass fraction, the mass of the Cu element accounts for 10%-18% of the mass of the supported metal catalyst; the mass of the Zn element accounts for 4%-7% of the mass of the supported metal catalyst; and the mass of the Ni element accounts for 1%-3% of the mass of the supported metal catalyst.

[0021] It should be noted that controlling the loading amount of each metal within a certain range can more effectively ensure the stability and activity of the supported metal catalyst, and its application in the production of N-methylmorpholine is beneficial to improving the yield of N-methylmorpholine and the conversion rate of morpholine raw materials.

[0022] In a second aspect, an embodiment of the present invention provides a method for preparing a supported metal catalyst as described above, the method comprising: using an impregnation method to load an active metal on mesoporous carbon to prepare a supported metal catalyst.

[0023] It should be noted that the mesoporous carbon used in the present invention is prepared by the inventors and has the following characteristics: very fine particles and a large specific surface area.

[0024] In an optional embodiment of the present invention, the preparation of mesoporous carbon comprises the following steps:

[0025] The organic precursor and the acid solution are mixed and then heated; the heated product is washed until the pH of the washing liquid is 6-7, and the washed product is dried to obtain mesoporous carbon; the mass ratio of the organic precursor to the acid solution is 1:(6-8).

[0026] In an optional embodiment of the present invention, the heating treatment includes a first heating stage and a second heating stage; the temperature of the first heating stage is 150℃-180℃, and the time is 0.5h-1h; the temperature of the second heating stage is 600℃-700℃, and the time is 1h-2h.

[0027] It should be noted that the organic precursor and the acid solution are heated in an inert atmosphere to reduce the oxygen content in the environment, provide a stable environment for the reaction, and make the mesoporous carbon obtained after the reaction have uniform pores and a large specific surface area. The present invention does not particularly limit the inert gas. The inert gas used in the embodiment of the present invention is nitrogen. In other embodiments of the present invention, inert gases such as argon and helium can be selected according to actual needs.

[0028] The main purpose of using staged heating is to control the temperature to gradually increase and optimize the structure and performance of the organic precursor. In order to prevent the pores of the organic precursor from becoming irregular due to the sudden increase in temperature during the heating process, staged heating can ensure that the mesoporous carbon has uniform and dense pores and a large specific surface area.

[0029] In an optional embodiment of the present invention, the organic precursor is selected from any one of wood powder and sucrose; the acid solution is selected from any one of phosphoric acid aqueous solution and hydrochloric acid aqueous solution.

[0030] Furthermore, the organic precursor is wood powder, and the acid solution is a phosphoric acid aqueous solution.

[0031] It should be noted that the organic precursor is wood powder because wood powder is a biomass raw material with a wide source and is cheap and easy to obtain. The main function of the acid solution is to pretreat the wood powder so that it can easily form a porous structure. The acid solution of the present invention is a phosphoric acid aqueous solution.

[0032] In an optional embodiment of the present invention, the mass fraction of phosphoric acid in the phosphoric acid aqueous solution is 25%-35% by mass fraction.

[0033] In an optional embodiment of the present invention, the organic precursor is added to an acid solution for immersion treatment, the immersion temperature is 30°C-50°C, and the immersion time is 2h-4h; it should be noted that the main function of the immersion treatment is to make the wood powder eventually form a porous material with a larger specific surface area.

[0034] In an optional embodiment of the present invention, the washed product is dried in a drying oven; the drying temperature is 100°C-110°C, the pressure is -0.09MPa to -0.10MPa, and the time is 18h-24h.

[0035] It should be noted that the present invention does not specifically limit the drying equipment. In an embodiment of the present invention, drying is carried out in a vacuum drying oven, and the pressure of the vacuum drying oven needs to be controlled to be -0.09 MPa to -0.1 MPa. This operation provides a controllable vacuum environment for drying, achieving rapid drying while ensuring the stability of the object to be dried.

[0036] Specifically, the preparation of mesoporous carbon in the embodiment of the present invention is as follows:

[0037] Wood powder is added to a phosphoric acid aqueous solution and soaked for a period of time, and then the mixture is slowly heated to the first heating stage in a nitrogen atmosphere and kept warm for a period of time, and then the temperature is continued to be raised to the second heating stage and kept warm for a period of time, and the heated product is washed until the pH of the washing liquid is 6-7, and placed in a vacuum drying oven to dry, so as to obtain a mesoporous carbon carrier.

[0038] It should be noted that the mesoporous carbon carrier prepared by the above method has uniform and dense pore distribution and a large specific surface area. The heated product is washed to make it nearly neutral to avoid the subsequent impact on the conversion rate of morpholine and the yield of N-methylmorpholine.

[0039] In an optional embodiment of the present invention, the preparation of the supported metal catalyst comprises the following steps:

[0040] The active metal salt and mesoporous carbon are immersed in water to obtain a mixed solution; the mixed solution is dried, and the dried product is ground and roasted to obtain a supported metal catalyst; wherein the mass ratio of the active metal salt, water and mesoporous carbon is (0.72-1.6):6:1.

