Phosphine-containing organic polymer supported catalyst as well as preparation and application thereof
The phosphine-containing organic polymer-supported catalyst addresses recovery and synthesis challenges of homogeneous catalysts by providing high selectivity and stability, enhancing olefin hydroformylation efficiency and product separation.
Patent Information
- Application Number
- CN202310641150.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-06-01
- Publication Date
- 2024-12-06
AI Technical Summary
Existing homogeneous catalysts for olefin hydroformylation are difficult to recover and synthesize, leading to low selectivity and stability issues, and the synthesis of ligands is challenging, hindering large-scale production.
A phosphine-containing organic polymer-supported catalyst is developed, utilizing a multiphase system with metal components like Rh, Ru, or Ir, and a phosphine-containing organic polymer carrier formed by aldehyde-amine condensation, featuring a multi-level pore structure and multiple coordination bonds, allowing high dispersion of active metals and easy separation.
The catalyst achieves high selectivity and stability, enabling efficient olefin hydroformylation with simple separation of reactants and products, improving conversion rates and selectivity of aldehydes, suitable for industrial applications.
Smart Images

Figure CN119076061A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of heterogeneous catalysis and fine chemical industry, and specifically relates to a phosphine-containing organic polymer supported catalyst, a preparation method thereof and application thereof in olefin hydroformylation reaction. Background Art
[0002] In recent years, with the implementation of the national dual carbon policy, green chemistry has become an increasingly hot topic in research. Atom economic reaction is a typical green chemical reaction. Olefin hydroformylation is a typical atom economic reaction, which is a reaction in which olefins react with CO and H2 to generate aldehydes with one more carbon atom under the action of a catalyst. The atoms in the raw material molecules are 100% converted into products, and there is zero waste emission.
[0003] The product of olefin hydroformylation is aldehyde which has one more carbon atom than olefin. Aldehyde products are important chemical intermediates. Aldehydes and their derivatives are widely used in the production of detergents, plasticizers, surfactants and other products. Therefore, the study of hydroformylation reaction has important research value and important application value.
[0004] Patent CN1319580A describes a variety of bidentate phosphite ligands with large steric hindrance, which have high selectivity for the hydroformylation of high carbon olefins with Rh and Co coordinated homogeneous catalysts. However, homogeneous catalysts are not easy to recover and the ligand synthesis is difficult.
[0005] Patent CN108794527A reports a diphosphine ligand that connects phosphite and diphenylphosphine to an N-benzylidene aniline skeleton. This ligand coordinated with the Rh complex catalyzes the hydroformylation of 1-pentene with high linear aldehyde selectivity, but the reaction is a homogeneous reaction, the catalyst is not easy to recover and the ligand synthesis is relatively difficult.
[0006] Patent CN109942750A uses vinylated bisphosphoramidite ligands and tri(4-vinylphenyl)phosphine to form a supported catalyst, which is then impregnated with acetylacetonato carbonyl rhodium and used in the hydroformylation reaction of hexene. The molar ratio of n-heptanal to isoheptanal is greater than 40, and the catalyst can be recycled. However, the synthesis of vinylated bisphosphoramidite ligands is difficult and has a low yield, which is not conducive to large-scale production. Summary of the invention
[0007] In order to solve the above problems, the object of the present invention is to provide a phosphine-containing organic polymer-supported olefin hydroformylation catalyst which is easy to synthesize, has good stability and has good selectivity.
[0008] The technical solution of the present invention is:
[0009] A phosphine-containing organic polymer supported catalyst, characterized in that: the multiphase catalyst uses one or two or more of metal Rh, Ru, and Ir as active components, uses a phosphine-containing organic polymer as a carrier, and the phosphine-containing organic polymer is formed by aldehyde-amine condensation of a monodentate organic phosphorus ligand and an aromatic compound containing two or more amino groups, and the metal loading range in the catalyst is 0.01 to 5wt%, preferably 0.1 to 0.3wt%.
