Processing method of aluminum-scandium alloy target material for casting molding

By coarse grinding and ultrasonic flaw detection of aluminum scandium alloy target blanks, combined with wire cutting and fine grinding, the problem of high scandium content aluminum scandium alloy targets is solved, and the pass rate of the target is improved. stability.

CN119077288APending Publication Date: 2024-12-06LEADING THIN FILM MATERIALS (JIANGSU) CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411044442.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-31
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

High scandium content aluminum scandium alloy targets are prone to cracks, edge collapse and overall fragmentation during machining. Especially when the thickness of the target blank is less than 10mm, the pass rate is low and there is a lack of effective solutions.

Method used

By roughly grinding the bottom and top surfaces of the aluminum scandium alloy target blank, the roughness of the surface is reduced, the defect location and area is determined using ultrasonic flaw detection, wire cutting and fine grinding of the minimum defect area is performed, and finally polishing is performed to obtain the finished target material.

Benefits of technology

The pass rate of aluminum scandium alloy targets during machining is improved, the occurrence of adverse phenomena is reduced, and the stability and use efficiency of the target are ensured.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119077288A_ABST
    Figure CN119077288A_ABST
Patent Text Reader

Abstract

The invention relates to the field of target material preparation, and discloses a processing method of an aluminum-scandium alloy target material for casting molding, which comprises the following steps: step 1, carrying out bottom surface coarse grinding and top surface coarse grinding on an aluminum-scandium alloy target blank to obtain a coarse grinding target blank; the horizontal distance between the edge of the grinding surface of the bottom surface of the roughly ground target blank and the contour edge of the aluminum-scandium alloy target blank is 10-20mm; 2, ultrasonic flaw detection is conducted on the rough grinding target blank, and the position, the area and the depth of the defect of the rough grinding target blank are obtained; 3, according to the positions and the areas of the defects, linear cutting is conducted on the rough grinding target blank in the mode that the minimum defect area is contained, and a linear cutting target blank is obtained; and 4, the wire-cut target blank is subjected to accurate grinding and polishing, and a finished product target material is obtained. By the adoption of the machining method, the conditions of cracks, edge breakage and local and even overall fragmentation of the aluminum-scandium alloy target material in the machining process can be reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of target material preparation, and in particular to a processing method of an aluminum-scandium alloy target material for casting. Background Art

[0002] The aluminum-scandium target prepared by the melting and casting method can improve the stress of the sputtered film and the stability of the end product. However, in the aluminum-scandium alloy with a high scandium content, the brittleness of the alloy increases due to the almost non-existence of the single phase of aluminum. During the machining process, the aluminum-scandium alloy target blank is very prone to defects such as cracks and edge collapse, and even direct breakage. As the thickness of the aluminum-scandium alloy target blank continues to decrease, the probability of this problem occurring increases.

[0003] In order to solve the above problems, attempts were made to change the thickness of the target blank during casting. However, increasing the target blank thickness during the casting process cannot reduce the risk of target blank breakage when the target blank is close to the finished product thickness, and may even greatly increase the cost of raw materials and the time cost during machining. Reducing the target blank thickness during the casting process will produce a large number of pores inside the target blank, resulting in a small number of usable parts and a low pass rate. There is currently no better way to solve the problem of cracks, edge collapse, partial or even overall breakage of the target blank during machining of aluminum-scandium alloy targets with high scandium content, especially when the target blank thickness is less than 10mm.

[0004] CN202111091816.6 discloses a silicon carbide target assembly and a preparation method thereof, the preparation method comprising the following steps: (1) cutting, rough grinding, wire cutting and fine grinding of silicon carbide target blanks in sequence to obtain silicon carbide target; (2) brazing the back plate and the silicon carbide target obtained in step (1) to obtain a silicon carbide target semi-finished product assembly; (3) heat shaping and polishing the silicon carbide target semi-finished product assembly obtained in step (2) in sequence to obtain a silicon carbide target assembly; during the wire cutting process in step (1), the tool path depth is ≤0.2mm; the temperature of the heat shaping in step (3) is 200-220°C. The preparation method provided by the invention is simple and easy to operate, solves the cracking phenomenon during the welding of silicon carbide target, improves the bonding rate between silicon carbide target and back plate, and reduces the single defect rate.

