Preparation method of novel environment-friendly organic silicon leather with three-layer structure
A three-layer silicone leather manufacturing process addresses environmental and labor issues by using chemically modified silicone rubber, achieving durable and eco-friendly leather with enhanced properties for diverse applications.
Patent Information
- Application Number
- CN202411129290.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-16
- Publication Date
- 2024-12-06
AI Technical Summary
Traditional leather manufacturing processes produce significant environmental pollution and have poor labor conditions, while silicone leather research faced stability and cost issues, limiting its widespread use.
A method for preparing a novel environmentally friendly silicone leather with a three-layer structure, involving specific compositions and processing steps to create a surface layer, intermediate layer, and adhesive layer using chemically modified liquid silicone rubber, which are then subjected to hot pressing and cooling to form a durable, wear-resistant leather.
The method results in a silicone leather with improved wear resistance, softness, and adhesion, using environmentally friendly materials that reduce pollution and health risks, suitable for various applications including aerospace and automobile manufacturing.
Abstract
Description
Technical Field
[0001] The invention relates to the field of leather, and in particular to a method for preparing a novel environmentally friendly organic silicon leather with a three-layer structure. Background Art
[0002] The origin of leather can be traced back to ancient times, when primitive people living in the wild used animal skins to make clothes, shoes and other items to protect themselves from the weather and wild beasts. Around the world, people from different cultures and regions have begun to use leather and developed different methods to process and dye leather.
[0003] In Europe, leather products became one of the important commodities in the Middle Ages. Cities in Germany and Italy became centers of leather processing, with many butchers and tanners engaged in leather manufacturing. In the 14th century, London, Paris and Amsterdam also became major leather production centers in Europe. In the 16th century, Spain and Portugal brought back fresh animal hides from the Americas, making the leather industry in Europe more prosperous.
[0004] Today, leather remains a popular material. Although some people dispute the practice of using animal leather, leather is still a durable, beautiful material that is widely used in clothing, shoes, handbags and other fields. In addition, leather is also used in industries such as furniture, automobile and aircraft manufacturing. In some developing countries, leather manufacturing is an important employment and economic pillar. For example, in India, leather manufacturing accounts for more than 2% of the country's entire manufacturing industry. However, in some developing countries, the production environment and labor conditions of leather manufacturing are often poor and need better management and supervision.
[0005] From the 1950s to the 1970s, the research on silicone leather was in its infancy. Scientists were mainly committed to exploring the synthesis methods of silicone and its potential application in the leather field. At this stage, the performance of silicone leather was not stable enough and the production cost was high, so it was not widely used. In the 1980s, with the advancement of science and technology, the research on silicone leather made a breakthrough. Scientists improved the performance of silicone leather and reduced the production cost by continuously improving the synthesis process, making it gradually ready for commercialization. By the 21st century, the research and application of silicone leather ushered in a period of rapid development, the production technology became increasingly mature, and the application field continued to expand.
[0006] The chemicals and processes used in traditional leather manufacturing produce large amounts of wastewater, waste gas and waste, causing serious pollution to the environment. Summary of the invention
[0007] The invention provides a method for preparing a novel environment-friendly organic silicon leather with a three-layer structure, which is beneficial to environmental protection.
[0008] The present invention provides a method for preparing a novel environmentally friendly silicone leather with a three-layer structure, comprising the following steps: coating a first liquid silicone rubber on a release paper to obtain a primary coating, and drying the primary coating to obtain a surface layer. Coating a second liquid silicone rubber on the surface layer to obtain a secondary coating, and drying the secondary coating to obtain an intermediate layer. Coating a third liquid silicone rubber on the intermediate layer and laminating a substrate fabric to obtain a tertiary coating, and drying the tertiary coating to obtain an adhesive layer. The surface layer, the intermediate layer, and the adhesive layer are subjected to a hot pressing roller pressure treatment, and after cooling, the release paper is peeled off to obtain a novel environmentally friendly silicone leather with a three-layer structure.
[0009] Further, the first liquid silicone rubber is composed of component A, component B and component C in a mass ratio of 100:3:1, component A of the first liquid silicone rubber includes silicone rubber, component B of the first liquid silicone rubber includes hydrogen-containing silicone oil with a hydrogen content of 0.36-0.50%, vinyl silicone oil, and filler, and the mass ratio of hydrogen-containing silicone oil, vinyl silicone oil, and filler is 6-30:80-100:25-30. Component C of the first liquid silicone rubber includes 3-glycidyloxypropyltrimethoxysilane and γ-aminopropyltriethoxysilane, and the mass ratio of 3-glycidyloxypropyltrimethoxysilane and γ-aminopropyltriethoxysilane is 5:5.
[0010] Furthermore, when preparing the first liquid silicone rubber, a mixture of component A, component B and component C of the first liquid silicone rubber is added to a three-necked flask, and an appropriate amount of acetic acid is added dropwise under stirring conditions. The mixture is reacted at 70° C. under stirring conditions for 30 minutes, and the first liquid silicone rubber can be obtained after standing.
[0011] Furthermore, the organic silicone rubber includes RTV-2 liquid organic silicone rubber. The filler includes color paste pigment.
[0012] Furthermore, when the first liquid silicone rubber is coated on the release paper, the coating thickness is 0.15-0.25 mm and the coating speed is 6 M / min.
[0013] Furthermore, when the coating is dried once, it is carried out in a hot air drying oven, the drying temperature is 115° C., the hot air speed is 0.5-1 m / s, and the drying time is 2-30 min.