[0041] It should be noted that water can be selected from deionized water, purified water, ultrapure water, etc. according to actual needs. The active metal is loaded on the mesoporous carbon carrier by the impregnation method, so that the active metal has good dispersion on the carrier, and then the prepared supported metal catalyst has excellent performance.

[0042] In an optional embodiment of the present invention, the immersion treatment temperature is 50°C-70°C, the time is 6h-10h, and the mixed liquid drying treatment temperature is 90°C-100°C, the pressure is -0.09MPa to -0.10MPa, and the time is 18h-24h.

[0043] It should be noted that the impregnation treatment is mainly to enable the active metal to be loaded on the mesoporous carbon in a highly dispersed form, and the temperature and time of the impregnation treatment can be reasonably adjusted according to the actual amount of sample to be processed.

[0044] The specific values ​​of the temperature and time for the drying of the mixed solution can be reasonably adjusted according to the actual amount of sample to be processed.

[0045] The purpose of grinding is to reduce the particle size of the dried material, enhance uniformity and specific surface area, and facilitate the subsequent roasting process.

[0046] In an optional embodiment of the present invention, the calcination temperature is 400° C.-500° C., and the calcination time is 2 h-4 h.

[0047] The purpose of roasting is to evenly disperse the active metal on the carrier to form catalytic active sites. The roasting equipment selected in the embodiment of the present invention is a muffle furnace, mainly because the muffle furnace uses advanced electric heating elements and a temperature control system that can accurately control the heating temperature and constant temperature time of the material, ensuring that the temperature fluctuation is small during the experiment or production process, and then ensuring that the material is heated evenly during the heating process to avoid overheating or local temperature unevenness; its high thermal conversion rate can quickly heat the material to a high temperature, greatly shortening the heating time, improving production efficiency and energy utilization efficiency, and helping to obtain better heating effects and product quality. In other embodiments of the present invention, other suitable roasting equipment can be selected according to actual needs.

[0048] In an optional embodiment of the present invention, the salt of the active metal is selected from any one of an active metal chloride, an active metal sulfate and an active metal nitrate.

[0049] It should be noted that the salt of the active metal is a soluble salt, which can be completely dissolved in an aqueous solution, which is conducive to the active metal being well loaded on the carrier. In other embodiments of the present invention, other soluble salts of the active metal can be selected according to actual needs. In addition, the salts of the active metal Cu element, Zn element and Ni element can also be selected from the same category or different categories of substances according to actual needs, such as cupric chloride, zinc nitrate and nickel sulfate, copper nitrate, zinc nitrate and nickel nitrate, copper sulfate, zinc sulfate and nickel nitrate, etc.

[0050] In an optional embodiment of the present invention, the salts of active metals are all active metal nitrates.

[0051] The mass ratio of active metal nitrates is (0.45-0.95):(0.21-0.44):(0.06-0.21) of Cu(NO3)2·3H2O, Zn(NO3)2·6H2O and Ni(NO3)2·6H2O.

[0052] When the ratio is within this range, the synergistic effect of the three active metals enables the supported metal catalyst to have the best catalytic performance. If it exceeds this range, the catalytic performance of the supported metal catalyst will decrease.

[0053] In a third aspect, an embodiment of the present invention provides a use of the aforementioned supported metal catalyst or the supported metal catalyst prepared by the aforementioned preparation method in the preparation of N-methylmorpholine.

[0054] In an optional embodiment of the present invention, the preparation of N-methylmorpholine comprises the following steps:

[0055] In a reducing gas atmosphere, a supported metal catalyst, morpholine and methanol are subjected to a methylation reaction;

[0056] It should be noted that, before the supported metal catalyst is subjected to the methylation reaction, the supported metal catalyst is activated and reduced.

[0057] The activation reduction of the supported metal catalyst includes: adding the supported metal catalyst into a fixed bed, replacing the air in the fixed bed with nitrogen, and in a nitrogen atmosphere, heating up in stages and introducing reducing gas to completely replace the nitrogen with reducing gas; during the activation and reduction, the pressure is controlled to be 0.15MPa-0.2MPa, the flow rate of the reducing gas is 120mL / min-140mL / min, and the activation and reduction time is 6h-8h.

[0058] During the activation and reduction of the supported metal catalyst, the activation and reduction pressure and the flow rate of the reducing gas are controlled in order to fully reduce the active metal in the supported metal catalyst and thereby stimulate the catalytic activity.

[0059] Furthermore, the stage heating includes first stage heating and second stage heating; the temperature of the first stage heating is 150℃-170℃, and the time is 2h-3h; the temperature of the second stage heating is 280℃-300℃, and the time is 4h-5h.

[0060] The activation reduction of the supported metal catalyst adopts staged temperature increase, starting from a lower temperature for reduction and then gradually increasing the temperature, so that the supported metal catalyst can form uniform catalytic active sites.

[0061] It should be noted that the activation reduction using the above conditions can not only ensure the activation effect of the supported metal catalyst, but also avoid sintering of the supported metal catalyst due to excessively high temperature, thereby ensuring that the supported metal catalyst has good performance. Then, in a reducing gas atmosphere, the supported metal catalyst is used to catalyze the methylation reaction of morpholine and methanol.