[0005] The comparative document prepares silicon carbide targets by rough grinding, wire cutting, fine grinding, and then brazing.

[0006] CN112951348A discloses a method for manufacturing an AlSc target material for improving the yield rate of chip manufacturing. By using an ultrasonic flaw detector to obtain an internal image of an aluminum-scandium target material, it is possible to clearly know whether the aluminum-scandium target material has defects inside. By comparing the size information of the defect with the preset size information, it is possible to clearly obtain three results: the aluminum-scandium target material is a qualified product, an unqualified product but meets the repair standard, and an unqualified product and does not meet the repair standard. Through the subsequent target material repairing step, the defects of the unqualified aluminum-scandium target material that meets the repair standard can be removed, so that the originally unqualified aluminum-scandium target material can be converted into a qualified product. The yield rate of the aluminum-scandium target material is improved, and the manufacturing cost of the aluminum-scandium target material is reduced. In addition, while ensuring the yield rate of the aluminum-scandium target material, the phenomenon of arcing and the like in the process flow of the aluminum-scandium target material actually used in chip manufacturing is correspondingly reduced.

[0007] The comparative document uses an ultrasonic flaw detector to detect aluminum-scandium targets, and then performs analysis and grinding based on the detection results. However, this method is mainly for die-cast aluminum-scandium targets, and is not completely applicable to cast aluminum-scandium targets.

[0008] Therefore, the technical problem to be solved by the present invention is: how to improve the qualified rate of aluminum-scandium alloy target during machining. Summary of the invention

[0009] The main purpose of the present invention is to provide a processing method for an aluminum-scandium alloy target material for casting, by first coarsely grinding the aluminum-scandium alloy target blank to reduce the roughness of the target blank's surface, thereby facilitating ultrasonic flaw detection of the target blank and making targeted adjustments according to the defect positions of the target blank, thereby reducing the undesirable phenomena of the aluminum-scandium alloy target material during the machining process.

[0010] To achieve the above objectives, the technical solutions adopted in this application are:

[0011] A method for processing an aluminum-scandium alloy target material for casting, comprising the following steps:

[0012] Step 1: performing bottom surface rough grinding and top surface rough grinding on the aluminum-scandium alloy target blank to obtain a rough-ground target blank;

[0013] The horizontal distance between the edge of the grinding surface of the bottom surface of the rough-ground target blank and the contour edge of the aluminum-scandium alloy target blank is 10 to 20 mm;

[0014] Step 2: Perform ultrasonic flaw detection on the rough-ground target blank to obtain the position, area and depth of the defects of the rough-ground target blank;

[0015] Step 3: According to the position and area of ​​the defect, the rough ground target blank is wire cut in a manner that includes the minimum defect area to obtain a wire cut target blank;

[0016] Step 4: Fine grinding and polishing the wire-cut target blank to obtain the finished target material.

[0017] In the solution of the present invention, the distance between the edge of the area of ​​the bottom surface of the aluminum-scandium alloy target blank after processing and the edge of the target blank can be selected to be 10 mm, 12 mm, 14 mm, 16 mm, 18 mm, or 20 mm.

[0018] Preferably, in step 1, the feed amount of the bottom surface rough grinding is 2 to 3 μm; the feed amount of the top surface rough grinding is 2 to 3 μm.

[0019] In the scheme of the present invention, the feed amount for rough grinding of the bottom surface can be selected as 2μm, 2.2μm, 2.4μm, 2.6μm, 2.8μm, and 3μm; the feed amount for rough grinding of the top surface can be selected as 2μm, 2.2μm, 2.4μm, 2.6μm, 2.8μm, and 3μm.