[0010] The phosphine ligand is a monodentate organic phosphine ligand functionalized with an aldehyde group, and the preferred monodentate phosphine ligand is triphenylphosphine.
[0011] The supported catalyst is characterized in that the porous organic polymer carrier has a multi-level pore structure and a specific surface area of 100 to 900 m 2 / g, containing macropores, mesopores and micropores, with a pore volume of 0.1-2.0cm 3 / g, and the pore size distribution is 0.2~50.0nm.
[0012] The supported catalyst is prepared by dissolving a monodentate organic phosphine, adding a small amount of acetic acid, stirring evenly, and then dropping a solution of hydrazine or an aromatic compound containing two or more amino groups, polymerizing in a hydrothermal kettle to generate a phosphine-containing organic polymer as a carrier, stirring the precursor of the active component and the carrier in an organic solvent, and forming multiple coordination bonds between the active component and the exposed P in the phosphine-containing porous organic polymer carrier, and after evaporating the volatile solvent, a coordination bond-type multiphase catalyst is obtained.
[0013] The catalyst preparation method is:
[0014] a) adding an aldehyde-functionalized monodentate organophosphine ligand and a small amount of acetic acid solution to an organic solvent at 273 to 303 K in an argon atmosphere, mixing, and stirring the mixture for 0.1 to 5 hours, preferably in the range of 0.1 to 1 hour;
[0015] b) transferring the mixed solution obtained in step a) to a reaction kettle, dissolving hydrazine or an aromatic compound containing two or more amino groups in an organic solvent, adding the mixture dropwise to a tube, and performing a polymerization reaction at 353-473K (preferably 373-393K) in an inert gas atmosphere by a solvent thermal polymerization method, standing for 12-100 hours (preferably 24-48 hours), to obtain a phosphine-containing organic polymer;
[0016] c) removing the solvent from the polymer obtained in step b) under vacuum at 338K to obtain an organic polymer containing P, i.e., the carrier of the heterogeneous catalyst;
[0017] d) adding the organic polymer support obtained in step c) to a solvent containing an active component precursor at 273-313K under an inert gas atmosphere, stirring for 1-48 hours, preferably for 6-24 hours, and then removing the organic solvent under vacuum to obtain a heterogeneous catalyst.
[0018] The organic solvent in step a) is one or more of benzene, mesitylene, tetrahydrofuran, and 1,4-dioxane; the concentration of acetic acid is 1-10 mol / L, preferably 2-4 mol / L.
[0019] The molar ratio of the monodentate organic phosphine ligand and the aromatic compound containing two or more amino groups in step a) is 1:1.5 to 2:1.
[0020] The molar ratio of the amount of acetic acid added in step a) to the monodentate organic phosphine ligand is 10:1 to 1:10, preferably 1:1.
[0021] The solvent described in step d) is one or more of water, benzene, toluene, tetrahydrofuran, methanol, ethanol, 1,4-dioxane or mesitylene, and the active component is Rh, Ru, Ir, preferably Rh. The precursor of Rh is Rh(CH3COO)2, RhH(CO)(PPh3)3, Rh(CO)2(acac), RhCl3, preferably Rh(CO)2(acac). The metal loading range in the catalyst is 0.01 to 5wt%. The application of the supported catalyst in olefin hydroformylation reaction is characterized in that the reaction process is to load the prepared catalyst into a reactor, introduce a reaction mixed gas, the main components of the mixed gas are H2 and CO, the volume content of H2+CO is 20-70%, the volume ratio of H2 / CO is 0.5-5.0, the purity of the raw olefin is 20-100%, preferably 80-98%, the reaction temperature is 323-423K, the reaction pressure is 0.1-10.0MPa, and the reactor is a reactor, a fixed bed, a slurry bed, a trickle bed or a bubbling bed reactor.