[0014] Furthermore, the second liquid silicone rubber is composed of component A and component B in a mass ratio of 1:1, and component A of the second liquid silicone rubber includes special resin and k-carrageenan, and the mass ratio of special resin and k-carrageenan is 2:1. Component B of the second liquid silicone rubber includes a solution containing calcium ions, hydrogen-containing silicone oil with a hydrogen content of 0.2% to 0.6% and / or 0.9% to 1.6%, and a reinforcing filler, and the mass ratio of the solution containing calcium ions, hydrogen-containing silicone oil, and reinforcing filler is 5-10:80-100:25-30. When preparing the second liquid silicone rubber, the components A and B of the second liquid silicone rubber are mixed and stirred evenly to obtain the second liquid silicone rubber, wherein the rotation speed during stirring is 190r / min to 210r / min.
[0015] Furthermore, when the second liquid silicone rubber is coated on the surface layer, the coating thickness is 40 μm and the coating speed is 8 M / min.
[0016] Furthermore, when the secondary coating is dried, it is carried out in a hot air drying oven, the drying temperature is 120° C., the hot air speed is 0.5-1 m / s, and the drying time is 2.5 min.
[0017] Further, the third liquid silicone rubber is composed of component A and component B in a mass ratio of 1:1, component A of the third liquid silicone rubber includes special resin and modified gelatin, and the mass ratio of special resin and modified gelatin is 2:1. Component B of the third liquid silicone rubber includes vinyl silicone oil, silicone resin tackifier, and reinforcing filler, and the mass ratio of vinyl silicone oil, silicone resin tackifier, and reinforcing filler is 80-100:1-10:25-30.
[0018] Furthermore, the special resin includes LJ-12510 hyperbranched polyester acrylate special resin. The modified gelatin includes industrial gelatin and water-based polyurethane with a mass fraction of 15%-20%. The silicone resin tackifier includes one or more of γ-aminopropyl triethoxysilane, γ-aminopropyl trimethoxysilane, vinyl triethoxysilane, vinyl trimethoxysilane, and vinyl triisopropoxysilane. The reinforcing filler includes one or more of white carbon black, nano calcium carbonate, fatty acid calcium, and nano silicon dioxide.
[0019] Furthermore, when the third liquid silicone rubber is coated on the intermediate layer, the coating thickness is 0.35-0.45 mm and the coating speed is 6 M / min.
[0020] Furthermore, the coating is dried three times in a hot air drying oven, the drying temperature is 130° C., the hot air speed is 0.5-1 m / s, and the drying time is 3-20 min.
[0021] Furthermore, the surface layer, the middle layer and the bonding layer are subjected to a hot pressing roller pressing treatment, and then vulcanized and cooled. During the vulcanization, the vulcanization is performed at a temperature of 150° C. for 5-10 minutes.
[0022] Compared with the prior art, the present invention has the following effects:
[0023] In the three-layer structure of the novel environmentally friendly silicone leather of the present invention, the surface layer is formed by coating a chemically modified liquid silicone rubber. The chemical modification makes the surface of the coating have good wear resistance and provides good film-forming properties for the coating, so that it will not produce cracks during the curing process, and achieve the effect of dry and wear-resistant surface touch, while improving the surface density, achieving the characteristics of wear resistance, scratch resistance, and scratch resistance; the surface layer rubber feel, wear resistance, oil resistance and mechanical properties are comprehensively balanced. The bonding layer is formed by coating a chemically modified liquid silicone rubber, which is used to provide a reliable interlayer bonding effect for the silicone resin and the microfiber base cloth. By adding gelatin containing water-based polyurethane, the viscosity of the bonding glue can be further improved, and the curing speed of the bonding layer and the bonding strength control of the surface layer are comprehensively balanced.
[0024] The preparation method of the three-layer structure of the novel environmentally friendly organic silicon leather of the present invention has the effect of significantly improving the softness, stretchability, and wear resistance of the organic silicon leather, and improving the adhesion between the adhesive layers. In the present invention, the organic silicon used in the whole process itself is an environmentally friendly material, so the leather fabric prepared by the preparation method of the present invention meets the environmental protection requirements, and the solid content of the fabric reaches 100% of organic silicon molecules, which is more conducive to environmental protection requirements and protects the health of operators. DETAILED DESCRIPTION
[0025] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.
[0026] The embodiment of the present invention provides a method for preparing a novel environmentally friendly silicone leather with a three-layer structure, comprising the following steps:
[0027] (1) coating a first liquid silicone rubber on a release paper to obtain a primary coating, and then drying the primary coating in a heated hot air drying oven to obtain a surface layer.
[0028] In the above steps, the first liquid silicone rubber is composed of component A, component B and component C in a mass ratio of 100:3:1.
[0029] Component A includes organic silicone rubber, wherein the organic silicone rubber includes RTV-2 liquid organic silicone rubber.
[0030] Component B includes hydrogen-containing silicone oil with a hydrogen content of 0.36-0.50%, vinyl silicone oil, and filler, and the mass ratio of hydrogen-containing silicone oil, vinyl silicone oil, and filler is 6-30:80-100:25-30. Among them, the filler includes color paste pigment.
[0031] The operation time of components A and B of the first liquid silicone rubber is 4 to 8 hours, the curing time is 2 to 5 minutes, and the hardness is 45 to 65 Shore A. The viscosity of component A of the first liquid silicone rubber is 100,000 to 500,000 / mPa·S, and the viscosity of component B is 100,000 to 500,000 / mPa·S.
[0032] Component C includes 3-glycidyloxypropyltrimethoxysilane (KH-560) and γ-aminopropyltriethoxysilane (KH-550), and the mass ratio of 3-glycidyloxypropyltrimethoxysilane to γ-aminopropyltriethoxysilane is 5: 5. Component C may also include a small amount of ethanol.