[0020] Preferably, the thickness of the roughly ground target blank is 2 to 3 mm greater than the thickness of the finished target blank.

[0021] In the solution of the present invention, the thickness of the roughly ground target blank is larger than the size of the finished target material, including but not limited to 2 mm, 2.2 mm, 2.4 mm, 2.6 mm, 2.8 mm, and 3 mm.

[0022] Preferably, the step 2 specifically includes: using an ultrasonic flaw detector to perform flaw detection on the top surface and / or bottom surface of the semi-finished target material to obtain the position, area and depth of the defects.

[0023] Preferably, the diameter of the wire-cut target blank is 0.5 to 1 mm larger than the diameter of the finished target material.

[0024] In the solution of the present invention, the diameter of the wire-cut target blank is larger than the diameter of the finished target material, including but not limited to 0.5 mm, 0.6 mm, 0.7 mm, 0.8 mm, 0.9 mm, and 1 mm.

[0025] Preferably, in step 4, the feed amount of fine grinding is 1-2 μm, and the mesh number of the grinding wheel is 300-400 meshes.

[0026] In the solution of the present invention, the feed amount is preferably 1 μm, 1.2 μm, 1.4 μm, 1.6 μm, 1.8 μm, and 2 μm; the mesh size of the grinding wheel is preferably 300 mesh, 320 mesh, 340 mesh, 360 mesh, 380 mesh, and 400 mesh.

[0027] Preferably, the step 1 specifically comprises: determining the initial thickness of the bottom surface and the top surface of the aluminum-scandium alloy target blank respectively by a multi-point tool setting method, and performing bottom surface rough grinding and top surface rough grinding on the aluminum-scandium alloy target blank to obtain a rough-ground target blank;

[0028] The multi-point tool setting method is specifically as follows: the grinding wheel is lowered until it contacts the surface of the aluminum-scandium alloy target blank, and the height of the contact point is recorded. The heights of contact points at multiple different positions are recorded in the same way and compared, and the maximum height is used as the initial thickness of the aluminum-scandium alloy target blank.

[0029] Preferably, in step 4, a polishing cloth is used to polish the side surface of the wire-cut target blank.

[0030] Compared with the prior art, this solution has the following beneficial effects:

[0031] 1. The processing method of the present invention performs rough grinding on the bottom surface of the aluminum-scandium alloy target blank, and the horizontal distance between the edge of the grinding surface of the bottom surface and the contour edge of the aluminum-scandium alloy target blank is 10 to 20 mm, and the remaining rough grinding allowance is ground by the top surface of the aluminum-scandium alloy target blank. In this way, a smoother plane can be provided for the next flaw detection process to improve the flaw detection accuracy. Secondly, by retaining the bottom surface of the aluminum-scandium alloy target blank as much as possible, more processing allowance is left for subsequent defect removal by wire cutting and fine grinding according to the flaw detection structure, thereby improving the qualified rate of aluminum-scandium alloy target blank machining.

[0032] 2. The processing method of the present invention finds the highest point of the target blank through multiple measurements, and uses this height as the initial grinding height of the target blank, thereby avoiding excessive processing volume in a single grinding process, which causes the aluminum-scandium alloy target blank to be subjected to too much force and cause the aluminum-scandium alloy target blank to break. BRIEF DESCRIPTION OF THE DRAWINGS

[0033] Figure 1 is a step diagram of the processing method of Example 1;

[0034] Figure 2 This is a diagram showing the effect of rough grinding of the bottom surface of the target blank in Example 1;

[0035] Figure 3 This is a diagram showing the effect of rough grinding of the top surface of the target blank in Example 1;

[0036] Figure 4 This is a rendering of the target blank wire cutting trajectory of Example 1;

[0037] Figure 5 This is a rendering of the target blank of Example 1 with the gasket and fixture installed;

[0038] Figure 6 This is a rendering of the finished target material of Example 1;

[0039] Figure 7 Schematic diagram of the multi-point tool setting method of Example 4. DETAILED DESCRIPTION

[0040] In order to make the purpose, technical solution and advantages of the embodiments of the present application clearer, the technical solution in the embodiments of the present application will be clearly and completely described below in conjunction with the drawings in the embodiments of the present application. Obviously, the described embodiments are part of the embodiments of the present application, not all of the embodiments. The components of the present application implemented as described and shown in the drawings here can be arranged and designed in various different configurations.