[0062] In an optional embodiment of the present invention, the mass ratio of morpholine to methanol is 1:(0.5-1.5); the temperature of the methylation reaction is 170°C-200°C, and the pressure is 0.7MPa-1.0MPa; and hydrogen is used as the reducing gas.

[0063] Reasonable control of the quality of morpholine and methanol can reduce the formation of by-products, thereby increasing the yield of the target product. The temperature and pressure of the methylation reaction are set to increase the yield of the target product.

[0064] In an optional embodiment of the present invention, morpholine and methanol are gases during the methylation reaction, and the space velocity of the mixed gas formed by morpholine and methanol is 0.1 g / h / mL-0.2 g / h / mL.

[0065] It should be noted that the reaction space velocity refers to the mass of the raw material treated by the catalyst per unit volume per unit time under specified conditions. The space velocity of the present invention can ensure that the activity of the catalyst-treated reactant reaches the optimal state within a set range. If it exceeds this range, the feed amount increases when the space velocity increases. A large space velocity means that more raw materials pass through the catalyst per unit time, the residence time of the raw materials on the catalyst is short, and the degree of reaction is shallow. On the contrary, a small space velocity means a long reaction time, and reducing the space velocity is beneficial for improving the conversion rate of the reaction. However, a lower space velocity means that a larger number of catalysts are required under the same treatment capacity, and the reactor volume is larger, which is economically unreasonable. Therefore, a reasonable space velocity range is set by comprehensively considering factors such as device investment, catalyst activity, raw material properties, and product properties.

[0066] In an optional embodiment of the present invention, after the methylation reaction is completed, post-treatment is also included; the post-treatment includes sequentially subjecting the material after the methylation reaction to gas-liquid separation treatment, methanol and water removal treatment, and distillation treatment to obtain N-methylmorpholine.

[0067] It should be noted that the gas-liquid separation process is mainly to obtain a liquid product. In the embodiment of the invention, gas-liquid separation is performed by condensation; methanol is a by-product. In order to avoid affecting the yield and purity of N-methylmorpholine, it is removed by distillation in the embodiment of the invention. The by-product water in the product is removed by adsorption with anhydrous magnesium sulfate. Finally, by means of atmospheric distillation, the fraction is collected at a temperature of 115°C-117°C to obtain N-methylmorpholine; the use of distillation can ensure the purity of the recovered product.

[0068] The features and performance of the present invention are further described in detail below in conjunction with the embodiments.

[0069] Example 1

[0070] This embodiment provides a method for preparing a supported metal catalyst, which comprises the following steps:

[0071] ① Preparation of mesoporous carbon carrier: Add 50g of wood powder to 400g of 25% phosphoric acid aqueous solution, soak at 30℃ for 3h, then slowly heat the mixture to 170℃ in a nitrogen atmosphere, keep it warm for 0.5h, continue to heat to 700℃ and keep it warm for 2h, then wash the solid product until the pH of the washing liquid is 6-7, place it in a vacuum drying oven at 110℃, -0.09MPa and dry it for 18h to obtain a mesoporous carbon carrier.

[0072] ② Preparation of supported metal catalysts: Add 15.6g Cu(NO3)2·3H2O, 5.8g Zn(NO3)2·6H2O and 1.9g Ni(NO3)2·6H2O to 120.0g distilled water respectively, stir and dissolve to prepare a nitrate aqueous solution, add 20.0g mesoporous carbon to the aqueous solution, stir and soak at 70℃ for 8h, dry in a vacuum drying oven at 100℃, -0.1MPa for 18h, grind the dried solid into powder, and calcine in a muffle furnace at 400℃ for 3h to obtain a supported metal catalyst.

[0073] This embodiment also provides an application of a supported metal catalyst in catalytic synthesis of N-methylmorpholine. The preparation of N-methylmorpholine comprises the following steps:

[0074] ① Activation reduction of supported metal catalyst: 20 mL of supported metal catalyst prepared by the above method was added to a fixed bed reactor with a volume of 100 mL. The air in the system was then replaced with nitrogen. After the replacement was completed, the temperature was gradually raised to 170°C under a nitrogen atmosphere, and hydrogen was introduced. The reduction temperature was continued to rise to 290°C, the hydrogen flow rate was controlled to 130 mL / min, the pressure in the system was controlled to 0.2 MPa, and the total reduction time was 8 h.

[0075] ②Methylation reaction: morpholine and methanol are added into the batching tank at a mass ratio of 1:1.2. The morpholine-methanol mixture enters the upper vaporization section of the fixed bed reactor for vaporization, and then enters the catalyst bed at a mixed gas space velocity of 0.15 g / h / mL together with hydrogen at a flow rate of 80 mL / min, and reacts at a temperature of 190°C and a pressure of 0.8 MPa.

[0076] After the reaction is completed, the reaction product is condensed and then separated into gas and liquid; the separated liquid product is first distilled to recover methanol, then the water therein is removed, and then atmospheric distillation is performed to collect the fraction of 115-117° C., which is the N-methylmorpholine product.

