Production method for reducing A / B-level pinholes of battery aluminum foil
By introducing low-temperature annealing and rolling parameter optimization in the rolling process of battery aluminum foil, combined with online testing, the problem of excessive A/B pinholes in the battery aluminum foil is solved, and cost-effectiveness is improved and mechanical properties are maintained.
Patent Information
- Application Number
- CN202411383971.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-30
- Publication Date
- 2024-12-06
AI Technical Summary
The number of A/B grade pinholes in the aluminum foil of the power battery positive electrode material battery has too many, affecting the production efficiency and the mechanical properties of the finished product. The existing control methods are costly, low efficiency and unstable.
In the foil rolling process of battery aluminum foil, the rolling parameters and roll roughness are adjusted, and the rolling process is controlled to reduce the number of pinholes.
The number of A/B grade pinholes of battery aluminum foil is significantly reduced, the tensile strength and elongation of aluminum foil is maintained, the production cost and hazardous waste output are reduced, and the production efficiency and product quality are improved.
Smart Images

Figure BDA0005070577200000071 
Figure BDA0005070577200000081 
Figure BDA0005070577200000082
Abstract
Description
1. Technical field:
[0001] The invention belongs to the technical field of battery aluminum foil preparation, and specifically relates to a production method for reducing A / B level pinholes in battery aluminum foil without affecting the tensile strength and elongation of the aluminum foil. 2. Background technology:
[0002] In recent years, the development of the country's new energy industry has made great progress. Among them, new energy batteries, mainly power batteries, have shown a rapid development momentum and become the core pillar of the new energy industry. Battery aluminum foil, as an indispensable and excellent substrate in new energy batteries, has also ushered in significant development.
[0003] Since aluminum foil has good electrical conductivity, it is usually coated with ternary materials, lithium iron phosphate materials, etc. as the positive electrode current collector of lithium batteries. The cost of aluminum foil in lithium-ion batteries accounts for about 1.5-2.0%. In sodium-ion batteries, which are mainly used for energy storage, since sodium does not react with aluminum, aluminum foil can be used for both positive and negative electrode current collectors, thereby increasing the amount of aluminum foil used in sodium batteries, and its cost share can basically reach about 5.0%.
[0004] Battery aluminum foil is the highest quality product among all types of aluminum foil. Its technical requirements are almost harsh and the product is almost perfect, especially the aluminum foil used for power new energy batteries, which is basically a zero-defect product.
[0005] In terms of pinhole requirements, the thickness of battery aluminum foil has dropped from the more commonly used 15um-20um to the current 8um-13um in a relatively short period of time. The adverse effects caused by the pinhole problem have gradually emerged, which will cause the pole piece to break during the rolling process, especially the pinholes in the blank area of the pole piece have the greatest impact. However, the leading battery manufacturers will not reduce the requirements for the number and diameter of pinholes due to the thinning of the aluminum foil. On the contrary, they will require higher requirements. In theory, the fewer the number of pinholes, the smaller the diameter, the better. However, whether it is a hot-rolled product or a cast-rolled product, based on the current technical level and control capabilities of the quality of the molten aluminum, the pinhole requirements for battery aluminum foil have basically reached the limit. Therefore, some battery foil billet manufacturers change the ductility of battery aluminum foil by adjusting the content of metals such as Cu and Ti in the battery aluminum foil during the melting and casting stage to reduce the generation of pinholes during the cold rolling process; secondly, by controlling the light transmittance of the rolling oil in the cold rolling stage, the filtration accuracy is improved, and the aluminum powder content in the rolling oil is reduced, thereby controlling the generation of pinholes during the rolling process; thirdly, by controlling the roughness of the rolls in each rolling pass to control the rolling speed and thus the number of pinholes in the aluminum foil; fourthly, by controlling the number of solid dust particles in the workshop air, the influence of dust particles on pinholes in the aluminum foil during the rolling process is reduced; fifthly, by using four passes for intermediate annealing treatment; the tensile strength of the aluminum foil is reduced, the ductility is improved, and the generation of pinholes during the rolling of the finished product is reduced.