[0041] Example 1

[0042] refer to Figure 1-6 A method for processing an aluminum-scandium alloy target for casting, comprising the following steps:

[0043] Step 1: performing bottom surface rough grinding and top surface rough grinding on an aluminum-scandium alloy (30at% AlSc) target blank to obtain a rough-ground target blank;

[0044] In this embodiment, step 1 is specifically as follows: obtaining a cast aluminum-scandium alloy target blank with a diameter of 400 mm and a thickness of 20 mm, placing the aluminum-scandium alloy target blank on a grinding machine, lowering the grinding wheel to a position where it just contacts the aluminum-scandium alloy target blank, which is the initial thickness of the bottom surface of the aluminum-scandium alloy target blank, and then rough-grinding the bottom surface of the aluminum-scandium alloy target blank from the initial thickness, with a feed amount of 2.5 μm for rough grinding of the bottom surface, until the horizontal distance between the edge of the grinding surface of the bottom surface and the contour edge of the aluminum-scandium alloy target blank is 15 mm; after the bottom surface of the aluminum-scandium alloy target blank is processed, the initial thickness of the top surface of the aluminum-scandium alloy target blank is determined in the same manner, and then the top surface of the aluminum-scandium alloy target blank is rough-grinded, with a feed amount of 2.5 μm for rough grinding of the top surface, until the thickness of the rough-ground target blank is 10 mm.

[0045] It should be noted that the grinding surface of the bottom surface of the rough-ground target blank is the grinding surface formed after the bottom surface is rough-ground. Since the aluminum-scandium alloy target blank is formed by casting, the bottom surface of the aluminum-scandium alloy target blank will be slightly convex outward. Therefore, when the bottom surface of the aluminum-scandium alloy target blank is rough-ground, the convexity of the bottom surface will be rough-ground first. At this time, there is a horizontal distance between the grinding surface of the bottom surface of the rough-ground target blank and the contour edge of the aluminum-scandium alloy target blank until the convexity is completely ground, and the horizontal distance between the edge of the grinding surface of the bottom surface and the contour edge of the aluminum-scandium alloy target blank is 15 mm, that is, the convexity is not completely removed, and part of the convexity is retained.

[0046] Step 2: Use an ultrasonic flaw detector to detect the rough ground target blank to obtain the position, area and depth of the defects in the rough ground target blank;

[0047] In this embodiment, an ultrasonic flaw detector is used to detect the bottom surface of the rough ground target blank to obtain the position, area and depth of the defects of the rough ground target blank;

[0048] Step 3: According to the position and area of ​​the defect, the rough ground target blank is wire cut in a manner that includes the minimum defect area to obtain a wire cut target blank;

[0049] In this embodiment, step 3 is specifically as follows: a thin aluminum plate with a diameter of 311 mm is used as a tool for drawing the wire cutting trajectory, the thin aluminum plate is placed on the bottom surface of the rough ground target blank, and the thin aluminum plate is moved according to the position and area of ​​the defect obtained by flaw detection until the defect area covered by the thin aluminum plate is the smallest, and the wire cutting trajectory is drawn along the edge of the thin aluminum plate. After the wire cutting trajectory is drawn on the rough ground target blank, the rough ground target blank is placed on the wire cutting machine for wire cutting, and the rough ground target blank is wire cut in a manner that includes the least defect area. After the wire cutting is completed, a wire cutting target blank with a diameter of 311 mm is obtained.