[0077] Example 2

[0078] This embodiment provides a method for preparing a supported metal catalyst, which comprises the following steps:

[0079] ① Preparation of mesoporous carbon carrier: Add 50g of wood powder to 350g of 30% phosphoric acid aqueous solution, soak at 50℃ for 2h, then slowly heat the mixture to 160℃ in a nitrogen atmosphere, keep it warm for 0.5h, continue to heat to 600℃ and keep it warm for 2h, then wash the solid product until the pH of the washing liquid is 6-7, place it in a vacuum drying oven at 100℃, -0.1MPa and dry it for 18h to obtain a mesoporous carbon carrier.

[0080] ② Preparation of supported metal catalysts: Add 18.7g Cu(NO3)2·3H2O, 8.7g Zn(NO3)2·6H2O and 2.7g Ni(NO3)2·6H2O to 120.0g distilled water respectively, stir and dissolve to prepare a nitrate aqueous solution, add 20.0g mesoporous carbon to the aqueous solution, stir and soak at 60℃ for 10h, dry in a vacuum drying oven at 90℃, -0.1MPa for 24h, grind the dried solid into powder, and calcine in a muffle furnace at 400℃ for 3h to obtain a supported metal catalyst.

[0081] This embodiment also provides an application of a supported metal catalyst in catalytic synthesis of N-methylmorpholine. The preparation of N-methylmorpholine comprises the following steps:

[0082] ① Activation reduction of supported metal catalyst: 20 mL of supported metal catalyst prepared by the above method was added to a fixed bed reactor with a volume of 100 mL. The air in the system was then replaced with nitrogen. After the replacement was completed, the temperature was gradually raised to 150°C under a nitrogen atmosphere, and hydrogen was introduced. The reduction temperature was continued to rise to 300°C, and the hydrogen flow rate was controlled to 120 mL / min. The pressure in the system was controlled to 0.15 MPa, and the total reduction time was 8 h.

[0083] ②Methylation reaction: morpholine and methanol are added into the batching tank at a mass ratio of 1:1.5. The morpholine-methanol mixture enters the upper vaporization section of the fixed bed reactor for vaporization, and then enters the catalyst bed at a mixed gas space velocity of 0.2 g / h / mL together with hydrogen at a flow rate of 100 mL / min, and reacts at a temperature of 200°C and a pressure of 0.7 MPa.

[0084] After the reaction is completed, the reaction product is condensed and then separated into gas and liquid; the separated liquid product is first distilled to recover methanol, then the water therein is removed, and then atmospheric distillation is performed to collect the fraction of 115-117° C., which is the N-methylmorpholine product.

[0085] Example 3

[0086] This embodiment provides a method for preparing a supported metal catalyst, which comprises the following steps:

[0087] ① Preparation of mesoporous carbon carrier: Add 50g of wood powder to 300g of 35% phosphoric acid aqueous solution, soak at 40℃ for 2h, then slowly heat the mixture to 150℃ in a nitrogen atmosphere, keep it warm for 1h, continue to heat to 650℃ and keep it warm for 1h, then wash the solid product until the pH of the washing liquid is 6-7, place it in a vacuum drying oven at 100℃, -0.1MPa and dry it for 24h to obtain a mesoporous carbon carrier.

[0088] ② Preparation of supported metal catalysts: Add 9.2g Cu(NO3)2·3H2O, 4.4g Zn(NO3)2·6H2O and 3.6g Ni(NO3)2·6H2O to 120.0g distilled water respectively, stir and dissolve to prepare a nitrate aqueous solution, add 20.0g mesoporous carbon to the aqueous solution, stir and soak at 70℃ for 6h, dry in a vacuum drying oven at 100℃, -0.1MPa for 24h, grind the dried solid into powder, and calcine in a muffle furnace at 500℃ for 2h to obtain a supported metal catalyst.

[0089] This embodiment also provides an application of a supported metal catalyst in catalytic synthesis of N-methylmorpholine. The preparation of N-methylmorpholine comprises the following steps:

[0090] ① Activation reduction of supported metal catalyst: 20 mL of supported metal catalyst prepared by the above method was added to a fixed bed reactor with a volume of 100 mL. The air in the system was then replaced with nitrogen. After the replacement was completed, the temperature was gradually raised to 150°C under a nitrogen atmosphere, and hydrogen was introduced. The reduction temperature was continued to rise to 300°C, and the hydrogen flow rate was controlled to 120 mL / min. The pressure in the system was controlled to 0.15 MPa, and the total reduction time was 6 h.

[0091] ②Methylation reaction: morpholine and methanol are added into the batching tank at a mass ratio of 1:1. The morpholine-methanol mixture enters the upper vaporization section of the fixed bed reactor for vaporization, and then enters the catalyst bed at a mixed gas space velocity of 0.1 g / h / mL together with hydrogen at a flow rate of 90 mL / min, and reacts at a temperature of 180°C and a pressure of 0.9 MPa.