[0033] The first liquid silicone rubber with multiple crosslinks of main chain and side chain was prepared by sol-gel method. When preparing the first liquid silicone rubber, a mixture of component A, component B and component C of the first liquid silicone rubber was added into a three-necked flask, and an appropriate amount of acetic acid was added dropwise under stirring conditions, and reacted at 70°C for 30 minutes under stirring conditions, and the first liquid silicone rubber was obtained after standing.
[0034] When the first liquid organic silicone rubber is coated on the release paper, the coating thickness of the first liquid organic silicone rubber is 0.15-0.25 mm, the coating speed is 6 M / min, and the coating temperature is room temperature.
[0035] When the primary coating is dried in a heated hot air drying oven, the drying temperature of the hot air drying oven is 115°C, the hot air speed is 0.5-1m / s, and the drying time is 2-30min. By using a hot air drying oven, the primary coating is first dried at a constant speed and then dried at a reduced speed. The specific description is as follows: Since the hot air directly acts on the surface of the coating layer, the solvent on the surface of the coating layer is completely vaporized, and the slurry solvent inside the coating layer migrates to the surface due to capillary action, continuously evaporates, and the coating layer gradually shrinks. When the moisture content reaches a critical state, discontinuous dry spots appear on the surface of the coating layer, and this stage is a constant speed drying stage. When the solvent content in the coating layer is low, the temperature of the coating layer rises as a whole and forms a temperature gradient, and heat is transferred from the surface of the coating layer to the inside of the coating layer, while the solvent continuously diffuses to the surface of the coating layer, which is a reduced speed drying stage. In addition, by setting the drying temperature to 115°C, the hot air speed to 0.5-1m / s, and the drying time to 2-30min, the performance uniformity and stability of the surface layer are effectively improved.
[0036] (2) coating the surface layer with a second liquid silicone rubber to obtain a secondary coating, and then drying the secondary coating in a heated hot air drying oven to obtain an intermediate layer.
[0037] In the above steps, the second liquid silicone rubber is composed of component A and component B in a mass ratio of 1:1.
[0038] Component A includes special resin and k-carrageenan, and the mass ratio of the special resin to the k-carrageenan is 2: 1. Among them, the special resin includes LJ-12510 hyperbranched polyester acrylate special resin.
[0039] Component B includes a solution containing calcium ions, hydrogen-containing silicone oil with a hydrogen content of 0.2% to 0.6% and / or 0.9% to 1.6%, and a reinforcing filler. The mass ratio of the solution containing calcium ions, the hydrogen-containing silicone oil, and the reinforcing filler is 5-10:80-100:25-30. Among them, the solution containing calcium ions includes a calcium chloride solution. The concentration of the calcium chloride solution can be 4-6%. The reinforcing filler includes one or more of white carbon black, nano calcium carbonate, fatty acid calcium, and nano silicon dioxide.
[0040] The operation time of components A and B of the second liquid silicone rubber is 4 to 8 hours, the curing time is 2 to 5 minutes, and the hardness is 45 to 65 Shore A.
[0041] When preparing the second liquid organic silicone rubber, the component A and the component B of the second liquid organic silicone rubber are mixed and stirred evenly to obtain the second liquid organic silicone rubber, wherein the rotation speed during stirring is 190 r / min to 210 r / min.
[0042] When the second liquid silicone rubber is coated on the surface layer, the coating thickness is 40 μm, the coating speed is 8 M / min, and the coating temperature is room temperature.
[0043] When the secondary coating is dried in a heated hot air drying oven, the drying temperature of the hot air drying oven is 120°C, the hot air speed is 0.5-1m / s, and the drying time is 2.5min. By using a hot air drying oven, the primary coating is first dried at a constant speed and then dried at a reduced speed. The specific description is as follows: Since the hot air directly acts on the surface of the coating layer, the solvent on the surface of the coating layer is completely vaporized, and the slurry solvent inside the coating layer migrates to the surface due to capillary action, continuously evaporates, and the coating layer gradually shrinks. When the moisture content reaches a critical state, discontinuous dry spots appear on the surface of the coating layer, and this stage is a constant speed drying stage. When the solvent content in the coating layer is low, the temperature of the coating layer rises as a whole and forms a temperature gradient, and heat is transferred from the surface of the coating layer to the inside of the coating layer, while the solvent continuously diffuses to the surface of the coating layer, which is a reduced speed drying stage. In addition, by setting the drying temperature to 120°C, the hot air speed to 0.5-1m / s, and the drying time to 2.5min, the performance uniformity and stability of the surface layer are effectively improved.
[0044] (3) coating the third liquid silicone rubber on the middle layer and laminating the base fabric to obtain a third coating layer, and then drying the third coating layer in a heated hot air drying oven to obtain a bonding layer.
[0045] In the above steps, the third liquid silicone rubber is composed of component A and component B in a mass ratio of 1:1.
[0046] The A component of the third liquid silicone rubber includes a special resin and modified gelatin, and the mass ratio of the special resin to the modified gelatin is 2:1. Among them, the special resin includes LJ-12510 hyperbranched polyester acrylate special resin. The modified gelatin includes industrial gelatin (INGE) and water-based polyurethane (MEKO-WPU) with a mass fraction of 15%-20%.
[0047] The B component of the third liquid silicone rubber includes vinyl silicone oil, silicone resin tackifier, and reinforcing filler, and the mass ratio of vinyl silicone oil, silicone resin tackifier, and reinforcing filler is 80-100: 1-10: 25-30. Among them, the silicone resin tackifier includes one or more of γ-aminopropyl triethoxysilane, γ-aminopropyl trimethoxysilane, vinyl triethoxysilane, vinyl trimethoxysilane, and vinyl triisopropoxysilane. The reinforcing filler includes one or more of white carbon black, nano calcium carbonate, fatty acid calcium, and nano silicon dioxide.
[0048] When the third liquid silicone rubber is coated on the middle layer, the coating thickness is 0.35-0.45 mm, the coating speed is 6 M / min, and the coating temperature is room temperature.
