Step-by-step strengthened recovery method for recovering multiple complex copper ores

Through step-by-step strengthening recycling methods, combined with flotation and strong magnetic separation processes, the problem of low recovery rates of multiple complex oxidized copper ores is solved, and efficient comprehensive recovery of multiple copper ores is achieved, with a copper recovery rate of more than 85%.

CN119076200AActive Publication Date: 2024-12-06ZIJIN MINING GROUP CO LTD +1
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202411365356.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-29
Publication Date
2024-12-06
Estimated Expiration
2044-09-29

AI Technical Summary

Technical Problem

The existing technology is difficult to effectively recover a variety of complex copper oxide ores, resulting in low recycling rates, and a single process is difficult to adapt to the characteristics of different copper oxide ores, and comprehensive recycling cannot be achieved.

Method used

Step by step strengthening recovery methods, including copper sulfide flotation, free copper oxide flotation, combined with copper oxide flotation and magnetic bonding copper oxide strong magnetic separator. Through step-by-step flotation and strong magnetic separator, different collectors and Activator, sorting a variety of copper minerals step by step, reducing the inhibitory effect of sodium sulfide and improving the recovery rate of copper ore.

Benefits of technology

The purpose of efficient comprehensive recycling of different copper ores has been achieved, with the copper recovery rate reaching more than 85%, which significantly improves the recovery rate of copper oxide ores and solves the problem of low recovery rate of a single process.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119076200A_ABST
    Figure CN119076200A_ABST
Patent Text Reader

Abstract

The invention discloses a step-by-step strengthened recovery method for recovering multiple complex copper ores, which comprises the following steps: grinding a sample to a proper particle size, and directly floating copper sulfide by adopting amyl xanthate; performing desliming on tailings subjected to flotation of copper sulphide; after desliming, activating by adopting sodium sulfide, and floating free copper oxide by adopting a collecting agent amyl xanthate and ammonium dibutyl dithiophosphate; then ethylenediamine phosphate is adopted for intensified activation, and then sodium sulfide and a collecting agent amyl xanthate and ammonium dibutyl dithiophosphate are added for flotation and combination of copper oxide; and finally, recovering weakly magnetic combined copper oxide which is difficult to float and adsorbs or is mingled with minerals such as iron, manganese and cobalt in micro-fine particles by adopting high-gradient high-intensity magnetic separation. The total copper recovery rate can reach 85% or above and is more than ten% higher than the average beneficiation recovery rate of the world copper oxide ore, and the technical problem that the recovery rate of an existing copper oxide ore single process is low can be well solved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of ore dressing, and in particular to a step-by-step enhanced recovery method for recovering multiple complex copper ores. Background Art

[0002] Copper oxide is mainly obtained by the long-term oxidation reaction of copper sulfide deposits. Copper oxide ores generally contain blue / chalcocite, malachite, chrysocolla, cuprite and other combined copper oxides. The properties of copper oxide ores are very complex, with a large content of ore mud, many types of copper minerals, and large differences in the floatability of various copper minerals. The copper oxide in it generally has a strong surface hydrophilicity, high oxidation rate and binding rate, and useful minerals are often adsorbed or fine particles are mixed with iron, manganese, cobalt and other minerals. Therefore, to a certain extent, the difficulty of flotation of copper oxide ores is increased, and there has always been a problem of low recovery rate. In order to comprehensively utilize these complex copper oxide ore resources, mineral processing workers have developed many mineral processing methods. Commonly used mineral processing methods include direct flotation, sulfide flotation, sulfide flotation + acid leaching, acid leaching, separation method and combined treatment method of mineral processing. The best processing technology for copper oxide ores of different properties is different. At present, the beneficiation technology of copper oxide ores is generally mainly studied on one or two copper ores. There are few processes for comprehensive recycling of multiple copper ores, which makes it difficult to achieve the purpose of comprehensive recycling of multiple copper ores. Therefore, it is very necessary to conduct experimental research and development to strengthen the efficient step-by-step recovery of multiple copper ores according to the beneficiation characteristics of different copper oxide ores, which is of great significance for improving the comprehensive recovery rate of multiple complex copper oxide ores. Summary of the invention

[0003] In view of the deficiencies of the prior art, the present invention aims to provide a step-by-step enhanced recovery method for recovering multiple complex copper ores.