[0092] After the reaction is completed, the reaction product is condensed and then separated into gas and liquid; the separated liquid product is first distilled to recover methanol, then the water therein is removed, and then atmospheric distillation is performed to collect the fraction of 115-117° C., which is the N-methylmorpholine product.

[0093] Example 4

[0094] This embodiment provides a method for preparing a supported metal catalyst, which comprises the following steps:

[0095] ① Preparation of mesoporous carbon carrier: Add 50g of wood powder to 300g of 30% phosphoric acid aqueous solution, soak at 30℃ for 2h, then slowly heat the mixture to 160℃ in a nitrogen atmosphere, keep it warm for 1h, continue to heat to 700℃ and keep it warm for 1h, then wash the solid product until the pH of the washing liquid is 6-7, place it in a vacuum drying oven at 110℃, -0.09MPa and dry it for 24h to obtain a mesoporous carbon carrier.

[0096] ② Preparation of supported metal catalysts: Add 12.4g Cu(NO3)2·3H2O, 6.8g Zn(NO3)2·6H2O and 1.2g Ni(NO3)2·6H2O to 120.0g distilled water respectively, stir and dissolve to prepare a nitrate aqueous solution, add 20.0g mesoporous carbon to the aqueous solution, stir and soak at 60℃ for 8h, dry in a vacuum drying oven at 90℃, -0.1MPa for 24h, grind the dried solid into powder, and calcine in a muffle furnace at 400℃ for 4h to obtain a supported metal catalyst.

[0097] This embodiment also provides an application of a supported metal catalyst in catalytic synthesis of N-methylmorpholine. The preparation of N-methylmorpholine comprises the following steps:

[0098] ① Activation reduction of supported metal catalyst: 20 mL of supported metal catalyst prepared by the above method was added to a fixed bed reactor with a volume of 100 mL. The air in the system was then replaced with nitrogen. After the replacement was completed, the temperature was gradually raised to 160°C under a nitrogen atmosphere, and hydrogen was introduced. The reduction temperature was continued to rise to 290°C, the hydrogen flow rate was controlled to 130 mL / min, the pressure in the system was controlled to 0.2 MPa, and the total reduction time was 7 h.

[0099] ② Methylation reaction: morpholine and methanol are added into the batching tank at a mass ratio of 1:0.7. The morpholine-methanol mixture enters the upper vaporization section of the fixed bed reactor for vaporization, and then enters the catalyst bed at a mixed gas space velocity of 0.1 g / h / mL together with hydrogen at a flow rate of 100 mL / min, and reacts at a temperature of 190°C and a pressure of 1.0 MPa.

[0100] After the reaction is completed, the reaction product is condensed and then separated into gas and liquid; the separated liquid product is first distilled to recover methanol, then the water therein is removed, and then atmospheric distillation is performed to collect the fraction of 115-117° C., which is the N-methylmorpholine product.

[0101] Example 5

[0102] This embodiment provides a method for preparing a supported metal catalyst, which comprises the following steps:

[0103] ① Preparation of mesoporous carbon carrier: same as Example 1.

[0104] ② Preparation of supported metal catalysts: Add 14.6g Cu(NO3)2·3H2O, 5.8g Zn(NO3)2·6H2O and 2.5g Ni(NO3)2·6H2O to 120.0g distilled water respectively, stir and dissolve to prepare a nitrate aqueous solution, add 20.0g mesoporous carbon to the aqueous solution, stir and soak at 70℃ for 8h, dry in a vacuum drying oven at 100℃, -0.1MPa for 18h, grind the dried solid into powder, and calcine in a muffle furnace at 400℃ for 3h to obtain a supported metal catalyst.

[0105] This embodiment also provides an application of a supported metal catalyst in catalytic synthesis of N-methylmorpholine. The preparation of N-methylmorpholine comprises the following steps:

[0106] ① Activation and reduction of supported metal catalyst: same as in Example 1.

[0107] ②Methylation reaction: morpholine and methanol are added into the batching tank at a mass ratio of 1:0.5. The morpholine-methanol mixture enters the upper vaporization section of the fixed bed reactor for vaporization, and then enters the catalyst bed at a mixed gas space velocity of 0.1 g / h / mL together with hydrogen at a flow rate of 100 mL / min, and reacts at a temperature of 200°C and a pressure of 0.9 MPa.

[0108] After the reaction is completed, the reaction product is condensed and then separated into gas and liquid; the separated liquid product is first distilled to recover methanol, then the water therein is removed, and then atmospheric distillation is performed to collect the fraction of 115-117° C., which is the N-methylmorpholine product.

[0109] Example 6

[0110] This embodiment provides a method for preparing a supported metal catalyst, which is the same as that of Embodiment 1.

[0111] This embodiment also provides an application of a supported metal catalyst in catalytic synthesis of N-methylmorpholine. The preparation of N-methylmorpholine comprises the following steps:

[0112] ① Activation and reduction of supported metal catalyst: same as in Example 1.