[0006] At present, most manufacturers use the above-mentioned means to control the number of pinholes in battery foil. However, the above-mentioned measures are not specific and directional. The first two measures will greatly increase production costs if they are used in long-term production. The third measure reduces pinholes by controlling the rolling speed, which greatly affects production efficiency. The fourth measure is also extremely unstable due to the influence of environmental weather. Although the number of pinholes in the finished product after rolling is improved by the fifth measure, the mechanical properties of the finished product are reduced due to annealing. 3. Summary of the invention:
[0007] The technical problem to be solved by the present invention is: in view of the problem of too many A / B-level pinholes in thin materials in the existing production technology of battery aluminum foil, which is the positive electrode material of power batteries, the present invention provides a production method for reducing A / B-level pinholes in battery aluminum foil without affecting the tensile strength and elongation of the aluminum foil. The technical solution of the present invention improves the pass process of battery aluminum foil in the foil rolling stage, adds a low-temperature annealing process after rough rolling, and significantly reduces the number of A / B-level pinholes in the foil rolling finished product without affecting the performance of battery aluminum foil (tensile strength and elongation).
[0008] In order to solve the above problems, the technical solution adopted by the present invention is:
[0009] The present invention provides a production method for reducing A / B level pinholes in battery aluminum foil, the production method comprising the following steps:
[0010] a. Rough rolling is performed on the 1070 alloy battery aluminum foil blank prepared according to the conventional method, and the rough rolling pass distribution is 220-104-47 μm;
[0011] The rough rolling process is two rolling passes, the rolling force of the first pass is 1400-1800 KN, and the rolling force of the second pass is 1700-2100 KN; the rolling speed of the first pass is ≤650 m / min, and the rolling speed of the second pass is ≤850 m / min; the rough rolling roll Ra is 0.2-0.25 during the rough rolling;
[0012] b. The battery aluminum foil coil obtained after rough rolling is subjected to low-temperature annealing. The annealing temperature is set at 210-230°C. The annealing time is divided into two periods: a 2.5-3.5h heating period and an 8-9h insulation period;
[0013] c. The battery aluminum foil coil obtained after annealing is subjected to intermediate rolling, and the thickness of the coil obtained after intermediate rolling is 23 μm;
[0014] During the intermediate rolling process, the rolling force is 1700-2100 KN, the rolling speed is ≤900 m / min, and the rolling oil conditions are: the intermediate rolling viscosity is 1.9-2.0 cst, and the intermediate rolling roll Ra is 0.12-0.15 during the intermediate rolling;
[0015] d. The battery aluminum foil coil obtained after the intermediate rolling is subjected to finish rolling, and the thickness of the coil obtained after the finish rolling is 13 μm;
[0016] During the finishing rolling process, the rolling force is 2700-3300 KN, and the rolling speed is ≤600 m / min; during the finishing rolling, the finishing roller Ra is 0.10-0.12;
[0017] e. Cut the coil after finish rolling once;
[0018] f. The material roll after the first slitting is subjected to corona fine cutting, and the finished product obtained after corona fine cutting is packaged.
[0019] According to the above-mentioned production method for reducing A / B grade pinholes in battery aluminum foil, the 1070 alloy battery aluminum foil blank in step a has a specification of 0.22*1210mm or 0.22*1470mm, an alloy state of H16, a tensile strength of ≥155MPa, and an elongation of ≥2.7%.
[0020] According to the above-mentioned production method for reducing A / B grade pinholes in battery aluminum foil, the rolling speed of the first pass in step a is 500-650 m / min, and the rolling speed of the second pass is 700-850 m / min.
[0021] According to the above-mentioned production method for reducing A / B grade pinholes in battery aluminum foil, the mechanical properties of the coil before annealing in step b have a tensile strength of 183-193 MPa and an elongation of 3.8-4.5%; the mechanical properties of the coil after annealing have a tensile strength of 170-187 MPa and an elongation of 3.0-4.0%.
[0022] According to the above-mentioned production method for reducing A / B grade pinholes in battery aluminum foil, the rolling speed in step c is 700-900 m / min.
[0023] According to the above-mentioned production method for reducing A / B grade pinholes in battery aluminum foil, the rolling speed in step d is 500-600 m / min.