[0050] Secondly, when performing wire cutting on the rough-ground target blanks, three pause positions are set, that is, the machine needs to be stopped once every time 25% of the circumference of the rough-ground target blanks is cut. During the pause, pads and clamps are installed on the semi-finished target materials to reduce cracks or edge collapse caused by local stress on the semi-finished target materials. After the installation is completed, wire cutting continues.

[0051] Step 4: Fine grinding and polishing the wire-cut target blank to obtain the finished target material.

[0052] In this embodiment, step 4 is specifically as follows: placing the wire cut target blank on a grinding machine, and fine grinding the wire cut target blank according to the position and depth of the defect obtained by flaw detection. If the defect position is close to the bottom surface of the wire cut target blank, fine grinding is performed from the bottom surface of the wire cut target blank; if the defect position is close to the top surface of the wire cut target blank, fine grinding is performed from the top surface of the wire cut target blank. The feed amount of fine grinding is 1.5 μm, and the mesh number of the grinding wheel used is 350 mesh. After fine grinding, the side of the wire cut target blank is polished with a polishing cloth to remove the cutting lines and the oxidized surface to obtain a finished target material. The diameter of the finished target material is 310 mm and the thickness is 8 mm.

[0053] Example 2

[0054] This embodiment is basically the same as Embodiment 1, with the only difference being that in step 1: the horizontal distance between the edge of the grinding surface of the bottom surface and the contour edge of the aluminum-scandium alloy target blank is 10 mm.

[0055] Example 3

[0056] This embodiment is basically the same as the embodiment 1, and the only difference is that in step 1: the horizontal distance between the edge of the grinding surface of the bottom surface and the contour edge of the aluminum-scandium alloy target blank is 20 mm.

[0057] Example 4

[0058] refer to Figure 7 This embodiment is basically the same as embodiment 1, and the only difference is that in step 1: a multi-point tool setting method is used to determine the initial thickness of the bottom surface and the initial thickness of the top surface of the aluminum-scandium alloy target blank.

[0059] The multi-point tool setting method is as follows: the grinding wheel is lowered to contact the surface of the aluminum-scandium alloy target blank, and the height of the contact point is recorded. The heights of the contact points at five different positions are recorded in the same way and compared, and the maximum height is taken as the initial thickness of the aluminum-scandium alloy target blank.

[0060] Example 5

[0061] This embodiment is basically the same as the embodiment 1, and the only difference is that: in step 1: the feed amount of the bottom surface rough grinding is 2 μm; the feed amount of the top surface rough grinding is 2 μm; the thickness of the rough ground target blank is 11 mm;

[0062] In step 2: using an ultrasonic flaw detector to detect flaws on the top surface of the rough ground target blank;

[0063] In step 3: a thin aluminum plate with a diameter of 310.5 mm is used as a tool for drawing the wire cutting trajectory line, and the diameter of the wire cutting target blank is 310.5 mm;

[0064] In step 4: the feed amount of fine grinding is 2 μm, and the mesh size of the grinding wheel is 400 mesh.

[0065] Example 6

[0066] This embodiment is basically the same as the embodiment 1, and the only difference is that: in step 1: the feed amount of the bottom surface rough grinding is 3 μm; the feed amount of the top surface rough grinding is 3 μm; the thickness of the rough ground target blank is 10.5 mm;

[0067] In step 2: using an ultrasonic flaw detector to detect flaws on the top and bottom surfaces of the rough-ground target blank;

[0068] In step 3: a thin aluminum plate with a diameter of 310.8 mm is used as a tool for drawing the wire cutting trajectory line, and the diameter of the wire cutting target blank is 310.8 mm;

[0069] In step 4: the feed amount of fine grinding is 1 μm, and the mesh number of the grinding wheel is 300 mesh.

[0070] Comparative Example 1

[0071] It is basically the same as Example 1, except that:

[0072] Step 1: Use an ultrasonic flaw detector to perform flaw detection on the bottom surface of a cast aluminum-scandium alloy target blank having a diameter of 400 mm and a thickness of 20 mm to obtain the position, area and depth of defects in the aluminum-scandium alloy target blank; the aluminum-scandium alloy target blank is a 30at% AlSc target blank.