[0113] ② Methylation reaction: morpholine and methanol are added into the batching tank at a mass ratio of 1:0.8. The morpholine-methanol mixture enters the upper vaporization section of the fixed bed reactor for vaporization, and then enters the catalyst bed at a mixed gas space velocity of 0.15 g / h / mL together with hydrogen at a flow rate of 90 mL / min, and reacts at a temperature of 200°C and a pressure of 0.7 MPa.

[0114] After the reaction is completed, the reaction product is condensed and then separated into gas and liquid; the separated liquid product is first distilled to recover methanol, then the water therein is removed, and then atmospheric distillation is performed to collect the fraction of 115-117° C., which is the N-methylmorpholine product.

[0115] Comparative Example 1

[0116] This comparative example provides a method for preparing a supported metal catalyst, which differs from Example 1 in that the mass fraction of the active metal Cu in the supported metal catalyst is not within the range, specifically including:

[0117] ① Preparation of mesoporous carbon carrier: same as Example 1.

[0118] ② Preparation of supported metal catalysts: Add 6.2g Cu(NO3)2·3H2O, 5.3g Zn(NO3)2·6H2O and 1.7g Ni(NO3)2·6H2O to 120.0g distilled water respectively, stir and dissolve to prepare a nitrate aqueous solution, add 20.0g mesoporous carbon to the aqueous solution, stir and soak at 70℃ for 8h, dry in a vacuum drying oven at 100℃, -0.1MPa for 18h, grind the dried sample into powder, and calcine in a muffle furnace at 400℃ for 3h to obtain a supported metal catalyst.

[0119] This comparative example also provides an application of a supported metal catalyst in the catalytic synthesis of N-methylmorpholine. The preparation of N-methylmorpholine is the same as that in Example 1.

[0120] Comparative Example 2

[0121] This comparative example provides a method for preparing a supported metal catalyst, which differs from Example 1 in that the impregnation temperature during the preparation of the supported metal catalyst is not within the range, and specifically includes:

[0122] ① Preparation of mesoporous carbon carrier: same as Example 1.

[0123] ② Preparation of supported metal catalysts: Add 15.6g Cu(NO3)2·3H2O, 5.8g Zn(NO3)2·6H2O and 1.9g Ni(NO3)2·6H2O to 120.0g distilled water respectively, stir and dissolve to prepare a nitrate aqueous solution, add 20.0g mesoporous carbon to the aqueous solution, stir and soak at 40℃ for 8h, dry in a vacuum drying oven at 100℃, -0.1MPa for 18h, grind the dried solid into powder, and calcine in a muffle furnace at 400℃ for 3h to obtain a supported metal catalyst.

[0124] This comparative example also provides an application of a supported metal catalyst in the catalytic synthesis of N-methylmorpholine. The preparation of N-methylmorpholine is the same as that in Example 1.

[0125] Comparative Example 3

[0126] This comparative example provides a method for preparing a supported metal catalyst, which is the same as that of Example 1.

[0127] This comparative example also provides an application of a supported metal catalyst in the catalytic synthesis of N-methylmorpholine. The preparation of N-methylmorpholine differs from that of Example 1 in that the methylation reaction temperature is not within the range, and specifically includes:

[0128] Methylation reaction: morpholine and methanol are added into the batching tank at a mass ratio of 1:1.2. The morpholine-methanol mixture enters the upper vaporization section of the fixed bed reactor for vaporization, and then enters the catalyst bed at a mixed gas space velocity of 0.15 g / h / mL together with hydrogen at a flow rate of 80 mL / min, and reacts at a temperature of 140°C and a pressure of 0.8 MPa.

[0129] After the reaction is completed, the reaction product is condensed and then separated into gas and liquid; the separated liquid product is first distilled to recover methanol, then the water therein is removed, and then atmospheric distillation is performed to collect the fraction of 115-117° C., which is the N-methylmorpholine product.

[0130] Comparative Example 4

[0131] This comparative example provides a method for preparing a supported metal catalyst, which is the same as that of Example 1.

[0132] This comparative example also provides an application of a supported metal catalyst in the catalytic synthesis of N-methylmorpholine. The preparation of N-methylmorpholine differs from that of Example 1 in that the mass ratio of morpholine to methanol in the methylation reaction is not within the range, and specifically includes:

[0133] Methylation reaction: morpholine and methanol are added into the batching tank at a mass ratio of 1:0.4. The morpholine-methanol mixture enters the upper vaporization section of the fixed bed reactor for vaporization, and then enters the catalyst bed at a mixed gas space velocity of 0.15 g / h / mL together with hydrogen at a flow rate of 80 mL / min, and reacts at a temperature of 190°C and a pressure of 0.8 MPa.

[0134] After the reaction is completed, the reaction product is condensed and then separated into gas and liquid; the separated liquid product is first distilled to recover methanol, then the water therein is removed, and then atmospheric distillation is performed to collect the fraction of 115-117° C., which is the N-methylmorpholine product.