[0022] Reaction principle of the present invention:
[0023] The present invention introduces an aldehyde functional group into the aromatic ring of a typical monodentate phosphine ligand such as triphenylphosphine, that is, a monodentate organic phosphine ligand containing an aldehyde group is used as a polymerization monomer, and a solvent thermal polymerization method is used in an autoclave to form an organic polymer through aldehyde amine condensation with an aromatic compound containing two or more amino groups. Since the organic polymer skeleton has a large number of exposed P containing lone pairs of electrons, it can be used as a catalyst carrier to form multiple coordination bonds with the empty orbits of active transition metal ions, thereby forming catalytic active sites. In the catalyst, the organic phosphine polymer has the dual functions of a carrier and a ligand at the same time, and the active metal component is highly dispersed in the carrier to form multiple coordination bonds with the high concentration of exposed P. The active metal component is highly dispersed in the organic phosphine polymer carrier in the form of a single atom, which greatly improves the utilization efficiency of the metal. In addition, the active component is not easy to be lost, the catalyst has a long life, and the phosphine ligand in the skeleton has a significant stereo effect. The prepared catalyst can significantly improve the stereoselectivity of the product.
[0024] The catalyst organic polymer carrier skeleton provided by the present invention contains P, and the organic polymer has the dual functions of a ligand and a carrier; the active metal component can be dispersed in the organic polymer carrier in the form of a single atom or an ion, which greatly improves the metal utilization efficiency. The monophosphine ligand structural unit in the carrier organic phosphine polymer skeleton enables the mixed polymer to have a high P concentration, and it is easy to form a double or multiple metal-P coordination bond with the active metal component. The coordination bond has a strong chemical bonding ability, so that the active component is not easy to lose.
[0025] The beneficial effects of the present invention are:
[0026] The multiphase catalyst skeleton of the present invention contains a monodentate organic phosphine ligand structural unit, wherein there is a relatively high exposed P on the surface of the polymer, and the active metal atoms or ions form multiple coordination bonds with the exposed P on the polymer, and the active components are not easy to be lost. The active components of the catalyst are Rh, Co or Ir. Such catalysts have high stereoselectivity, and the polymer has a high specific surface area multi-level pore structure and has the dual functions of a carrier and a ligand. The active metal components may be highly dispersed in the pores or on the surface of the organic phosphine polymer carrier in the form of single atoms, thereby improving the utilization efficiency of the metal components.
[0027] The carrier is simple and easy to obtain, and it is easy to realize industrial application. This type of coordination bond type heterogeneous catalyst is suitable for fixed bed, slurry bed, bubbling bed and trickle bed reactors. The heterogeneous catalyst provided by the present invention has good performance in the production of olefin hydroformylation to prepare aldehydes, and can obtain aldehyde products with extremely high yields. The heterogeneous catalyst has good stability, and the separation of the catalyst from the reactants and products is simple and efficient.
[0028] This type of coordination bond type heterogeneous catalyst is suitable for fixed bed, slurry bed, bubbling bed and trickle bed reaction processes. The method for producing nonanal by octene hydroformylation provided by the present invention can significantly improve the conversion rate of olefins and the selectivity of normal aldehydes, and can solve the problems of poor stability and selectivity, and serious loss of metal components that have existed for a long time in the heterogeneous process of olefin hydroformylation reaction. At the same time, the aldehyde produced by this olefin hydroformylation reaction has high selectivity, good catalyst stability, and simple and efficient separation of reactants and products from the catalyst, which provides a new industrial technology for producing aldehyde products by olefin hydroformylation. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] Figure 1 Taking L1 as an example, the synthesis route of L1 to L3 as building blocks;
[0030] Figure 2 shows the L1, L2 and L3 ligands 1 H, 13 C and 31 P NMR spectrum: (A) L1 1 H NMR spectrum; (B) L1 13 C NMR spectrum; (C) L1 31 P NMR spectrum; (D) L2 1 H NMR spectrum; (E) L2 13 C NMR spectrum; (F) L2 31 P NMR spectrum; (G) L3 1 H NMR spectrum; (H) L3 13 C NMR spectrum; (I) L3 31 P NMR spectrum.
