Preparation method of monodisperse nano metal oxide

By mixing the polymer precursor with the metal salt at high temperature and performing secondary calcination, the problems of long preparation period and agglomeration of nanometal oxide particles in the prior art are solved, and nanometal oxidation with high dispersion and uniform particle size are achieved Preparation of particles has good industrial application prospects.

CN119079933APending Publication Date: 2024-12-06CHINA PETROLEUM & CHEMICAL CORP +1
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202310653866.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-06-05
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

The prior art is difficult to produce monodispersed nanometal oxide particles on a large scale in the industry, and common methods have problems such as long preparation period, product agglomeration, uneven particle size distribution, and high cost. It is difficult to control the particle size, morphology and structure of the particles. .

Method used

By mixing the polymer precursor and metal salt in a certain proportion, performing high-temperature polymerization and secondary calcining, the coordinated ability of the polymer precursor disperses metal species at high temperature, and then removing organic matter to prepare highly dispersed nanometers Metal oxide particles.

Benefits of technology

The high dispersion, uniform particle size and regular appearance of nanometal oxide particles are achieved, which reduces the preparation cost and process complexity, and has good industrial application prospects.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119079933A_ABST
    Figure CN119079933A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of a monodisperse nano metal oxide, which comprises the following steps: (1) uniformly mixing a polymer precursor and a metal salt according to a certain proportion, and then carrying out high-temperature polymerization reaction; and (2) roasting the reactant obtained in the step (1) to obtain the monodisperse nano metal oxide. The particle size of the nano metal oxide particles is 1 to 600 nm, preferably 20 to 100 nm. The method can be used for preparing various nano metal oxide particles, the prepared nano particle material is good in dispersion and regular in morphology, and the preparation method is simple, low in raw material cost and good in industrial application prospect.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of nano materials, and specifically relates to a method for preparing monodisperse nano metal oxide particles. Background Art

[0002] In recent years, with the rapid development of modern industry and science and technology, the development and application of nanomaterials have attracted the continuous attention of scientists. Nanomaterials have basic characteristics such as quantum size effect, surface effect and macroscopic quantum tunneling effect, which make them show different properties from bulk materials in optics, electricity and chemistry. Nanometal oxide materials are an important part of nanomaterials science, and their application prospects are very broad. They have shown very unique properties in electricity, magnetism, optics, environment, metal corrosion protection and catalysis, and have become the research focus in the field of nanomaterials in recent years. Especially in the field of catalysis, they have good application prospects and can be used for hydrogenation, oxidation, photocatalysis, synthetic ammonia catalytic reactions, etc. Their catalytic activity and stability are not only related to the size and dispersibility of nanometal oxide particles, but also affected by shape and composition. However, due to their high surface energy, nanoparticles are very easy to spontaneously agglomerate, resulting in a decrease in the specific surface area of ​​nanoparticles, a weakening of the nano effect, and thus a decrease in their performance. Therefore, the research and preparation technology of monodisperse nanometal oxide particles is of great significance.

[0003] Common methods for preparing nano-metal oxide particles include solid phase method, sol-gel method, precipitation method, etc. However, these methods are either only suitable for preparing single metal oxides, or are costly and complex, making it difficult to mass-produce in industry, or have disadvantages such as long preparation cycle, product agglomeration, difficulty in simultaneously controlling product composition and particle size, and environmental pollution. Solid phase method is a traditional pulverization process. Li et al. (Solid State Sciences, 200, 2(8), 767-772) used solid phase method to synthesize SiO 2 、CeO 2 SnO 2 However, this method has the disadvantages of high energy consumption, easy mixing of impurities, uneven particle size distribution and irregular appearance of nanoparticles. Homogeneous precipitation method is also a general technology for preparing monodisperse nanometal oxide particles. CN 102757053A adopts chemical precipitation method and adds surfactant to stabilize the dispersion to prepare monodisperse SiO 2 Nanospheres. However, this method has the disadvantages of long reaction cycle, long post-processing time, and difficulty in controlling the particle size, morphology and structure. Summary of the invention

[0004] In view of the shortcomings of the prior art, the present invention provides a method for preparing monodisperse nano-metal oxides, which can prepare a variety of nano-metal oxide particles. The prepared nano-particle materials are well dispersed and have regular morphology. The preparation method is simple and the raw material cost is low, and it has good industrial application prospects.