[0073] Step 2: Place the aluminum-scandium alloy target blank that has completed ultrasonic flaw detection on a grinding machine, and lower the grinding wheel to the position where it just contacts the aluminum-scandium alloy target blank, which is the initial thickness of the bottom surface of the aluminum-scandium alloy target blank. Rough grinding is performed on the bottom surface of the aluminum-scandium alloy target blank from the initial thickness, with a feed amount of 2.5 μm for rough grinding of the bottom surface, until the horizontal distance between the edge of the grinding surface of the bottom surface and the contour edge of the aluminum-scandium alloy target blank is 15 mm. After the bottom surface of the aluminum-scandium alloy target blank is processed, the initial thickness of the top surface of the aluminum-scandium alloy target blank is determined in the same way, and then the top surface of the aluminum-scandium alloy target blank is rough ground, with a feed amount of 2.5 μm for rough grinding of the top surface, until the thickness of the rough-ground target blank is 10 mm.

[0074] Step 3: Use a thin aluminum plate with a diameter of 311 mm as a tool to draw the wire cutting trajectory. Place the thin aluminum plate on the bottom surface of the rough ground target blank. According to the position and area of ​​the defect obtained by flaw detection, move the thin aluminum plate until the defect area covered by the thin aluminum plate is the smallest, and draw the wire cutting trajectory along the edge of the thin aluminum plate. After drawing the wire cutting trajectory on the rough ground target blank, place the rough ground target blank on the wire cutting machine for wire cutting, so as to achieve wire cutting of the rough ground target blank in a manner that contains the least defect area. After the wire cutting is completed, a wire cutting target blank with a diameter of 311 mm is obtained.

[0075] Secondly, when performing wire cutting on the rough-ground target blanks, three pause positions are set, that is, the machine needs to be stopped once every time 25% of the circumference of the rough-ground target blanks is cut. During the pause, pads and clamps are installed on the semi-finished target materials to reduce cracks or edge collapse caused by local stress on the semi-finished target materials. After the installation is completed, wire cutting continues.

[0076] Step 4: Place the wire cut target blank on the grinder, and fine grind the wire cut target blank according to the position and depth of the defect obtained by flaw detection. If the defect position is close to the bottom surface of the wire cut target blank, fine grind from the bottom surface of the wire cut target blank; if the defect position is close to the top surface of the wire cut target blank, fine grind from the top surface of the wire cut target blank. The feed amount of fine grinding is 1.5μm, and the mesh number of the grinding wheel used is 350 mesh. After fine grinding, polish the side of the wire cut target blank with a polishing cloth to remove the cutting lines and oxidation surface to obtain a finished target material with a diameter of 310mm and a thickness of 8mm.

[0077] Comparative Example 2

[0078] It is basically the same as Example 1, with the only difference being that in step 1: when the bottom surface and top surface of the aluminum-scandium alloy target are roughly ground, the grinding amount of the bottom surface rough grinding and the top surface rough grinding are equal, and the bottom surface rough grinding and the top surface rough grinding are ground by 5 mm respectively.

[0079] Comparative Example 3

[0080] It is basically the same as Example 1, with the only difference being that in step 1: the horizontal distance between the edge of the grinding surface of the bottom surface and the contour edge of the aluminum-scandium alloy target blank is 5 mm.

[0081] Comparative Example 4

[0082] It is basically the same as Example 1, with the only difference being that in step 1: the horizontal distance between the edge of the grinding surface of the bottom surface and the contour edge of the aluminum-scandium alloy target blank is 50 mm.