[0049] Base fabrics include polyester, spandex, pure cotton, and microfiber base fabrics.
[0050] When the three coatings are dried in a heated hot air drying oven, the drying temperature of the hot air drying oven is 130°C, the hot air speed is 0.5-1m / s, and the drying time is 3-20min. Similarly, by using a hot air drying oven, the three coatings are first dried at a constant speed and then dried at a reduced speed. The specific description is as follows: Since the hot air directly acts on the surface of the coating layer, the solvent on the surface of the coating layer is completely vaporized, and the slurry solvent inside the coating layer migrates to the surface due to capillary action, continuously evaporates, and the coating layer gradually shrinks. When the moisture content reaches a critical state, discontinuous dry spots appear on the surface of the coating layer, and this stage is a constant speed drying stage. When the solvent content in the coating layer is low, the temperature of the coating layer rises as a whole and forms a temperature gradient, and heat is transferred from the surface of the coating layer to the inside of the coating layer, while the solvent continuously diffuses to the surface of the coating layer, which is a reduced speed drying stage. In addition, by setting the drying temperature to 130°C, the hot air speed to 0.5-1m / s, and the drying time to 3-20min, the performance uniformity and stability of the bonding layer are effectively improved.
[0051] (4) The surface layer, the middle layer, and the adhesive layer are subjected to a hot pressing roller pressure treatment, and after cooling, the release paper is peeled off to obtain a new type of environmentally friendly silicone leather with a three-layer structure.
[0052] In the above steps, the surface layer, the middle layer and the middle layer are subjected to hot pressing roller pressure treatment, and then can be transferred to the tunnel furnace for vulcanization. After the vulcanization is completed, the surface layer, the middle layer and the middle layer are taken out of the tunnel furnace for drying, and then cooled. During vulcanization, the vulcanization is performed at a temperature of 150°C for 5-10 minutes.
[0053] The new environmentally friendly silicone leather with a three-layer structure includes a surface layer, a middle layer, and a bonding layer arranged from top to bottom.
[0054] In summary, the surface layer is a layer of silicone formed by coating, which achieves the effect of dry and wear-resistant surface touch, while improving the surface density to achieve the characteristics of wear resistance, scratch resistance, and scratch resistance; comprehensively balances the feel, wear resistance, oil resistance and mechanical properties of the surface layer. The bonding layer is a layer of silicone formed by coating, which is used to provide a strong interlayer bonding effect for the silicone resin and the microfiber base cloth, and comprehensively balances the curing speed of the bonding layer and the bonding strength control of the surface layer. The preparation method of the new environmentally friendly silicone leather with a three-layer structure of the present invention has the effect of significantly improving the softness, stretchability and wear resistance of the silicone leather. In the present invention, the silicone used in the whole process itself is an environmentally friendly material, so the leather fabric prepared by the preparation method of the present invention meets the environmental protection requirements, and the fabric solid content reaches 100% of silicone molecules, which is more conducive to environmental protection requirements and protects the health of operators.
[0055] In general, the three-layer structure of the present invention has good performance and sustainable development characteristics, and is a new synthetic material with environmental protection characteristics. The above-mentioned new environmentally friendly silicone leather abandons the non-wear-resistant materials such as PU or PVC on the surface of traditional leather, adopts environmentally friendly silicone resin as the surface material, increases silicon oxygen bonds, makes the leather more resilient, thinner and softer, and uses vinyl silicone oil and environmentally friendly thickener as the bonding materials of the high-viscosity bonding layer, and adopts low-energy consumption and low-pollution processes in the manufacturing process, which can well solve the problems of easy degumming, easy wear, production raw materials, processes and other environmentally unfriendly problems of traditional double-layer leather, reduce the impact on the environment, help protect the ecological environment, promote global fair trade, and increase the added value of leather. The above-mentioned new environmentally friendly silicone leather can replace traditional animal leather and reduce harm to animals. The three-layer structure of the present invention has good wear resistance, weather resistance, waterproofness and other characteristics, and can meet people's needs for leather products. At the same time, it has a long service life, and can be recycled after being abandoned to reduce the waste of resources, which is conducive to the implementation and development of the concept of green and sustainable development. The present invention can be applied in a wide range of fields, such as aerospace, automobile manufacturing, office furniture, 3C electronics, etc.
[0056] The following is a detailed description with reference to specific embodiments:
[0057] Example 1
[0058] (1) Coating the first liquid silicone rubber on the release paper to obtain a primary coating, and then drying the primary coating in a heated hot air drying oven to obtain a surface layer. The first liquid silicone rubber is composed of component A, component B and component C in a mass ratio of 100:3:1. Component A is RTV-2 liquid silicone rubber, and component B includes hydrogen-containing silicone oil with a hydrogen content range of 0.36-0.50%, vinyl silicone oil, and color paste pigment in a mass ratio of 6:80:25. Component C includes 3-glycidyloxypropyltrimethoxysilane (KH-560) and γ-aminopropyltriethoxysilane (KH-550) in a mass ratio of 5:5. The coating thickness of the first liquid silicone rubber is 0.15 mm, the coating speed is 6 M / min, and the coating temperature is room temperature. The drying temperature of the hot air drying oven is 115°C, the hot air speed is 0.5 m / s, and the drying time is 10 min.
[0059] (2) Apply a second liquid silicone rubber on the surface layer to obtain a secondary coating, and then dry the secondary coating in a heated hot air drying oven to obtain an intermediate layer. The second liquid silicone rubber is composed of component A and component B in a mass ratio of 1:1. Component A includes LJ-12510 hyperbranched polyester acrylate special resin and k-carrageenan in a mass ratio of 2:1. Component B includes 4% calcium chloride solution, hydrogen-containing silicone oil with a hydrogen content of 0.2% to 0.6%, and white carbon black in a mass ratio of 5:80:25. The coating thickness of the second liquid silicone rubber is 40μm, the coating speed is 8M / min, and the coating temperature is room temperature. The drying temperature of the hot air drying oven is 120°C, the hot air speed is 0.5m / s, and the drying time is 2.5min.