[0024] According to the above-mentioned production method for reducing A / B grade pinholes in battery aluminum foil, a Comp slitting machine is used for the first slitting in step e, and the first slitting speed is controlled to be 600-750 m / min.
[0025] According to the above-mentioned production method for reducing A / B grade pinholes in battery aluminum foil, in the corona fine cutting process described in step f, a 1750mm wide corona machine is used, and its model is Baolishida. The corona speed is controlled to be 100-120m / min, the corona power is 13-15KW, and the corona number is 1 time; Wanying aluminum foil slitting machine is used for fine cutting, and its fine cutting speed is 200-240m / min.
[0026] The positive beneficial effects of the present invention are:
[0027] 1. The technical solution of the present invention adds a low-temperature annealing process after rough rolling to perform low-temperature annealing on the rough-rolled battery aluminum foil. The annealing temperature is set at 210-230°C, the heating time period is set at 2.5-3.5h, and the heat preservation time period is set at 8-9h. The nature of this annealing is to heat the aluminum coil to a specified temperature, keep it warm for a certain period of time, and then slowly cool it to promote the precipitation of Fe, Si compounds and air in the aluminum foil, and at the same time refine the size of the second phase compound, so as to reduce the generation of pinholes in the subsequent rolling process.
[0028] In addition, the annealing temperature is set relatively low compared to the normal annealing temperature, and the heat preservation period is relatively short. The purpose is to ensure that the internal structure of the aluminum foil will not change or change slightly during the annealing process, thereby ensuring that the tensile strength and elongation of the aluminum foil are not affected or are less affected, and removing the internal stress generated by the aluminum coil during the plastic deformation process. Comparing the tensile strength and the number of A / B grade pinholes of the same alloy battery aluminum foil products produced before and after the addition of the low-temperature annealing process, the following data are summarized:
[0029] Taking 1070 alloy 12μm battery aluminum foil as an example, the tensile strength and the number of A / B grade pinholes of 10 rolls of battery aluminum foil with and without the low temperature annealing process are compared in detail in the attached figure. Figure 1-3 .
[0030] By the attached Figure 1-3 From the comparison, it can be seen that after adding the low-temperature annealing process, the tensile strength of the finished product has basically not changed compared with the finished product without the low-temperature annealing process within the allowable error range, while the number of A / B grade pinholes per 100㎡ has been significantly reduced.
[0031] 2. The technical solution of the present invention uses low roughness rolls from rough rolling, with roughing rolls Ra 0.2-0.25, medium rolls Ra 0.12-0.15, and finishing rolls Ra 0.10-0.12. The roughness of each roll is greatly reduced compared with the existing process. The lower the roll roughness, the slower the rolling speed, and the use of post-tension is relatively small, thereby reducing the generation of pinholes during the rolling process. However, considering the viscosity of the rolling oil in each process, the lower limit of the roll roughness is not set too low to prevent slipping during starting and rolling.
[0032] By using low-roughness rolls in each pass, controlling the rolling speed in each pass, reducing the generation of deformation heat, and extending the service life of the rolls, energy conservation and consumption reduction can be achieved. From production statistics, battery aluminum foil without low-temperature annealing process consumes an average of 2 to 4 more pairs of rolls in the rolling process from the second pass to the finished product than battery aluminum foil with low-temperature annealing.
[0033] 3. In the technical solution of the present invention, in terms of rolling parameters and tension parameter control, each pass uses a large rolling force for rolling, and the rolling force of the finished product is controlled at about 3100KN. The large rolling force can control the rolling speed on the one hand, and then reduce the use of the back tension parameters; each pass uses a small back tension control, and the back tension of the finished product is controlled at 30-38N / mm 2 By changing and controlling the forward slip value during rolling, the aluminum foil shape variable in the rolling direction is increased, thereby reducing the generation of pinholes.
[0034] 4. The technical solution of the present invention uses an online pinhole detection system (EDS) during the slitting production stage to perform online real-time detection of pinholes in the finished coils of the rolling mill, and the pinhole size detection range is Class A: 15-50um, Class B: 50-200um, Class C: 200-500um, Class D>500um.