[0083] The aluminum-scandium alloy target materials were processed by the processing methods of Examples 1 to 6 and Comparative Examples 1 to 4, respectively. The testing method was as follows: 23 aluminum-scandium alloy target blanks were processed, and the aluminum-scandium alloy target materials after machining were detected by a water-immersion ultrasonic flaw detector to obtain the number of defect-free aluminum-scandium alloy targets, thereby obtaining the qualified rate of the aluminum-scandium alloy targets. The results are shown in Table 1:

[0084] Table 1 Qualified rate of aluminum-scandium alloy target

[0085] Group Pass rate Group Pass rate Example 1 65.2% Comparative Example 1 21.7% Example 2 62.9% Comparative Example 2 26.1% Example 3 63.6% Comparative Example 3 52.2% Example 4 73.4% Comparative Example 4 56.5% Example 5 63.6% Example 6 64.1%

[0086] Result analysis:

[0087] According to Examples 1, 2 and 3, after the rough grinding of the bottom surface of the aluminum-scandium alloy target blank, the horizontal distance between the edge of the ground surface of the bottom surface of the aluminum-scandium alloy target blank and the contour edge of the aluminum-scandium alloy target blank is 10 to 20 mm, and the qualified rate does not fluctuate much.

[0088] Compared with Example 4, Example 1 uses a single tool setting method to determine the initial thickness, that is, the position where the grinding wheel just contacts the aluminum-scandium alloy target blank is the initial thickness of the bottom surface of the aluminum-scandium alloy target blank; while Example 4 uses multiple tool setting methods to determine the initial thickness, that is, the heights of the contact points at five different positions are recorded and compared in the same way, and the maximum height is used as the initial thickness of the aluminum-scandium alloy target blank. Since the aluminum-scandium alloy target blank is formed by casting, its surface may be uneven. Multiple tool setting can determine the highest point (i.e., the initial thickness) on the surface of the aluminum-scandium alloy target blank. By starting grinding from the highest point, excessive single grinding can be avoided, which may cause cracks or damage on the surface of the aluminum-scandium alloy target blank. From the perspective of the qualified rate, Example 4 is the best.

[0089] According to Examples 1, 5, and 6, the qualified rate does not fluctuate much, and the qualified rate can be improved within the corresponding parameter range.

[0090] Compared with Example 1, the qualified rate of the target material in Example 1 is significantly higher than that in Example 1. The reason is that: since this scheme is mainly for the cast aluminum-scandium alloy target blank, the roughness of the target blank surface is relatively large after the casting is completed, and direct ultrasonic flaw detection will affect the accuracy of ultrasonic flaw detection. After rough grinding, ultrasonic flaw detection is performed. Rough grinding can reduce the roughness of the target blank surface and improve the accuracy of ultrasonic flaw detection. Secondly, flaw detection after rough grinding can reduce the consumption of the defect-free part of the target blank, leaving more margin to eliminate the defect after the specific defect position is obtained by flaw detection, proving that the timing of ultrasonic flaw detection has a synergistic effect with the rough grinding of the bottom surface.

[0091] Compared with Example 2, Example 1 has a higher qualified rate than Comparative Example 2, because: since the bottom surface of the aluminum-scandium alloy target blank formed by casting has fewer defects, the bottom surface of the aluminum-scandium alloy target blank can be retained as much as possible by the method of Example 1, so that the subsequent wire cutting and fine grinding have more margin to remove the defects of the aluminum-scandium alloy target blank, thereby improving the qualified rate of the target material. In Comparative Example 2, the grinding amount of the bottom surface rough grinding and the top surface rough grinding is the same. In this way, the defects may be closer to the size of the finished target material, so that the defects cannot be removed, resulting in the scrapping of the target material, thereby reducing the qualified rate.

[0092] Compared with Example 1 and Comparative Example 3, the qualified rate of Example 1 is higher than that of Comparative Example 3. The reason is that the horizontal distance between the edge of the grinding surface of the bottom surface in Comparative Example 3 and the contour edge of the aluminum-scandium alloy target blank is 5 mm, that is, the thickness of the retained bottom surface of the aluminum-scandium alloy target blank is relatively small, which reduces the processing allowance for subsequent wire cutting and fine grinding to remove defects, so that some defects cannot be removed, thereby reducing the qualified rate.