[0004] In order to achieve the above object, the present invention adopts the following technical solution:

[0005] A step-by-step enhanced recovery method for recovering multiple complex copper ores comprises the following steps:

[0006] A. Copper sulfide flotation: After the raw ore is ground, the collector amyl xanthate and the foaming agent 2# oil are added to the pulp ground to the target particle size for copper sulfide roughing. The roughing tailings obtained from the copper sulfide roughing are sent to the copper sulfide scavenging operation, and the roughing concentrate obtained from the copper sulfide roughing is sent to the copper sulfide concentrating operation; the concentrating concentrate finally obtained from the copper sulfide concentrating operation is the copper sulfide concentrate, and the scavenging tailings finally obtained from the copper sulfide scavenging operation are transferred to the treatment of step B;

[0007] B. Desliming: The scavenging tailings obtained in step A are deslimed by a cyclone, and the deslimed ore sand enters step C for treatment;

[0008] C. Free oxidation copper flotation: The ore sand obtained in step B is dispersed with dispersant sodium fluorosilicate, activated with sodium sulfide, and then amyl xanthate, butyl ammonium black medicine and 2# oil are added, and then enters the free oxidation copper roughing operation, the roughing concentrate obtained by the free oxidation copper roughing enters the free oxidation copper concentration operation, and the roughing tailings obtained by the free oxidation copper roughing enter the free oxidation copper scavenging operation; the final concentrated concentrate obtained by the free oxidation copper concentration is the first oxide copper concentrate, and the final scavenging tailings obtained by the free oxidation copper scavenging enter the treatment of step D;

[0009] D. Combined copper oxide flotation: The scavenging tailings finally obtained by free copper oxide scavenging are activated by ethylenediamine phosphate, and then sodium sulfide, amyl xanthate, butyl ammonium black medicine and 2# oil are added to carry out combined copper oxide roughing, the roughing concentrate obtained by combined copper oxide roughing enters the combined copper oxide concentrating operation, and the roughing tailings obtained by combined copper oxide roughing enter the combined copper oxide scavenging operation; the concentrated concentrate finally obtained by combined copper oxide concentrating is copper oxide concentrate II, and the scavenging tailings finally obtained by combined copper oxide scavenging enter the treatment of step E;

[0010] E. Magnetic combined with strong magnetic separation of copper oxide: The scavenging tailings obtained by scavenging copper oxide are subjected to high gradient strong magnetic separation to obtain copper oxide concentrate 3 and final tailings.

[0011] Furthermore, in step A, one copper sulfide roughing selection, one copper sulfide scavenging selection and four copper sulfide concentrations are carried out; the concentrated tailings obtained in the first stage of copper sulfide concentration are returned to the copper sulfide roughing selection, and the concentrated tailings obtained in the remaining stages of copper sulfide concentration are returned to the previous stage of copper sulfide concentration in sequence, and the concentrated concentrate obtained in each stage of copper sulfide concentration enters the next stage of copper sulfide concentration, and the copper sulfide concentrated concentrate obtained in the last stage of copper sulfide concentration is a high-grade copper sulfide concentrate.

[0012] Furthermore, in step A, based on the dry ore weight per ton of raw ore, 40 g / t of collector amyl xanthate and 30 g / t of foaming agent 2# oil are added in the roughing of copper sulfide; and 20 g / t of amyl xanthate is added in the scavenging of copper sulfide.

[0013] Furthermore, in step C, one free oxidation copper roughing, two free oxidation copper scavenging and one free oxidation copper concentration are carried out; the concentrated tailings obtained from the free oxidation copper concentration are returned to the free oxidation copper roughing operation in sequence; the scavenged ore obtained from the first-level free oxidation copper scavenging is returned to the free oxidation copper roughing operation in sequence, and the scavenged ore obtained from the second-level free oxidation copper scavenging is returned to the first-level free oxidation copper scavenging operation in sequence; the scavenged tailings obtained from the first-level free oxidation copper scavenging enter the second-level free oxidation copper scavenging operation, and the scavenged tailings obtained from the second-level free oxidation copper scavenging enter the treatment of step D.

[0014] Furthermore, in step C, before sodium sulfide activation, sodium fluorosilicate as a dispersant is added to the ore sand obtained in step B; sodium sulfide, amyl xanthate and butyl ammonium xanthate are added to both the free oxidation copper selection and the free oxidation copper scavenging.