[0031] Taking L1 as an example, the synthesis process of the ligand monomer is as follows: 51mmol magnesium chips and 2 iodine particles are placed in a flask, and 50mmol 4-bromo-benzene diethyl acetal is dissolved in 50mL ultra-dry tetrahydrofuran under an argon atmosphere and slowly added dropwise. After the reaction is complete, 16mmol phosphine trichloride is dissolved in 30mL ultra-dry tetrahydrofuran and slowly added dropwise at -10°C, and the reaction progress is monitored by thin layer chromatography until it is complete. Then the reaction is quenched with a saturated ammonium chloride solution, the organic phase is extracted twice with ethyl acetate, the organic phases are combined, and separated and purified by column chromatography. The obtained product is dissolved in 50mL tetrahydrofuran, 50mL of hydrochloric acid solution with a pH of 1 is added, and heated at 40°C for hydrolysis for 6h. The reaction solution is extracted twice with ethyl acetate, the organic phases are combined, and L1 is obtained after vacuum rotary evaporation.
[0032] The preparation process and conditions of L2 are the same as those of L1, except that 4-bromo-phenylenediethyl acetal is replaced by an equal molar amount of 3-bromo-phenylenediethyl acetal;
[0033] The preparation process and conditions of L3 are the same as those of L1, except that 4-bromo-phenylenediethyl acetal is replaced by an equal molar amount of 2-bromo-phenylenediethyl acetal. DETAILED DESCRIPTION
[0034] The following embodiments are provided to better illustrate the present invention, but are not intended to limit the scope of the present invention.
[0035] Example 1
[0036] In a 50mL reactor, at room temperature and in an inert gas argon atmosphere, 2mmol L1 was dissolved in 6mL 1,4-dioxane, 2mL 3M acetic acid solution was added to the above solution, and stirred for 1 hour. Then 3mmol L4 was dissolved in 4mL 1,4-dioxane, added dropwise to the former, and continued to stir for 1h, and then the reactor was sealed. The polymerization was carried out by solvent thermal polymerization at 120℃ and in an inert gas argon atmosphere for 72h. After the above-mentioned polymerization solution was cooled to room temperature, the solvent was removed by vacuum heating at 65℃ to obtain a polymer carrier with a pore size distribution of 0.2 to 50.0nm.
[0037] 6.28 mg of acetylacetonato dicarbonyl rhodium was weighed and dissolved in 100.0 mL of tetrahydrofuran solvent, 1.0 g of polymer carrier was added, and the mixture was stirred at room temperature under an inert gas atmosphere for 24 hours, and then the solvent was removed in vacuo at room temperature to obtain a heterogeneous catalyst for aliphatic and aromatic hydroformylation.
[0038] 0.05 g of the catalyst was loaded into a reactor, and the reaction mixture was introduced at 110° C. at a pressure of 2 MPa. The reaction gas was (CO:H2=1:1 volume ratio), the volume content of H2+CO was 70%, and the rest was nitrogen. The reaction time was 12 h, S / C (mol amount of olefin substrate: molar amount of active metal component in the catalyst)=4000. 1a was used as the substrate and 10 mL of acetonitrile was used as the solvent. The reaction was carried out in a kettle reactor (50 mL reactor).
[0039] Example 2
[0040] In Example 2, the catalyst synthesis process is the same as that of Example 1 except that L1 is replaced with an equal molar amount of L2.
[0041] Example 3
[0042] In Example 3, except that L1 was replaced with an equal molar amount of L3, the rest of the catalyst synthesis process was the same as in Example 1.