[0060] (3) Apply the third liquid silicone rubber on the middle layer and adhere it to the microfiber base cloth to obtain a three-layer coating, and then dry the three-layer coating in a heated hot air drying oven to obtain a bonding layer. The third liquid silicone rubber is composed of component A and component B in a mass ratio of 1:1. Component A includes LJ-12510 hyperbranched polyester acrylate special resin and modified gelatin in a mass ratio of 2:1, and the modified gelatin is gelatin modified by adding a water-based polyurethane (MEKO-WPU) with a mass fraction of 20%. Component B includes vinyl silicone oil, γ-aminopropyl triethoxysilane, and white carbon black in a mass ratio of 80:1:25. The coating thickness of the third liquid silicone rubber is 0.35 mm, the coating speed is 6 M / min, and the coating temperature is room temperature. The drying temperature of the hot air drying oven is 130°C, the hot air speed is 0.5 m / s, and the drying time is 5 min.
[0061] (4) The surface layer, the middle layer and the adhesive layer are subjected to a hot pressing roller pressure treatment, and then transferred to a tunnel furnace for vulcanization. After the vulcanization is completed, the surface layer, the middle layer and the adhesive layer are taken out of the tunnel furnace for drying, and after the temperature is lowered, the release paper is peeled off to obtain a new type of environmentally friendly silicone leather with a three-layer structure. The vulcanization is performed at a temperature of 150° C. for 5 minutes.
[0062] After testing, the new environmentally friendly silicone leather with a three-layer structure in this embodiment can reach more than 2,000 times under the ASTMD3884-09 (2017) (CS-10 grinding wheel / 1000G pressure) standard when performing leather wear resistance. It has reached more than 150,000 tests under the ASTM D4966 (load-bearing 12Kpa pressure) standard. There is no obvious change on the surface of the sample under the anti-fouling test AATCC 130 standard. After high and low temperature tests (maximum temperature 70C, duration: 4H, minimum temperature: -25℃, duration: 4H, 6 cycles, total test time: 48H) standards, the sample has no debonding, cracking, discoloration, shedding and other abnormalities, which is excellent.
[0063] Example 2
[0064] (1) Coating a first liquid silicone rubber on a release paper to obtain a primary coating, and then drying the primary coating in a heated hot air drying oven to obtain a surface layer. The first liquid silicone rubber is composed of component A, component B and component C in a mass ratio of 100:3:1. Component A is RTV-2 liquid silicone rubber. Component B includes hydrogen-containing silicone oil with a hydrogen content range of 0.36-0.50%, vinyl silicone oil, and color paste pigment in a mass ratio of 10:90:27. Component C includes 3-glycidyloxypropyltrimethoxysilane (KH-560) and γ-aminopropyltriethoxysilane (KH-550) in a mass ratio of 5:5. The coating thickness of the first liquid silicone rubber is 0.2 mm, the coating speed is 6 M / min, and the coating temperature is room temperature. The drying temperature of the hot air drying oven is 115°C, the hot air speed is 1 m / s, and the drying time is 10 min.
[0065] (2) Applying a second liquid silicone rubber on the surface layer to obtain a secondary coating, and then drying the secondary coating in a heated hot air drying oven to obtain an intermediate layer. The second liquid silicone rubber is composed of component A and component B in a mass ratio of 1:1. Component A includes LJ-12510 hyperbranched polyester acrylate special resin and k-carrageenan in a mass ratio of 2:1. Component B of the second liquid silicone rubber includes 6% calcium chloride solution, hydrogenated silicone oil with a hydrogen content of 0.9% to 1.6%, and nano calcium carbonate in a mass ratio of 10:100:30. The coating thickness of the second liquid silicone rubber is 40μm, the coating speed is 8M / min, and the coating temperature is room temperature. The drying temperature of the hot air drying oven is 120°C, the hot air speed is 1m / s, and the drying time is 2.5min.
[0066] (3) Apply the third liquid silicone rubber on the middle layer and adhere it to the microfiber base cloth to obtain a three-layer coating, and then dry the three-layer coating in a heated hot air drying oven to obtain a bonding layer. The third liquid silicone rubber is composed of component A and component B in a mass ratio of 1:1. Component A includes LJ-12510 hyperbranched polyester acrylate special resin and modified gelatin in a mass ratio of 2:1, and the modified gelatin is gelatin modified by adding a water-based polyurethane (MEKO-WPU) with a mass fraction of 20%. Component B includes vinyl silicone oil, γ-aminopropyl trimethoxysilane, and fatty acid calcium in a mass ratio of 90:5:27. The coating thickness of the third liquid silicone rubber is 0.4 mm, the coating speed is 6 M / min, and the coating temperature is room temperature. The drying temperature of the hot air drying oven is 130°C, the hot air speed is 1 m / s, and the drying time is 10 min.
[0067] (4) The surface layer, the middle layer and the adhesive layer are subjected to a hot pressing roller pressure treatment, and then transferred to a tunnel furnace for vulcanization. After the vulcanization is completed, the surface layer, the middle layer and the adhesive layer are taken out of the tunnel furnace for drying, and after the temperature is lowered, the release paper is peeled off to obtain a new type of environmentally friendly silicone leather with a three-layer structure. The vulcanization is performed at a temperature of 150° C. for 5 minutes.