[0035] In summary, through the technical solution of the present invention, the A-level pinholes of 1070 alloy battery aluminum foil can be reduced to 2 Less than 40, Class B pinholes reduced to every 100m 2 Within 20; after annealing, the tensile strength of the battery foil is maintained at 170-187Mpa, and the elongation of the aluminum foil is maintained at 3.0-4.0%; the finished product meets the mechanical performance requirements of customers after rolling, avoiding subsequent roller breakage due to excessive number of pinholes and excessive hole diameter.
[0036] The technical solution of the present invention does not require frequent replacement of new base oil in order to continuously ensure the high light transmittance of the oil product. A single machine can save more than 45 tons of new base oil per year.
[0037] The technical solution of the present invention does not need to continuously ensure high filtration accuracy, thereby reducing the usage of white clay and diatomaceous earth. A single machine can save more than 5 tons of white clay and diatomaceous earth each year, reducing the output of hazardous waste by 21%.
[0038] In summary, the present invention has significant economic and social benefits. 4. Description of the drawings:
[0039] Figure 1 Comparison of the tensile strength of 1070 alloy 12um battery aluminum foil obtained by adding a low-temperature annealing process and without adding a low-temperature annealing process;
[0040] Figure 2 1070 alloy 12um battery aluminum foil with and without low temperature annealing process, battery aluminum foil finished products per 100m 2 A's line graph comparison;
[0041] Figure 31070 alloy 12um battery aluminum foil with and without low temperature annealing process, battery aluminum foil finished products per 100m 2 B's line chart comparison.
[0042] Figure 4 A graph showing the relationship between the annealing temperature and the number of A / B pinholes obtained in an embodiment of the present invention;
[0043] Figure 5 A graph showing the relationship between the annealing temperature, tensile strength and elongation obtained in the embodiments of the present invention. V. Specific implementation methods:
[0044] The present invention is further described below in conjunction with embodiments, but the protection scope of the technical solution of the present invention is not limited thereto.
[0045] Embodiment 1:
[0046] The present invention provides a production method for reducing A / B grade pinholes in battery aluminum foil without affecting the performance (tensile strength and elongation) of the aluminum foil. The detailed operation steps are as follows:
[0047] a. Rough rolling of 1070 alloy battery aluminum foil blank prepared according to conventional method, with 2 rough rolling passes and pass distribution of 220-104-47μm; the specification of the blank used is 0.22*1210mm, the alloy state is 1070 / H16, the tensile strength is 166MPa, and the elongation is 3.1%; the rolling force of the first pass is 1600±200KN, the rolling speed is 650m / min, the rolling force of the second pass is 1900±200KN, the rolling speed is 850m / min, the viscosity of the rolling oil for the two rough rolling is 2.02cst, the roll roughness is Ra 0.21, and the post tension is controlled to be 25-32N / mm 2 The thickness of the aluminum foil obtained after rolling is 47um. The aluminum coil is divided into three small coils during the second rolling process, namely coil 1, coil 2, and coil 3.
[0048] b. The three small coils obtained after two rough rollings, namely, coil 1, coil 2 and coil 3, are subjected to intermediate low-temperature annealing treatment, wherein the intermediate low-temperature annealing processes are as follows: coil 1 annealing temperature is 180°C, heating section is 3.5h, and heat preservation section is 9h; coil 2 annealing temperature is 190°C, heating section is 3.5h, and heat preservation section is 9h; coil 3 annealing temperature is 200°C, heating section is 3.5h, and heat preservation section is 9h;
[0049] c. The three battery aluminum foil coils obtained after annealing were subjected to intermediate rolling, and the pass reduction distribution was 47-23um; during the intermediate rolling process, the rolling force was controlled to 2000KN, the rolling speed was controlled to 850m / min, the rolling oil viscosity was 1.91cst, the intermediate rolling roll roughness was Ra 0.12, and the post tension was controlled to 35-42N / mm2 ; The thickness of the aluminum foil obtained after rolling is 23um;
[0050] d. The battery aluminum foil coil obtained after the intermediate rolling is subjected to finish rolling. The thickness of the aluminum foil obtained after the finish rolling is 13um. During the finish rolling process, the rolling force is controlled to 3100KN, the rolling speed is controlled to 600m / min, the rolling oil viscosity is 1.85cst, the roll roughness is Ra 0.10, and the post tension is controlled to 30-38N / mm. 2 ;
[0051] e. Cut the finished rolled coil once; the cutting is performed using a Compu slitting machine, and the cutting speed is controlled to be 750 m / min;
[0052] f. The material roll after the first slitting is subjected to a corona finishing treatment. The corona is treated by a 1750mm wide corona machine (Baoleshida), with a corona power of 14Kw and a speed of 120m / min; the finishing machine (Wanying) has a speed of 240m / min.