[0015] Furthermore, in step C, 300 g / t of sodium fluorosilicate and 2400 g / t of sodium sulfide are added to the ore sand based on the dry ore weight per ton of raw ore; 160 g / t of collector amyl xanthate, 40 g / t of butyl ammonium black powder and 30 g / t of foaming agent 2# oil are added in the rough selection of free oxidation copper; 100 g / t of sodium sulfide, 10 g / t of amyl xanthate and 4 g / t of butyl ammonium black powder are added in the free oxidation copper selection; the dosage of reagents for the first-stage free oxidation copper scavenging is 800 g / t of sodium sulfide, 80 g / t of amyl xanthate and 20 g / t of butyl ammonium black powder, and the dosage of reagents for the second-stage free oxidation copper scavenging is 300 g / t of sodium sulfide, 20 g / t of amyl xanthate and 10 g / t of butyl ammonium black powder.

[0016] Further, in step D, one combined copper oxide roughing selection, two combined copper oxide scavenging selections and two combined copper oxide concentrating selections are carried out; the concentrating tailings obtained from the first-stage combined copper oxide concentrating are sequentially returned to the combined copper oxide roughing selection operation, the concentrating tailings obtained from the second-stage combined copper oxide concentrating are sequentially returned to the first-stage combined copper oxide concentrating operation, and the concentrating concentrate obtained from the first-stage combined copper oxide concentrating enters the second-stage combined copper oxide concentrating operation; the scavenged ore obtained from the first-stage combined copper oxide scavenging selection is sequentially returned to the combined copper oxide roughing selection operation, the scavenged ore obtained from the second-stage combined copper oxide scavenging selection is sequentially returned to the first-stage combined copper oxide scavenging operation, the scavenged tailings obtained from the first-stage combined copper oxide scavenging selection enters the second-stage combined copper oxide scavenging operation, and the scavenged tailings obtained from the second-stage combined copper oxide scavenging enters the treatment of step E.

[0017] Furthermore, in step D, the scavenging tailings obtained by scavenging free copper oxide are first activated by 200 g / t of ethylenediamine phosphate and 400 g / t of sodium sulfide, based on the dry weight of each ton of raw ore; in the combined copper oxide roughing, 30 g / t of amyl xanthate, 10 g / t of butyl ammonium black powder and 10 g / t of 2# oil are added as collectors; the dosage of the first-stage combined copper oxide selection reagents is 100 g / t of sodium sulfide, 10 g / t of amyl xanthate and The dosage of butyl ammonium black powder is 5g / t, and the dosage of the second-stage combined copper oxide selection is 100g / t of sodium sulfide, 10g / t of amyl xanthate and 4g / t of butyl ammonium black powder; the dosage of the first-stage combined copper oxide scavenging is 300g / t of sodium sulfide, 20g / t of amyl xanthate and 10g / t of butyl ammonium black powder, and the dosage of the second-stage combined copper oxide scavenging is 200g / t of sodium sulfide, 20g / t of amyl xanthate and 10g / t of butyl ammonium black powder.

[0018] The beneficial effects of the present invention are as follows: the method of the present invention mainly targets the differences in the properties of different copper minerals, and the step-by-step flotation process is adopted for copper sulfide and different copper oxide ores, which can reduce the inhibitory effect of sodium sulfide on copper sulfide and obtain high-grade copper sulfide concentrate at the same time. The free copper oxide is directly activated by sodium sulfide + combined collector for flotation to obtain high-grade copper oxide concentrate. The combined copper oxide that is difficult to activate flotation is activated by ethylenediamine phosphate and then sodium sulfide + combined collector is adopted for flotation recovery, and the weak magnetic combined copper oxide adsorbed or finely mixed with iron, manganese, cobalt and other minerals is recovered by strong magnetic separation. The method of the present invention adopts different processes for step-by-step strengthening of separation for copper ores containing multiple types of copper minerals, so as to achieve the purpose of efficient and comprehensive recovery of different copper ores, and forms an innovative mineral processing process for processing this type of difficult-to-select copper oxide ores. The total copper recovery rate of the present invention can reach more than 85%, which is more than ten percentage points higher than the average mineral processing recovery rate of copper oxide ores in the world, and can better solve the technical problem of low recovery rate of single process of copper oxide ores at present. BRIEF DESCRIPTION OF THE DRAWINGS

[0019] Figure 1 This is a process flow chart of Examples 1 and 2 of the present invention. DETAILED DESCRIPTION

[0020] The present invention will be further described below in conjunction with the accompanying drawings. It should be noted that this embodiment is based on the technical solution and provides a detailed implementation method and specific operation process, but the protection scope of the present invention is not limited to this embodiment.