[0043] Example 4
[0044] In Example 4, except that L4 was replaced with an equal molar amount of L5, the rest of the catalyst synthesis process was the same as in Example 1.
[0045] Example 5
[0046] In Example 5, except that L4 was replaced with an equal molar amount of L6, the rest of the catalyst synthesis process was the same as in Example 1.
[0047] Example 6
[0048] In Example 6, except that L4 was replaced with an equal molar amount of L7, the rest of the catalyst synthesis process was the same as in Example 1.
[0049] Example 7
[0050] In Example 7, except that 1,4-dioxane was replaced by a mixed solution of 1,4-dioxane and mesitylene in a volume ratio of 1:1 (1,4-dioxane was replaced by the same volume of the mixed solution), the rest of the catalyst synthesis process was the same as that of Example 1.
[0051] Example 8
[0052] In Example 8, the catalyst synthesis process is the same as that in Example 1, except that 12.6 mg of acetylacetonato dicarbonyl rhodium is weighed and dissolved in 10.0 ml of tetrahydrofuran solvent (instead of weighing 6.28 mg of acetylacetonato dicarbonyl rhodium and dissolving it in 100.0 ml of tetrahydrofuran solvent).
[0053] Example 9
[0054] In Example 9, the catalyst synthesis process is the same as that in Example 1, except that 25.2 mg of acetylacetonato dicarbonyl rhodium is weighed and dissolved in 10.0 ml of tetrahydrofuran solvent (instead of weighing 6.28 mg of acetylacetonato dicarbonyl rhodium and dissolving it in 100.0 ml of tetrahydrofuran solvent).
[0055] Example 10
[0056] In Example 10, 1a was replaced with 1b in the same molar amount, and the rest of the catalyst synthesis process was the same as in Example 1.
[0057] Embodiment 11
[0058] In Example 11, 1a was replaced by 1c in the same molar amount, and the rest of the catalyst synthesis process was the same as in Example 1.
[0059] Example 12
[0060] In Example 12, 1a was replaced by 1d in the same molar amount, and the rest of the catalyst synthesis process was the same as in Example 1.
[0061] Embodiment 13
[0062] In Example 13, 1a was replaced by 1e in the same molar amount, and the rest of the catalyst synthesis process was the same as in Example 1.
[0063] Embodiment 14
[0064] In Example 14, 1a was replaced with 1f in the same molar amount, and the rest of the catalyst synthesis process was the same as in Example 1.
[0065] Embodiment 15
[0066] In Example 15, 1a was replaced with 1g of the same molar amount, and the rest of the catalyst synthesis process was the same as in Example 1.
[0067] Example 16
[0068] In Example 16, 1a was replaced by 1h in the same molar amount, and the rest of the catalyst synthesis process was the same as in Example 1.
[0069] Embodiment 17
[0070] In Example 17, 1a was replaced by 1i in the same molar amount, and the rest of the catalyst synthesis process was the same as in Example 1.
[0071] Embodiment 18
[0072] In Example 18, 1a was replaced by 1j in the same molar amount, and the rest of the catalyst synthesis process was the same as that of Example 1.
[0073] Embodiment 19
[0074] In Example 19, 1a was replaced by 1k in the same molar amount, and the rest of the catalyst synthesis process was the same as in Example 1.
[0075] Embodiment 20
[0076] In Example 20, 1a was replaced with 1l in the same molar amount, and the rest of the catalyst synthesis process was the same as in Example 1.
[0077] Embodiment 21
[0078] In Example 21, 1a was replaced by 1m in the same molar amount, and the rest of the catalyst synthesis process was the same as in Example 1.
[0079] Embodiment 22
[0080] In Example 22, 1a was replaced by 1n in the same molar amount, and the rest of the catalyst synthesis process was the same as in Example 1.
[0081] Embodiment 23
[0082] In Example 23, 1a was replaced by 1o in the same molar amount, and the rest of the catalyst synthesis process was the same as in Example 1.