[0135] Comparative Example 5

[0136] This comparative example provides a method for preparing a supported metal catalyst, which differs from Example 1 in that the carrier of the supported metal catalyst is changed from mesoporous carbon to γ-Al2O3, specifically comprising:

[0137] Preparation of supported metal catalyst: 15.6g Cu(NO3)2·3H2O, 5.8g Zn(NO3)2·6H2O and 1.9g Ni(NO3)2·6H2O were added to 120.0g distilled water respectively, stirred and dissolved to prepare a nitrate aqueous solution, 20.0g γ-Al2O3 was added to the aqueous solution, stirred and immersed at 70°C for 8h, dried in a vacuum drying oven at 100°C, -0.1MPa for 18h, the dried solid was ground into powder, and calcined in a muffle furnace at 400°C for 3h to obtain a supported metal catalyst.

[0138] This comparative example also provides an application of a supported metal catalyst in the catalytic synthesis of N-methylmorpholine. The preparation of N-methylmorpholine is the same as that in Example 1.

[0139] The designed values ​​of active metal contents in the supported metal catalysts prepared in Examples 1-6 and Comparative Examples 1-5 are shown in Table 1.

[0140] Table 1 Active metal content in supported metal catalysts

[0141]

[0142] During the preparation of the supported metal catalyst, the active metal content of each embodiment and comparative example in Table 1 was obtained by adjusting the addition amount of three nitrates, Cu(NO3)2·3H2O, Zn(NO3)2·6H2O and Ni(NO3)2·6H2O.

[0143] Test Example 1

[0144] In this test example, the conversion rate of morpholine in the catalytic synthesis of N-methylmorpholine in Examples 1-6 and Comparative Examples 1-5 and the yield and purity of the N-methylmorpholine product finally prepared were tested using an Agilent 7820A gas chromatograph. Specific data are shown in Table 2.

[0145] Table 2 Gas chromatography test related data

[0146] Serial number Morpholine conversion rate / % N-methylmorpholine yield / % N-methylmorpholine purity / % Example 1 99.3 96.8 97.6 Example 2 99.1 96.3 97.1 Example 3 98.6 95.8 97.1 Example 4 99.6 96.9 98.1 Example 5 99.2 96.2 97.7 Example 6 98.4 95.3 96.7 Comparative Example 1 78.3 74.6 94.8 Comparative Example 2 85.5 82.2 95.5 Comparative Example 3 70.7 66.8 94.8 Comparative Example 4 84.3 80.8 95.3 Comparative Example 5 54.4 48.9 90.4

[0147] As can be seen from Table 2, in the embodiments 1-6 provided by the present invention, when the preparation method of the supported metal catalyst and N-methylmorpholine is within the scope provided by the embodiments of the present invention, the utilization rate of the morpholine raw material is high, and the yield and purity of the obtained N-methylmorpholine are higher. In comparative examples 1-2, the mass fraction of the active metal Cu in the supported metal catalyst in embodiment 1 is reduced, and the impregnation temperature in the supported metal catalyst preparation process is reduced, and the results show that the conversion rate of morpholine is reduced, and the yield and purity of the N-methylmorpholine product are reduced. In comparative examples 3-4, the methylation reaction temperature in embodiment 1 is reduced, and the mass ratio of morpholine and methanol in the methylation reaction is increased, and the results show that the conversion rate of morpholine is reduced, and the yield and purity of the N-methylmorpholine product are reduced. In comparative example 5, the carrier of the supported metal catalyst is changed from mesoporous carbon to γ-Al2O3, and the results show that the conversion rate of morpholine is reduced, and the yield and purity of the N-methylmorpholine product are reduced.

[0148] Test Example 2

[0149] In this test example, the specific surface area of ​​the supported metal catalysts prepared in Example 1 and Comparative Example 5 was tested using a Belsorp-MAX specific surface area analyzer. The relevant results are shown in Table 3.

[0150] Table 3 Specific surface area test data

[0151] Serial number <![CDATA[Specific surface area (m 2 / g)]]> Example 1 Mesoporous carbon support 348 Example 1 Supported metal catalyst 126 Comparative Example 5 Supported Metal Catalyst 49

[0152] As can be seen from Table 3, the mesoporous carbon carrier prepared in Example 1 has a large specific surface area. The active metal is loaded on the mesoporous carbon carrier, resulting in a portion of the surface of the mesoporous carbon being covered or blocked, so the specific surface area decreases. In Comparative Example 5, the carrier is changed from mesoporous carbon to γ-Al2O3, and the specific surface area of ​​the prepared supported metal catalyst is sharply reduced.

[0153] In summary, the active metal in the supported metal catalyst provided by the present invention has good dispersibility on the carrier, and the preparation process of the supported metal catalyst is simple and the production cost is low. The supported metal catalyst of the present invention has excellent catalytic activity and stability, can significantly improve the yield of N-methylmorpholine and the conversion rate of morpholine raw materials, and is conducive to the industrial production of N-methylmorpholine.

[0154] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A supported metal catalyst, It is characterized in that The supported metal catalyst comprises a carrier and an active metal supported on the carrier; The carrier includes mesoporous carbon, and the active metal includes at least one of Cu element, Zn element, Ni element and Cr element.