[0021] Example 1

[0022] The original ore is an oxidized copper ore, containing 6.05% copper and 0.18% sulfur. The main gangue is quartz (68.11%), followed by calcite, dolomite, apatite, etc. There are many types of copper minerals, mainly including oxidized copper minerals such as malachite (6.5%), chrysocolla (3.9%) and pseudomalachite (0.05%), and copper sulfide (0.96%). Cu is mainly found in malachite, followed by chrysocolla and copper sulfide, and is partially dispersed in other minerals (including manganese-cobalt-copper silicate ore, limonite, pyrolusite, etc.).

[0023] This embodiment provides a step-by-step enhanced recovery method for recovering multiple complex copper ores, such as Figure 1 As shown, the following steps are included:

[0024] A. Copper sulfide flotation: According to the dry weight of each ton of raw ore, after the raw ore is ground, 40g / t of collector amyl xanthate and 30g / t of frother 2# oil are added to the pulp ground to -74μm with a fineness of 65% for a copper sulfide roughing. The obtained copper sulfide roughing concentrate is subjected to 4 copper sulfide concentrations. The selected tailings obtained in the first level of copper sulfide concentration are returned to the copper sulfide roughing, and the selected tailings obtained in the remaining levels of copper sulfide concentration are returned to the previous level of copper sulfide concentration in sequence. The selected concentrate obtained in each level of copper sulfide concentration enters the next level of copper sulfide concentration. The copper sulfide selected concentrate obtained in the last level of copper sulfide concentration is a high-grade copper sulfide concentrate. 20g / t of amyl xanthate is added to the copper sulfide roughing tailings for a copper sulfide scavenging. The copper sulfide scavenging tailings are returned to the copper sulfide roughing, and the copper sulfide scavenging tailings enter the desludging;

[0025] B. Desliming: After the copper sulfide scavenging tailings are deslimed by a cyclone, the ore sand enters the free oxidation copper flotation;

[0026] C. Free oxidation copper flotation: The ore sand obtained in step B is first dispersed into ore mud with dispersant sodium fluorosilicate 300 g / t, then activated with sodium sulfide 2400 g / t, and then a combined collector amyl xanthate 160 g / t and butyl ammonium black powder 40 g / t are added, and a frother 2# oil 30 g / t is added to carry out a free oxidation copper roughing to obtain a free oxidation copper roughing concentrate. After adding sodium sulfide 100 g / t and a combined collector amyl xanthate 10 g / t and butyl ammonium black powder 4 g / t, a free oxidation copper concentration is carried out to obtain a high-grade copper oxide concentrate 1. The free oxidation copper roughing tailings are subjected to two free oxidation copper scavengings. The reagent dosage of the first stage free oxidation copper scavenging is 800g / t of sodium sulfide and 80g / t of combined collector amyl xanthate and 20g / t of butyl ammonium black medicine. The reagent dosage of the second stage free oxidation copper scavenging is 300g / t of sodium sulfide and 20g / t of combined collector amyl xanthate and 10g / t of butyl ammonium black medicine. The middlings from the first stage free oxidation copper scavenging are returned to the free oxidation copper roughing operation in sequence, and the middlings from the second stage free oxidation copper scavenging are returned to the first stage free oxidation copper scavenging operation in sequence. The tailings of each stage free oxidation copper scavenging enter the next stage free oxidation copper scavenging, and the tailings of the second stage free oxidation copper scavenging enter the combined oxide copper flotation.