[0053] After testing, the battery aluminum foil prepared in this embodiment has a 2 The number of internal A / B grade pinholes, tensile strength MPa, and elongation % are detailed in Table 1.
[0054] Table 1 Example 1 Battery aluminum foil obtained per 100m 2 Number of internal A / B grade pinholes and tensile strength MPa, elongation %
[0055]
[0056] Embodiment 2:
[0057] The present invention provides a production method for reducing A / B grade pinholes in battery aluminum foil without affecting the performance (tensile strength and elongation) of the aluminum foil. The detailed operation steps are basically the same as those in Example 1, except that:
[0058] In step a: the specification of the blank used is 0.22*1470mm, the alloy state is 1070 / H16, the tensile strength is 175MPa, and the elongation is 3.0%;
[0059] In step b: the aluminum coil after two passes of rough rolling is divided into coil 4 and coil 5, and the obtained coils 4 and 5 are subjected to intermediate low-temperature annealing treatment, wherein the intermediate low-temperature annealing processes are: the annealing temperature of coil 4 is 210°C, the heating section is 3.5h, and the insulation section is 9h; the annealing temperature of coil 5 is 220°C, the heating section is 3.5h, and the insulation section is 9h.
[0060] After testing, the battery aluminum foil prepared in this embodiment has a 2 The number of internal A / B grade pinholes, tensile strength MPa, and elongation % are detailed in Table 2.
[0061] Table 2 Battery aluminum foil obtained in Example 2 per 100m 2 Number of internal A / B grade pinholes and tensile strength MPa, elongation %
[0062]
[0063] Embodiment 3:
[0064] The present invention provides a production method for reducing A / B grade pinholes in battery aluminum foil without affecting the performance (tensile strength and elongation) of the aluminum foil. The detailed operation steps are basically the same as those in Example 1, except that:
[0065] In step a: the specification of the blank used is 0.22*1470mm, the alloy state is 1070 / H16, the tensile strength is 175MPa, and the elongation is 3.0%;
[0066] In step b: the aluminum coil after two passes of rough rolling is divided into coil 6, coil 7 and coil 8, and the obtained coil 6, coil 7 and coil 8 are subjected to intermediate low-temperature annealing treatment, wherein the intermediate low-temperature annealing processes are as follows: the annealing temperature of coil 6 is 220°C, the heating section is 3.5h, and the insulation section is 9h; the annealing temperature of coil 7 is 240°C, the heating section is 3.5h, and the insulation section is 9h; the annealing temperature of coil 8 is 245°C, the heating section is 3.5h, and the insulation section is 9h.
[0067] After testing, the battery aluminum foil prepared in this embodiment has a 2 The number of internal A / B grade pinholes, tensile strength MPa, and elongation % are detailed in Table 3.
[0068] Table 3 Battery aluminum foil obtained in Example 3 per 100m 2 Number of internal A / B grade pinholes and tensile strength MPa, elongation %
[0069]
[0070] The data in Table 4 can be obtained by combining the data in the above embodiments.
[0071] Table 4 Battery aluminum foil obtained in the present invention per 100m 2 Number of internal A / B grade pinholes and tensile strength MPa, elongation %
[0072]
[0073] From the data in Table 4, it can be seen that when the annealing temperature is between 210 and 230 °C, the A / B grade pinholes of the finished product after rolling are controlled at 2The number of pinholes in the finished product is within 40 and within 20, and the tensile strength and elongation of the aluminum foil have no decreasing trend within the error range; when the annealing temperature reaches above 230℃, the number of A / B pinholes in the finished product has no significant improvement compared with 230℃, but its tensile strength and elongation are significantly reduced (the relationship between the annealing temperature and the number of A / B pinholes is shown in the attached figure). Figure 4 The relationship between annealing temperature, tensile strength and elongation is shown in the attached figure. Figure 5 ).