2. The supported metal catalyst according to claim 1, It is characterized in that The active metal includes at least one of Cu, Zn and Ni; Preferably, the active metal comprises Cu, Zn and Ni elements at the same time. In terms of mass fraction, the mass of Cu element accounts for 10%-18% of the mass of the supported metal catalyst; the mass of Zn element accounts for 4%-7% of the mass of the supported metal catalyst; and the mass of Ni element accounts for 1%-3% of the mass of the supported metal catalyst.

3. A method for preparing a supported metal catalyst as claimed in any one of claims 1 to 2, It is characterized in that The preparation method comprises: using an impregnation method to load active metal on mesoporous carbon to obtain the loaded metal catalyst.

4. The preparation method according to claim 3, It is characterized in that The preparation of the mesoporous carbon comprises the following steps: The organic precursor and the acid solution are mixed and then heated; the heated product is washed until the pH of the washing solution is 6-7, and the washed product is dried to obtain the mesoporous carbon; The mass ratio of the organic precursor to the acid solution is 1:(6-8); Preferably, the heating treatment includes a first heating stage and a second heating stage; the temperature of the first heating stage is 150°C-180°C, and the time is 0.5h-1h; the temperature of the second heating stage is 600°C-700°C, and the time is 1h-2h.

5. The preparation method according to claim 4, It is characterized in that The organic precursor is selected from any one of wood powder and sucrose; the acid solution is selected from any one of phosphoric acid aqueous solution and hydrochloric acid aqueous solution; Preferably, the organic precursor is wood powder, and the acid solution is a phosphoric acid aqueous solution; Preferably, the mass fraction of phosphoric acid in the phosphoric acid aqueous solution is 25%-35% by mass fraction; Preferably, the organic precursor is added to the acid solution for soaking treatment, the soaking temperature is 30° C.-50° C., and the soaking time is 2 h-4 h; Preferably, the washed product is dried in a drying oven; the drying temperature is 100°C-110°C, the pressure is -0.09MPa to -0.10MPa, and the time is 18h-24h.

6. The preparation method according to claim 3, It is characterized in that The preparation of the supported metal catalyst comprises the following steps: The active metal salt and the mesoporous carbon are immersed in water to obtain a mixed solution; Drying the mixed solution, grinding and calcining the dried product to obtain the supported metal catalyst; The mass ratio of the active metal salt, the water and the mesoporous carbon is (0.72-1.6):6:1; Preferably, the immersion treatment is carried out at a temperature of 50°C-70°C and for a time of 6h-10h; Preferably, the temperature of the drying treatment of the mixed solution is 90°C-100°C, the pressure is -0.09MPa to -0.10MPa, and the time is 18h-24h; Preferably, the calcination temperature is 400°C-500°C, and the calcination time is 2h-4h.

7. The preparation method according to claim 6, It is characterized in that The active metal salt is selected from any one of active metal chloride, active metal sulfate and active metal nitrate; Preferably, the active metal salt is an active metal nitrate; Preferably, the mass ratio of the active metal nitrate is (0.45-0.95): (0.21-0.44): (0.06-0.21) Cu(NO 3 ) 2 ·3H 2 O、Zn(NO 3 ) 2 6H 2 O and Ni (NO 3 ) 2 6H 2 O.

8. Use of the supported metal catalyst according to any one of claims 1 to 2 or the supported metal catalyst prepared by the preparation method according to any one of claims 3 to 7 in the preparation of N-methylmorpholine.

9. The use according to claim 8, It is characterized in that The preparation of the N-methylmorpholine comprises the following steps: In a reducing gas atmosphere, subjecting the supported metal catalyst, morpholine and methanol to a methylation reaction; The mass ratio of the morpholine to the methanol is 1:(0.5-1.5); the temperature of the methylation reaction is 170°C-200°C, and the pressure is 0.7MPa-1.0MPa; the reducing gas is hydrogen; Preferably, when the methylation reaction is carried out, morpholine and methanol are gases, and the space velocity of the mixed gas formed by morpholine and methanol is 0.1 g / h / mL-0.2 g / h / mL; Preferably, the methylation reaction further includes post-treatment after completion; the post-treatment includes sequentially subjecting the material after the methylation reaction to gas-liquid separation treatment, methanol and water removal treatment, and distillation treatment to obtain the N-methylmorpholine.

10. The use according to claim 9, It is characterized in that Before the supported metal catalyst is subjected to the methylation reaction, the supported metal catalyst is activated and reduced; The activation reduction of the supported metal catalyst comprises: adding the supported metal catalyst into a fixed bed, replacing the air in the fixed bed with nitrogen, and in a nitrogen atmosphere, heating up the temperature in stages and introducing reducing gas to completely replace the nitrogen with reducing gas; during the activation reduction, the pressure is controlled to be 0.15MPa-0.2MPa, the flow rate of the reducing gas is 120mL / min-140mL / min, and the activation reduction time is 6h-8h; Preferably, the stage heating includes first stage heating and second stage heating; the temperature of the first stage heating is 150℃-170℃, and the time is 2h-3h; the temperature of the second stage heating is 280℃-300℃, and the time is 4h-5h.