[0068] After testing, the new environmentally friendly silicone leather with a three-layer structure in this embodiment has reached more than 2,000 times under the ASTMD3884-09 (2017) (CS-10 grinding wheel / 1000G pressure) standard when performing leather wear resistance. It has reached more than 150,000 tests under the ASTM D4966 (load-bearing 12Kpa pressure) standard. There is no obvious change on the surface of the sample under the anti-fouling test AATCC 130 standard. After high and low temperature tests (maximum temperature 70C, duration: 4H, minimum temperature: -25℃, duration: 4H, 6 cycles, total test time: 48H) standards, the sample has no debonding, cracking, discoloration, shedding and other abnormalities, which is excellent.
[0069] Example 3
[0070] (1) Coating a first liquid silicone rubber on a release paper to obtain a primary coating, and then drying the primary coating in a heated hot air drying oven to obtain a surface layer. The first liquid silicone rubber is composed of component A, component B and component C in a mass ratio of 100:3:1. Component A is RTV-2 liquid silicone rubber. Component B includes hydrogen-containing silicone oil with a hydrogen content of 0.36-0.50%, vinyl silicone oil, and color paste pigment in a mass ratio of 20:100:30. Component C includes 3-glycidyloxypropyltrimethoxysilane (KH-560) and γ-aminopropyltriethoxysilane (KH-550) in a mass ratio of 5:5. The coating thickness of the first liquid silicone rubber is 0.22 mm, the coating speed is 6 M / min, and the coating temperature is room temperature. The drying temperature of the hot air drying oven is 115°C, the hot air speed is 0.8 m / s, and the drying time is 10 min.
[0071] (2) Apply a second liquid silicone rubber on the surface layer to obtain a secondary coating, and then dry the secondary coating in a heated hot air drying oven to obtain an intermediate layer. The second liquid silicone rubber is composed of component A and component B in a mass ratio of 1:1. Component A includes LJ-12510 hyperbranched polyester acrylate special resin and k-carrageenan in a mass ratio of 2:1. Component B includes 5% calcium chloride solution, hydrogenated silicone oil with a hydrogen content of 0.2% to 0.6%, and fatty acid calcium in a mass ratio of 7:90:28. The coating thickness of the second liquid silicone rubber is 40μm, the coating speed is 8M / min, and the coating temperature is room temperature. The drying temperature of the hot air drying oven is 120℃, the hot air speed is 0.8m / s, and the drying time is 2.5min.
[0072] (3) Coating the third liquid silicone rubber on the middle layer and attaching the microfiber base cloth to obtain a three-layer coating, and then drying the three-layer coating in a heated hot air drying oven to obtain a bonding layer. The third liquid silicone rubber is composed of component A and component B in a mass ratio of 1:1. Component A includes LJ-12510 hyperbranched polyester acrylate special resin and modified gelatin in a mass ratio of 2:1, and the modified gelatin is gelatin modified by adding a water-based polyurethane (MEKO-WPU) with a mass fraction of 20%. Component B includes vinyl silicone oil, vinyl triethoxysilane, and nano calcium carbonate in a mass ratio of 100:10:30. The coating thickness of the third liquid silicone rubber is 0.42 mm, the coating speed is 6 M / min, and the coating temperature is room temperature. The drying temperature of the hot air drying oven is 130°C, the hot air speed is 0.8 m / s, and the drying time is 15 min.
[0073] (4) The surface layer, the middle layer and the adhesive layer are subjected to a hot pressing roller pressure treatment, and then transferred to a tunnel furnace for vulcanization. After the vulcanization is completed, the surface layer, the middle layer and the adhesive layer are taken out of the tunnel furnace for drying, and after the temperature is lowered, the release paper is peeled off to obtain a new type of environmentally friendly silicone leather with a three-layer structure. The vulcanization is performed at a temperature of 150° C. for 5 minutes.
[0074] After testing, the new environmentally friendly silicone leather with a three-layer structure in this embodiment can reach more than 2,000 times under the ASTMD3884-09 (2017) (CS-10 grinding wheel / 1000G pressure) standard when performing leather wear resistance. It has reached more than 150,000 tests under the ASTM D4966 (load-bearing 12Kpa pressure) standard. There is no obvious change on the surface of the sample under the anti-fouling test AATCC 130 standard. After high and low temperature tests (maximum temperature 70C, duration: 4H, minimum temperature: -25℃, duration: 4H, 6 cycles, total test time: 48H) standards, the sample has no debonding, cracking, discoloration, shedding and other abnormalities, which is excellent.
[0075] Example 4
[0076] (1) Coating a first liquid silicone rubber on a release paper to obtain a primary coating, and then drying the primary coating in a heated hot air drying oven to obtain a surface layer. The first liquid silicone rubber is composed of component A, component B and component C in a mass ratio of 100:3:1. Component A is RTV-2 liquid silicone rubber. Component B includes hydrogen-containing silicone oil with a hydrogen content of 0.36-0.50%, vinyl silicone oil, and color paste pigment in a mass ratio of 30:80:25. Component C includes 3-glycidyloxypropyltrimethoxysilane (KH-560) and γ-aminopropyltriethoxysilane (KH-550) in a mass ratio of 5:5. The coating thickness of the first liquid silicone rubber is 0.25 mm, the coating speed is 6 M / min, and the coating temperature is room temperature. The drying temperature of the hot air drying oven is 115°C, the hot air speed is 1 m / s, and the drying time is 2 min.