[0083] Embodiment 24
[0084] In Example 24, 1a was replaced by 1p in the same molar amount, and the rest of the catalyst synthesis process was the same as in Example 1.
[0085] Embodiment 25
[0086] In Example 25, 1a was replaced with 1q in the same molar amount, and the rest of the catalyst synthesis process was the same as in Example 1.
[0087] Embodiment 26
[0088] In Example 26, 1a was replaced by 1r in the same molar amount, and the rest of the catalyst synthesis process was the same as in Example 1.
[0089] Embodiment 27
[0090] In Example 27, 1a was replaced by 1s in the same molar amount, and the rest of the catalyst synthesis process was the same as in Example 1.
[0091] Embodiment 28
[0092] In Example 28, 1a was replaced by 1t in the same molar amount, and the rest of the catalyst synthesis process was the same as in Example 1.
[0093] The pore size distributions of the polymer carriers in the above examples are all in the range of 0.2 to 50.0 nm.
[0094] Comparative Example 1
[0095] A vinyl triphenylphosphine polymer (for the specific preparation method and structure, see patent CN112892602B) is used as a carrier (replacing the polymer carrier with equal mass), and the rest of the catalyst synthesis process is the same as that of Example 1.
[0096] Comparative Example 2
[0097] A homogeneous complex catalyst with the same Rh content was prepared using traditional homogeneous PPh3 as a ligand (replacing the polymer carrier with equal mass), and the reaction was carried out under the same reaction conditions as in Example 1.
[0098] The reaction products were collected by 700MHz NMR instrument. 1 H spectrum, using triphenylmethane as internal standard. The reaction results are listed in Table 1.
[0099] Table 1 Specific surface area of the catalysts synthesized in Examples 1-28 and the hydroformylation reaction data with different types of olefins
[0100]
[0101]
[0102] * Experimental conditions were catalyst 0.05 g (1.0 mL), 110°C, 2 MPa, reaction gas (CO:H2 = 1:1 volume ratio), reaction time 12 h, S / C = 4000. All metals were considered active sites in TOF calculations, and the reaction was carried out in a tank reactor.
[0103] The reaction results were analyzed by Agilent 7890A gas chromatograph with n-butanol as the internal standard.
[0104]
Claims
1. A phosphine-containing organic polymer supported catalyst, Features: The heterogeneous catalyst uses one or more metals of Rh, Ru, and Ir as active components and a phosphine-containing organic polymer as a carrier, wherein the phosphine-containing organic polymer is formed by condensation of one or more monodentate organic phosphorus ligands with one or more hydrazines or aromatic compounds containing two or more amino groups through aldehyde-amine reaction; The active component metal loading in the catalyst (mass ratio of active component metal to carrier) ranges from 0.01 to 5 wt%, preferably from 0.1 to 0.3 wt%.
2. The supported catalyst according to claim 1, Features: An aldehyde-functionalized monodentate organophosphine ligand, wherein the preferred monodentate organophosphine ligand is triphenylphosphine; The monodentate organic phosphine ligand structure is one or more of the following L1 to L3; The hydrazine or aromatic compound containing 2 or more amino groups has a structure of one or more of the following L4 to L10; 3. According to the supported catalyst of claim 1 or 2, Features: The porous organic polymer carrier has a multi-level pore structure and a specific surface area of 100 to 900 m 2 / g, containing macropores, mesopores and micropores, with a pore volume of 0.1-2.0cm 3 / g, and the pore size distribution is 0.2~50.0nm.
4. A supported catalyst according to any one of claims 1 to 3, Features: The supported catalyst is prepared by dissolving any one or more of the monodentate organic phosphine ligands, adding acetic acid, stirring evenly, and then dropping a solution of one or more of hydrazine or aromatic compounds containing two or more amino groups, mixing evenly, and transferring the mixture into a reaction kettle. Then, a phosphine-containing organic polymer is generated as a carrier through solvent thermal synthesis. The precursor of the active component and the carrier are stirred in an organic solvent, and the active component forms multiple coordination bonds with the exposed P in the phosphine-containing porous organic polymer carrier. After removing the solvent, a coordination bond-type multiphase catalyst is obtained.