Claims
1. A production method for reducing A / B grade pinholes in battery aluminum foil, characterized in that: The production method comprises the following steps: a. Rough rolling is performed on the 1070 alloy battery aluminum foil blank prepared according to the conventional method, and the rough rolling pass distribution is 220-104-47 μm; The rough rolling process is two rolling passes, the rolling force of the first pass is 1400-1800 KN, and the rolling force of the second pass is 1700-2100 KN; the rolling speed of the first pass is ≤650 m / min, and the rolling speed of the second pass is ≤850 m / min; the rough rolling roll Ra is 0.2-0.25 during the rough rolling; b. The battery aluminum foil coil obtained after rough rolling is subjected to low-temperature annealing. The annealing temperature is set at 210-230°C. The annealing time is divided into two periods: a 2.5-3.5h heating period and an 8-9h insulation period; c. The battery aluminum foil coil obtained after annealing is subjected to intermediate rolling, and the thickness of the coil obtained after intermediate rolling is 23 μm; During the intermediate rolling process, the rolling force is 1700-2100 KN, the rolling speed is ≤900 m / min, and the rolling oil conditions are: the intermediate rolling viscosity is 1.9-2.0 cst, and the intermediate rolling roll Ra is 0.12-0.15 during the intermediate rolling; d. The battery aluminum foil coil obtained after the intermediate rolling is subjected to finish rolling, and the thickness of the coil obtained after the finish rolling is 13 μm; During the finishing rolling process, the rolling force is 2700-3300 KN, and the rolling speed is ≤600 m / min; during the finishing rolling, the finishing roller Ra is 0.10-0.12; e. Cut the coil after finish rolling once; f. The material roll after the first slitting is subjected to corona fine cutting, and the finished product obtained after corona fine cutting is packaged.
2. The production method for reducing A / B grade pinholes in battery aluminum foil according to claim 1, characterized in that: The 1070 alloy battery aluminum foil blank described in step a has a specification of 0.22*1210mm or 0.22*1470mm, an alloy state of H16, a tensile strength of ≥155MPa, and an elongation of ≥2.7%.
3. The production method for reducing A / B grade pinholes in battery aluminum foil according to claim 1, characterized in that: The rolling speed of the first pass in step a is 500-650 m / min, and the rolling speed of the second pass is 700-850 m / min.
4. The production method for reducing A / B grade pinholes in battery aluminum foil according to claim 1, characterized in that: In step b, the mechanical properties of the coil before annealing are tensile strength of 183-193 MPa and elongation of 3.8-4.5%; the mechanical properties of the coil after annealing are tensile strength of 170-187 MPa and elongation of 3.0-4.0%.
5. The production method for reducing A / B grade pinholes in battery aluminum foil according to claim 1, characterized in that: The rolling speed in step c is 700-900 m / min.
6. The production method for reducing A / B grade pinholes in battery aluminum foil according to claim 1, characterized in that: The rolling speed in step d is 500-600 m / min.
7. The production method for reducing A / B grade pinholes in battery aluminum foil according to claim 1, characterized in that: The primary slitting in step e is performed using a Compu slitting machine, and the primary slitting speed is controlled to be 600-750 m / min.
8. The production method for reducing A / B grade pinholes in battery aluminum foil according to claim 1, characterized in that: In the corona finishing process described in step f, a 1750 mm wide corona machine is used, whose model is Baolishida, and the corona speed is controlled to be 100-120 m / min, the corona power is 13-15 KW, and the corona number is 1 time; a Wanying aluminum foil slitting machine is used for finishing, and its finishing speed is 200-240 m / min.
Citation Information
Patent Citations
Low-pinhole ultra-wide battery foil for new energy battery and preparation method of low-pinhole ultra-wide battery foil
CN115094275A
Unequal-thickness triple rolling method for ultrathin aluminum foil
CN116078818A
Technological method for reducing pinholes of finished aluminum foil
CN116116896A
Preparation method of lithium iron phosphate battery aluminum foil
CN117732876A
Manufacture of aluminum foil base
JP1989218702A
Cited By
Production method of aluminum foil base material for copper plating of PCB copper-aluminum composite foil
CN119819713A