[0077] (2) Apply a second liquid silicone rubber on the surface layer to obtain a secondary coating, and then dry the secondary coating in a heated hot air drying oven to obtain an intermediate layer. The second liquid silicone rubber is composed of component A and component B in a mass ratio of 1:1. Component A includes LJ-12510 hyperbranched polyester acrylate special resin and k-carrageenan in a mass ratio of 2:1. Component B includes 4% calcium chloride solution, hydrogenated silicone oil with a hydrogen content of 0.9% to 1.6%, and nano-silicon dioxide in a mass ratio of 10:80:30. The coating thickness of the second liquid silicone rubber is 40μm, the coating speed is 8M / min, and the coating temperature is room temperature. The drying temperature of the hot air drying oven is 120℃, the hot air speed is 1m / s, and the drying time is 2.5min.
[0078] (3) The third liquid organic silicone rubber is coated on the middle layer and attached to the microfiber base cloth to obtain a three-layer coating, and then the three-layer coating is dried in a heated hot air drying oven to obtain a bonding layer. The third liquid organic silicone rubber is composed of component A and component B in a mass ratio of 1:1. Component A includes LJ-12510 hyperbranched polyester acrylate special resin and modified gelatin in a mass ratio of 2:1, and the modified gelatin is gelatin modified by adding a water-based polyurethane (MEKO-WPU) with a mass fraction of 15%. Component B includes vinyl silicone oil, vinyl triisopropoxy silane, and nano-silicon dioxide in a mass ratio of 80:10:30. The coating thickness of the third liquid organic silicone rubber is 0.45 mm, the coating speed is 6 M / min, and the coating temperature is room temperature. The drying temperature of the hot air drying oven is 130°C, the hot air speed is 1 m / s, and the drying time is 3 min.
[0079] (4) The surface layer, the middle layer and the adhesive layer are subjected to a hot pressing roller pressure treatment, and then transferred to a tunnel furnace for vulcanization. After the vulcanization is completed, the surface layer, the middle layer and the adhesive layer are taken out of the tunnel furnace for drying, and after the temperature is lowered, the release paper is peeled off to obtain a new type of environmentally friendly silicone leather with a three-layer structure. The vulcanization is performed at a temperature of 150° C. for 5 minutes.
[0080] After testing, the new environmentally friendly silicone leather with a three-layer structure in this embodiment can reach more than 2,000 times under the ASTMD3884-09 (2017) (CS-10 grinding wheel / 1000G pressure) standard when performing leather wear resistance. It has reached more than 150,000 tests under the ASTM D4966 (load-bearing 12Kpa pressure) standard. There is no obvious change on the surface of the sample under the anti-fouling test AATCC 130 standard. After high and low temperature tests (maximum temperature 70C, duration: 4H, minimum temperature: -25℃, duration: 4H, 6 cycles, total test time: 48H) standards, the sample has no debonding, cracking, discoloration, shedding and other abnormalities, which is excellent.
[0081] Example 5
[0082] (1) Coating a first liquid silicone rubber on a release paper to obtain a primary coating, and then drying the primary coating in a heated hot air drying oven to obtain a surface layer. The first liquid silicone rubber is composed of component A, component B and component C in a mass ratio of 100:3:1. Component A is RTV-2 liquid silicone rubber. Component B includes hydrogen-containing silicone oil with a hydrogen content of 0.36-0.50%, vinyl silicone oil, and color paste pigment in a mass ratio of 20:100:30. Component C includes 3-glycidyloxypropyltrimethoxysilane (KH-560) and γ-aminopropyltriethoxysilane (KH-550) in a mass ratio of 5:5. The coating thickness of the first liquid silicone rubber is 0.2 mm, the coating speed is 6 M / min, and the coating temperature is room temperature. The drying temperature of the hot air drying oven is 115°C, the hot air speed is 0.8 m / s, and the drying time is 30 min.
[0083] (2) Apply a second liquid silicone rubber on the surface layer to obtain a secondary coating, and then dry the secondary coating in a heated hot air drying oven to obtain an intermediate layer. The second liquid silicone rubber is composed of component A and component B in a mass ratio of 1:1. Component A includes LJ-12510 hyperbranched polyester acrylate special resin and k-carrageenan in a mass ratio of 2:1. Component B includes 6% calcium chloride solution, hydrogenated silicone oil with a hydrogen content of 0.2% to 0.6%, and nano calcium carbonate in a mass ratio of 5:100:25. The coating thickness of the second liquid silicone rubber is 40μm, the coating speed is 8M / min, and the coating temperature is room temperature. The drying temperature of the hot air drying oven is 120℃, the hot air speed is 0.7m / s, and the drying time is 2.5min.
[0084] (3) The third liquid silicone rubber is coated on the middle layer and attached to the microfiber base cloth to obtain a three-layer coating, and then the three-layer coating is dried in a heated hot air drying oven to obtain a bonding layer. The third liquid silicone rubber is composed of component A and component B in a mass ratio of 1:1. Component A includes LJ-12510 hyperbranched polyester acrylate special resin and modified gelatin in a mass ratio of 2:1, and the modified gelatin is gelatin modified by adding a water-based polyurethane (MEKO-WPU) with a mass fraction of 15%. Component B includes vinyl silicone oil, vinyl trimethoxysilane, and nano calcium carbonate in a mass ratio of 100:1:25. The coating thickness of the third liquid silicone rubber is 0.4 mm, the coating speed is 6 M / min, and the coating temperature is room temperature. The drying temperature of the hot air drying oven is 130°C, the hot air speed is 0.5 m / s, and the drying time is 20 min.
[0085] (4) The surface layer, the middle layer, and the adhesive layer are subjected to a hot pressing roller pressure treatment, and after cooling, the release paper is peeled off to obtain a new type of environmentally friendly silicone leather with a three-layer structure.