[0093] Compared with Example 4, Example 1 has a higher pass rate than Example 4. The reason is that in Example 4, the horizontal distance between the edge of the ground surface of the bottom surface and the contour edge of the aluminum-scandium alloy target blank is 50 mm. Comparative Example 4 retains more of the bottom surface of the aluminum-scandium alloy target blank. However, at the same time, too much unground area of ​​the bottom surface will affect the accuracy of the ultrasonic flaw detector, and in the subsequent wire cutting process, it increases the difficulty of using a thin aluminum plate to draw a cutting trajectory line. Secondly, the area of ​​the bottom surface fine grinding is increased, the fine grinding time is increased, and the efficiency and pass rate are reduced.

[0094] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the claims and their equivalents.

Claims

1. A method for processing an aluminum-scandium alloy target for casting, characterized in that: The following steps are involved: Step 1: performing bottom surface rough grinding and top surface rough grinding on the aluminum-scandium alloy target blank to obtain a rough-ground target blank; The horizontal distance between the edge of the grinding surface of the bottom surface of the rough-ground target blank and the contour edge of the aluminum-scandium alloy target blank is 10 to 20 mm; Step 2: Perform ultrasonic flaw detection on the rough-ground target blank to obtain the position, area and depth of the defects of the rough-ground target blank; Step 3: According to the position and area of ​​the defect, the rough ground target blank is wire cut in a manner that includes the minimum defect area to obtain a wire cut target blank; Step 4: Fine grinding and polishing the wire-cut target blank to obtain the finished target material.

2. The method for processing the aluminum-scandium alloy target for casting according to claim 1, characterized in that: In the step 1, the feed amount of the bottom surface rough grinding is 2 to 3 μm; the feed amount of the top surface rough grinding is 2 to 3 μm.

3. The method for processing the aluminum-scandium alloy target for casting according to claim 1, characterized in that: The thickness of the roughly ground target blank is 2 to 3 mm greater than the thickness of the finished target blank.

4. The method for processing the aluminum-scandium alloy target for casting according to claim 1, characterized in that: The step 2 specifically includes: using an ultrasonic flaw detector to detect the top surface and / or bottom surface of the semi-finished target material to obtain the position, area and depth of the defects.

5. The method for processing the aluminum-scandium alloy target for casting according to claim 1, characterized in that: The diameter of the wire-cut target blank is 0.5 to 1 mm larger than the diameter of the finished target material.

6. The method for processing the aluminum-scandium alloy target for casting according to claim 1, characterized in that: In step 4, the feed amount of fine grinding is 1-2 μm, and the mesh number of the grinding wheel is 300-400 meshes.

7. The method for processing an aluminum-scandium alloy target for casting according to claim 1, characterized in that: The step 1 specifically comprises: determining the initial thickness of the bottom surface and the top surface of the aluminum-scandium alloy target blank respectively by a multi-point tool setting method, and performing bottom surface rough grinding and top surface rough grinding on the aluminum-scandium alloy target blank to obtain a rough-ground target blank; The multi-point tool setting method is specifically as follows: the grinding wheel is lowered until it contacts the surface of the aluminum-scandium alloy target blank, and the height of the contact point is recorded. The heights of contact points at multiple different positions are recorded in the same way and compared, and the maximum height is used as the initial thickness of the aluminum-scandium alloy target blank.

8. The method for processing an aluminum-scandium alloy target for casting according to claim 1, characterized in that: In the step 4, the side of the wire-cut target blank is polished with a polishing cloth.

Citation Information

Patent Citations

  • Manufacturing method of AlSc target material for improving chip manufacturing yield

    CN112951348A

  • Silicon carbide target material assembly and preparation method thereof

    CN113752403A

  • Preparation method of aluminum-scandium alloy target material

    CN112548069A

  • Preparation method of fine-grain low-hybrid-wave GH4720Li alloy small-specification bar

    CN116511841A

  • Production method of bathroom hardware shells

    US20190099846A1