[0027] D. Combined copper oxide flotation: The free copper oxide scavenging tailings are first activated by ethylenediamine phosphate 200g / t, and then 400g / t of sodium sulfide, 30g / t of combined collector amyl xanthate, 10g / t of butyl ammonium black powder and 10g / t of frother 2# oil are added to carry out a combined copper oxide roughing to obtain a combined copper oxide roughing concentrate. The combined copper oxide roughing concentrate is subjected to two combined copper oxide selections. The dosage of the reagents for the first stage of combined copper oxide selection is 100g / t of sodium sulfide, 10g / t of combined collector amyl xanthate and 10g / t of butyl ammonium black powder. The dosage of black powder is 5g / t, and the dosage of the second-stage combined copper oxide concentration is 100g / t of sodium sulfide and a combined collector of 10g / t of amyl xanthate and 4g / t of butyl ammonium black powder. The selected tailings from the first-stage combined copper oxide concentration are returned to the combined copper oxide roughing operation in sequence, and the selected tailings from the second-stage combined copper oxide concentration are returned to the first-stage combined copper oxide concentration operation in sequence. The selected concentrate from each stage of combined copper oxide concentration enters the next stage of combined copper oxide concentration operation, and the selected concentrate from the last stage of combined copper oxide concentration is the low-grade copper oxide concentrate 2. The copper oxide roughing tailings are subjected to two copper oxide scavenging operations. The first stage copper oxide scavenging agent dosage is 300g / t of sodium sulfide and 20g / t of combined collector amyl xanthate and 10g / t of butyl ammonium black medicine. The second stage copper oxide scavenging agent dosage is 200g / t of sodium sulfide and 20g / t of combined collector amyl xanthate and 10g / t of butyl ammonium black medicine. The scavenged ores from the first stage copper oxide scavenging are returned to the copper oxide roughing operation in sequence, and the scavenged ores from the second stage copper oxide scavenging are returned to the first stage copper oxide scavenging operation in sequence. The tailings from each stage of copper oxide scavenging enter the next stage of copper oxide scavenging operation, and the scavenged tailings from the last stage of copper oxide scavenging enter the magnetic copper oxide strong magnetic separation.

[0028] E. Magnetic-bonded copper oxide strong magnetic separation: The scavenging tailings of the last stage of scavenging copper oxide in step D are subjected to secondary strong magnetic separation with a magnetic field strength of 1.75 T to recover weakly magnetic-bonded copper oxide, thereby obtaining copper oxide concentrate 3 and final tailings.

[0029] Example 2

[0030] The original ore is an oxidized copper ore, containing 5.40% copper and 0.16% sulfur. The main gangue is quartz (77.36%), followed by dolomite, calcite, muscovite, etc. There are many types of copper minerals, mainly including oxidized copper minerals such as malachite (5.73%), chrysocolla (3.51%) and pseudomalachite (0.06%), and copper sulfide (0.86%). Cu is mainly found in malachite, followed by chrysocolla and copper sulfide, and is partially dispersed in manganese-cobalt-copper silicate minerals.

[0031] This embodiment uses the same method flow and reagent system as embodiment 1 to process the above raw ore.

[0032] Comparative Example 1

[0033] The original ore is an oxidized copper ore, containing 4.79% copper and 0.14% sulfur. The main gangue is quartz (75.90%), followed by muscovite, chlorite, dolomite, etc. There are many types of copper minerals, mainly including oxidized copper minerals such as malachite (5.15%), chrysocolla (3.11%) and pseudomalachite (0.04%), and copper sulfide (0.77%). Cu is mainly found in malachite, followed by chrysocolla and copper sulfide, and partially dispersed in other silicate minerals.

[0034] In this comparative example, the above raw ore is pre-selected into copper sulfide ore, activated with sodium sulfide after desludging, and then copper oxide is floated with amyl xanthate.

[0035] The implementation results of Example 1, Example 2 and Comparative Example 1 are shown in Table 1.

[0036]

[0037]

[0038] The results of Example 1 and Example 2 shown in Table 1 show that the copper grade of the original ore in Example 1 is 6.05%, and the following can be obtained: a high-grade copper sulfide concentrate with a yield of 1.19%, a copper grade of 58.50%, and a copper recovery rate of 11.51%; a high-grade copper oxide concentrate 1 with a yield of 10.63%, a copper grade of 28.74%, and a copper recovery rate of 50.53%; a low-grade copper oxide concentrate 2 with a yield of 6.55%, a copper grade of 17.56%, and a copper recovery rate of 19.02%; and a low-grade copper oxide concentrate 3 with a yield of 3.32%, a copper grade of 7.62%, and a copper recovery rate of 4.18%. The comprehensive copper recovery rate reaches 85.25%.

[0039] In Example 2, the copper grade of the original ore is 5.40%, and the following can be obtained: a high-grade copper sulfide concentrate with a yield of 1.09%, a copper grade of 59.88%, and a copper recovery rate of 12.08%; a high-grade copper oxide concentrate 1 with a yield of 9.89%, a copper grade of 27.74%, and a copper recovery rate of 50.76%; a low-grade copper oxide concentrate 2 with a yield of 5.82%, a copper grade of 16.71%, and a copper recovery rate of 17.99%; and a low-grade copper oxide concentrate 3 with a yield of 3.41%, a copper grade of 7.11%, and a copper recovery rate of 4.49%. The comprehensive copper recovery rate is 85.32%.