5. A method for preparing a supported catalyst according to any one of claims 1 to 4, Features: a) adding any one or more monodentate organophosphine ligands (such as L1 to L3) and acetic acid solution to an organic solvent in a reaction vessel at 273 to 303 K under an inert atmosphere (such as argon), and then stirring the mixture for 0.1 to 5 hours, preferably 0.1 to 1 hour; b) dissolving any one or more of hydrazine or aromatic compounds (such as L4 to L10) containing 2 or more amino groups in an organic solvent, adding dropwise to a reaction kettle containing the mixed solution obtained in step a), and performing a polymerization reaction by a solvent thermal polymerization method at 353 to 473 K (preferably 373-393 K) in an inert atmosphere gas (such as argon), standing for 12 to 100 hours (preferably 24 to 72 hours), to obtain a phosphine-containing organic polymer; c) removing the solvent from the polymer obtained in step b) at 293-338K to obtain an organic polymer containing P, i.e., the carrier of the heterogeneous catalyst; d) adding the organic polymer support obtained in step c) to a solvent containing an active component precursor at 273-313K under an inert gas atmosphere, stirring for 1-48 hours, preferably for 6-24 hours, and then removing the organic solvent to obtain a heterogeneous catalyst.
6. The preparation method according to claim 5, Features: The organic solvent in step a) is one or more of benzene, mesitylene, tetrahydrofuran, and 1,4-dioxane; the concentration of acetic acid is 1-10 mol / L, preferably 2-4 mol / L.
7. The preparation method according to claim 5, Features: The molar ratio of the monodentate organophosphine ligand (any one of L1 to L3) and the compound containing two or more amino groups (any one of L4 to L10) in step a) is 2:1 to 1:3, preferably 1:1 to 1:2; The molar ratio of the amount of acetic acid added in step a) to the monodentate organic phosphine ligand is 10:1 to 1:10, preferably 1:1 to 1:
3.
8. The preparation method according to claim 5, Features: The solvent in step d) is one or more of water, benzene, toluene, tetrahydrofuran, methanol, ethanol, 1,4-dioxane or mesitylene; The active component is any one or more of Rh, Ru, and Ir, preferably Rh; wherein the precursor of Rh is Rh(CH 3 COO 2 、RhH(CO)(PPh 3 ) 3 、Rh(CO) 2 (acac), RhCl 3 , preferably Rh(CO) 2 (acac); The metal loading amount in the catalyst (mass ratio of active component metal to carrier) ranges from 0.01 to 5 wt %, preferably from 0.01 to 2 wt %, and more preferably from 0.1 to 0.3 wt %.
9. Use of the supported catalyst according to any one of claims 1 to 4 in olefin hydroformylation reaction.
10. The use according to claim 9, It is characterized in that: It is characterized in that: The reaction process is to load the prepared catalyst into the reactor and introduce a reaction mixed gas, the main component of which is H 2 and CO, H 2 +CO volume content is 20-70%, H 2 The volume ratio of / CO is 0.5-5.0, the rest is nitrogen, the reaction temperature is 323-423K, the reaction pressure is 0.1-10.0MPa, and the reactor is a reactor, a fixed bed, a slurry bed, a trickle bed or a bubbling bed reactor.
Citation Information
Patent Citations
Bidentate phosphine ligand and application thereof in hydroformylation reaction
CN108794527A
Porous organic polymer containing bidentate phosphoramidite ligands, as well as preparation method and application thereof
CN109942750A
A phosphorus-containing porous organic polymer supported catalyst, its preparation method and application
CN112892602B
Process for preparing aldehyde by hydroformylating of olefines