[0086] After testing, the new environmentally friendly silicone leather with a three-layer structure in this embodiment can reach more than 2,000 times under the ASTMD3884-09 (2017) (CS-10 grinding wheel / 1000G pressure) standard when performing leather wear resistance. It has reached more than 150,000 tests under the ASTM D4966 (load-bearing 12Kpa pressure) standard. There is no obvious change on the surface of the sample under the anti-fouling test AATCC 130 standard. After high and low temperature tests (maximum temperature 70C, duration: 4H, minimum temperature: -25℃, duration: 4H, 6 cycles, total test time: 48H) standards, the sample has no debonding, cracking, discoloration, shedding and other abnormalities, which is excellent.
[0087] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A method for preparing a novel environmentally friendly silicone leather with a three-layer structure, characterized in that: The following steps are involved: Applying a first liquid silicone rubber on the release paper to obtain a primary coating, and drying the primary coating to obtain a surface layer; Applying a second liquid silicone rubber on the surface layer to obtain a secondary coating, and then drying the secondary coating to obtain an intermediate layer; Applying a third liquid silicone rubber on the middle layer and attaching the substrate fabric to obtain three coatings, and then drying the three coatings to obtain a bonding layer; The surface layer, the middle layer and the adhesive layer are subjected to a hot pressing roller pressure treatment, and after cooling, the release paper is peeled off to obtain a new type of environmentally friendly silicone leather with a three-layer structure.
2. The preparation method according to claim 1, characterized in that The first liquid silicone rubber is composed of component A, component B and component C in a mass ratio of 100:3:1, component A of the first liquid silicone rubber includes silicone rubber, component B of the first liquid silicone rubber includes hydrogen-containing silicone oil with a hydrogen content range of 0.36-0.50%, vinyl silicone oil, and filler, and the mass ratio of the hydrogen-containing silicone oil, the vinyl silicone oil, and the filler is 6-30:80-100:25-30; component C of the first liquid silicone rubber includes 3-glycidyloxypropyltrimethoxysilane and γ-aminopropyltriethoxysilane, and the mass ratio of the 3-glycidyloxypropyltrimethoxysilane to the γ-aminopropyltriethoxysilane is 5:
5.
3. The preparation method according to claim 2, characterized in that: When preparing the first liquid silicone rubber, a mixture of component A, component B and component C of the first liquid silicone rubber is added into a three-necked flask, and an appropriate amount of acetic acid is added dropwise under stirring. The mixture is reacted at 70° C. under stirring for 30 minutes, and the first liquid silicone rubber can be obtained after standing.
4. The preparation method according to claim 2, characterized in that: The organic silicone rubber includes RTV-2 liquid organic silicone rubber; The filler includes color paste pigment.
5. The preparation method according to claim 1, characterized in that: When the first liquid silicone rubber is coated on the release paper, the coating thickness is 0.15-0.25 mm and the coating speed is 6 M / min.
6. The preparation method according to claim 1, characterized in that: The primary coating is dried in a hot air drying oven at a drying temperature of 115° C., a hot air velocity of 0.5 to 1 m / s, and a drying time of 2 to 30 min.
7. The preparation method according to claim 1, characterized in that: The second liquid silicone rubber is composed of component A and component B in a mass ratio of 1:1, wherein component A of the second liquid silicone rubber includes special resin and k-carrageenan, and the mass ratio of the special resin to the k-carrageenan is 2:1; component B of the second liquid silicone rubber includes a solution containing calcium ions, hydrogen-containing silicone oil with a hydrogen content of 0.2% to 0.6% and / or 0.9% to 1.6%, and a reinforcing filler, and the mass ratio of the solution containing calcium ions, the hydrogen-containing silicone oil, and the reinforcing filler is 5-10:80-100:25-30; when preparing the second liquid silicone rubber, the component A and the component B of the second liquid silicone rubber are mixed and stirred uniformly to obtain the second liquid silicone rubber, wherein, The rotation speed during stirring is 190r / min~210r / min.
8. The preparation method according to claim 1, characterized in that: When the second liquid silicone rubber is coated on the surface layer, the coating thickness is 40 μm and the coating speed is 8 M / min.
9. The preparation method according to claim 1, characterized in that: The secondary coating is dried in a hot air drying oven at a drying temperature of 120° C., a hot air velocity of 0.5 to 1 m / s, and a drying time of 2.5 min.
10. The preparation method according to claim 1, characterized in that: The third liquid silicone rubber is composed of component A and component B in a mass ratio of 1:1, component A of the third liquid silicone rubber includes special resin and modified gelatin, and the mass ratio of special resin and modified gelatin is 2:1; component B of the third liquid silicone rubber includes vinyl silicone oil, silicone resin tackifier, and reinforcing filler, and the mass ratio of the vinyl silicone oil, the silicone resin tackifier, and the reinforcing filler is 80-100:1-10:25-30.
11. The preparation method according to claim 1, characterized in that: The special resin includes LJ-12510 hyperbranched polyester acrylate special resin; The modified gelatin comprises industrial gelatin and 15%-20% by mass of waterborne polyurethane; The silicone resin tackifier includes one or more of γ-aminopropyltriethoxysilane, γ-aminopropyltrimethoxysilane, vinyltriethoxysilane, vinyltrimethoxysilane, and vinyltriisopropoxysilane; The reinforcing filler includes one or more of white carbon black, nano calcium carbonate, fatty acid calcium, and nano silicon dioxide.
12. The preparation method according to claim 1, characterized in that: When the third liquid silicone rubber is coated on the intermediate layer, the coating thickness is 0.35-0.45 mm and the coating speed is 6 M / min.
13. The preparation method according to claim 1, characterized in that: The three coatings are dried in a hot air drying oven at a drying temperature of 130° C., a hot air velocity of 0.5 to 1 m / s, and a drying time of 3 to 20 min.
14. The preparation method according to claim 1, characterized in that: The surface layer, the middle layer and the bonding layer are subjected to a hot pressing roller pressure treatment, vulcanized, and then cooled; During vulcanization, vulcanize at 150°C for 5-10 minutes.