[0040] In comparative example 1, the copper grade of the original ore is 4.79%, and the following can be obtained: a high-grade copper sulfide concentrate with a yield of 0.89%, a copper grade of 57.88%, and a copper recovery rate of 10.76%; a copper oxide concentrate with a yield of 11.43%, a copper grade of 26.04%, and a copper recovery rate of 62.14%. The comprehensive copper recovery rate is 72.90%. The process of comparative example 1 adopts sodium sulfide activation and flotation for copper oxide, mainly for malachite, which has a flotation recovery effect. The copper in silica malachite and copper-containing silicate minerals is difficult to activate and flotate and recover, and is lost in the tailings. The final result is a low recovery rate.

[0041] For those skilled in the art, various corresponding changes and modifications can be made according to the above technical solutions and concepts, and all of these changes and modifications should be included in the protection scope of the claims of the present invention.

Claims

1. A step-by-step enhanced recovery method for recovering multiple complex copper ores, characterized in that: The steps include: A. Copper sulfide flotation: After the raw ore is ground, the collector amyl xanthate and the foaming agent 2# oil are added to the pulp ground to the target particle size for copper sulfide roughing. The roughing tailings obtained from the copper sulfide roughing are sent to the copper sulfide scavenging operation, and the roughing concentrate obtained from the copper sulfide roughing is sent to the copper sulfide concentrating operation; the concentrating concentrate finally obtained from the copper sulfide concentrating operation is the copper sulfide concentrate, and the scavenging tailings finally obtained from the copper sulfide scavenging operation are transferred to the treatment of step B; B. Desliming: The scavenging tailings obtained in step A are deslimed by a cyclone, and the deslimed ore sand enters step C for treatment; C. Free oxidation copper flotation: after the ore sand obtained in step B is activated with sodium sulfide, amyl xanthate, butyl ammonium black medicine and 2# oil are added, and then enter the free oxidation copper roughing operation, the roughing concentrate obtained by the free oxidation copper roughing operation enters the free oxidation copper concentration operation, and the roughing tailings obtained by the free oxidation copper roughing operation enter the free oxidation copper scavenging operation; the final concentrated concentrate obtained by the free oxidation copper concentration is the first oxide copper concentrate, and the final scavenging tailings obtained by the free oxidation copper scavenging operation enter the treatment of step D; D. Combined copper oxide flotation: The scavenging tailings finally obtained by free copper oxide scavenging are activated by ethylenediamine phosphate, and then sodium sulfide, amyl xanthate, butyl ammonium black medicine and 2# oil are added to carry out combined copper oxide roughing, the roughing concentrate obtained by combined copper oxide roughing enters the combined copper oxide concentrating operation, and the roughing tailings obtained by combined copper oxide roughing enter the combined copper oxide scavenging operation; the concentrated concentrate finally obtained by combined copper oxide concentrating is copper oxide concentrate II, and the scavenging tailings finally obtained by combined copper oxide scavenging enter the treatment of step E; E. Magnetic combined with strong magnetic separation of copper oxide: The scavenging tailings obtained by scavenging copper oxide are subjected to high gradient strong magnetic separation to obtain copper oxide concentrate 3 and final tailings.

2. The method according to claim 1, characterized in that: In step A, one copper sulfide roughing selection, one copper sulfide scavenging selection and four copper sulfide concentrations are carried out; the concentrated tailings obtained in the first stage of copper sulfide concentration are returned to the copper sulfide roughing selection, and the concentrated tailings obtained in the remaining stages of copper sulfide concentration are returned to the previous stage of copper sulfide concentration in sequence, and the concentrated concentrate obtained in each stage of copper sulfide concentration enters the next stage of copper sulfide concentration, and the copper sulfide concentrated concentrate obtained in the last stage of copper sulfide concentration is the copper sulfide concentrate.

3. The method according to claim 1 or 2, characterized in that: In step A, based on the dry weight of each ton of raw ore, 40 g / t of collector amyl xanthate and 30 g / t of frother 2# oil were added in the roughing of copper sulfide; 20 g / t of amyl xanthate was added in the scavenging of copper sulfide.

4. The method according to claim 1, characterized in that: In step C, one free oxidation copper roughing, two free oxidation copper scavenging and one free oxidation copper concentration are carried out; the concentrated tailings obtained from the free oxidation copper concentration are returned to the free oxidation copper roughing operation in sequence; the scavenged ore obtained from the first-level free oxidation copper scavenging is returned to the free oxidation copper roughing operation in sequence, and the scavenged ore obtained from the second-level free oxidation copper scavenging is returned to the first-level free oxidation copper scavenging operation in sequence; the scavenged tailings obtained from the first-level free oxidation copper scavenging enter the second-level free oxidation copper scavenging operation, and the scavenged tailings obtained from the second-level free oxidation copper scavenging enter the treatment of step D.

5. The method according to claim 1 or 4, characterized in that: In step C, before sodium sulfide activation, sodium fluorosilicate as a dispersant is added to the ore sand obtained in step B; sodium sulfide, amyl xanthate and butyl ammonium xanthate are added to both the free oxidation copper selection and the free oxidation copper scavenging.

6. The method according to claim 5, characterized in that In step C, 300 g / t of sodium fluorosilicate and 2400 g / t of sodium sulfide are added to the ore sand based on the dry weight of each ton of raw ore; 160 g / t of amyl xanthate collector, 40 g / t of butyl ammonium black powder and 30 g / t of frother 2 oil are added to the free oxidation copper roughing; 100 g / t of sodium sulfide, 10 g / t of amyl xanthate and 4 g / t of butyl ammonium black powder are added to the free oxidation copper concentration; the dosage of the reagents for the first-stage free oxidation copper scavenging is 800 g / t of sodium sulfide, 80 g / t of amyl xanthate and 20 g / t of butyl ammonium black powder, and the dosage of the reagents for the second-stage free oxidation copper scavenging is 300 g / t of sodium sulfide, 20 g / t of amyl xanthate and 10 g / t of butyl ammonium black powder.

7. The method according to claim 1, characterized in that In step D, one combined copper oxide roughing, two combined copper oxide scavenging and two combined copper oxide concentrating are carried out; the concentrating tailings obtained from the first-stage combined copper oxide concentrating are sequentially returned to the combined copper oxide roughing operation, the concentrating tailings obtained from the second-stage combined copper oxide concentrating are sequentially returned to the first-stage combined copper oxide concentrating operation, and the concentrating concentrate obtained from the first-stage combined copper oxide concentrating enters the second-stage combined copper oxide concentrating operation; the scavenged ore obtained from the first-stage combined copper oxide scavenging is sequentially returned to the combined copper oxide roughing operation, the scavenged ore obtained from the second-stage combined copper oxide scavenging is sequentially returned to the first-stage combined copper oxide scavenging operation, the scavenged tailings obtained from the first-stage combined copper oxide scavenging enters the second-stage combined copper oxide scavenging operation, and the scavenged tailings obtained from the second-stage combined copper oxide scavenging enters the treatment of step E.

8. The method according to claim 7, characterized in that In step D, based on the dry weight of each ton of raw ore, the scavenging tailings obtained by free copper oxide scavenging are first activated with 200 g / t of ethylenediamine phosphate and 400 g / t of sodium sulfide; in combination with copper sulfide roughing, collectors amyl xanthate 30 g / t, butyl ammonium black powder 10 g / t and 2# oil 10 g / t are added; the dosage of the reagents used in the first stage of copper oxide selection is sodium sulfide 100 g / t, amyl xanthate 10 g / t and butyl ammonium black powder The dosage of reagents for the second stage combined with copper oxide selection is 100g / t of sodium sulfide, 10g / t of amyl xanthate and 4g / t of butyl ammonium black medicine; the dosage of reagents for the first stage combined with copper oxide scavenging is 300g / t of sodium sulfide, 20g / t of amyl xanthate and 10g / t of butyl ammonium black medicine, and the dosage of reagents for the second stage combined with copper oxide scavenging is 200g / t of sodium sulfide, 20g / t of amyl xanthate and 10g / t of butyl ammonium black medicine.

Citation Information

Patent Citations

  • Flotation method of copper oxide ores

    CN105750093A

  • Method for promoting sulfide floatation of copper oxide ores with amino acid

    CN106824545A

  • Flotation technology for efficiently recycling complex copper oxide ore

    CN107486338A

  • Dressing and smelting combined treatment method for recycling complex copper oxide ore

    CN110681477A

  • Separation method for cupric oxide and copper sulfide mixed ore

    CN111790517A