[0005] The method for preparing monodisperse nano-metal oxides of the present invention comprises the following contents: (1) Mixing a polymer precursor and a metal salt in a certain proportion, and then performing a high-temperature polymerization reaction; (2) calcining the reactant obtained in step (1) to obtain a monodisperse nano-metal oxide. The nano-metal oxide particles have a particle size of 1 to 600 nm, preferably 20 to 100 nm.

[0006] In the method of the present invention, the polymer precursor in step (1) is selected from one or more of melamine, dicyandiamide, cyanamide, urea, thiourea, imidazole, dimethylimidazole, methylimidazole and citric acid.

[0007] In the method of the present invention, the metal salt described in step (1) is a precursor of nano metal oxide particles; the metal salt is selected from one or more salts of different metal elements selected from nitrates, sulfates, oxalates, acetates, phosphates, hypochlorites or halides of the corresponding metal; the metal in the metal salt can be one or more of Fe, Co, Ni, Cu, Ce, La, Ta, Mn, Mg, W, Mo, Al, Ti, Zr, Zn, Ga, Cr, V, In, Sn, Ag, Pt, Pd, Ir, Rh, Ru, Y or Sr.

[0008] In the method of the present invention, the mass ratio of the polymer precursor to the metal salt in step (1) can be 1 to 30:1.

[0009] In the method of the present invention, the mixing method in step (1) can be manual grinding or mechanical ball milling, and the mixing time can be 0.5 to 3 hours.

[0010] In the method of the present invention, the high temperature polymerization reaction temperature of step (1) is 300-650°C, the heating rate can be 1-15°C / min, the reaction time is 1-5 hours, and the reaction atmosphere can be air or an inert atmosphere, and the inert atmosphere can be selected from Ar, N 2 ; The reaction is generally carried out in a muffle furnace or a tubular furnace.

[0011] In the method of the present invention, the calcination temperature in step (2) is 400-700°C, the heating rate can be 1-15°C / min, the calcination time is 0.5-6 hours, the calcination atmosphere is generally carried out in an oxygen-containing atmosphere, preferably air, and the calcination process is generally carried out in a muffle furnace or a tubular furnace.

[0012] The present invention mixes the polymer precursor and the metal salt uniformly in advance, and then places the mixture in a muffle furnace or a tube furnace for baking, so that the polymer precursor is polymerized and the metal species are dispersed to obtain a solid powder. Subsequently, the solid powder obtained by the polymerization is subjected to a second high-temperature baking to remove organic matter, thereby obtaining highly dispersed nano-metal oxide particles.

[0013] Compared with the prior art, the beneficial effects of the present invention are as follows: the polymer precursor has a certain coordination ability, and can coordinate with metal ions to make them uniformly dispersed in the precursor mixture, and the metal species can still be highly dispersed due to the protection of the coordination effect during the calcination polymerization process; after secondary calcination, the organic matter that stabilizes the metal species is gradually removed, and highly dispersed nano metal oxide particles can be prepared. The particle size of the nano metal oxide particles is 1~600nm, the particle size is uniform, the appearance is regular and highly dispersed, and it has great application prospects in new energy materials, ecological environment materials, functional coating materials and catalytic materials. And the nano metal oxide particle preparation technology of the present invention is simple, the raw material cost is low, and it has good industrial application prospects. BRIEF DESCRIPTION OF THE DRAWINGS

[0014] Figure 1 This is a TEM electron microscope image of the nano-cerium oxide particles prepared in Example 1 of the present invention.

[0015] Figure 2 This is a TEM electron microscope image of the nano zirconium oxide particles prepared in Example 2 of the present invention.

[0016] Figure 3 This is a TEM electron microscope image of the cerium oxide particles prepared in Comparative Example 2 of the present invention. DETAILED DESCRIPTION

[0017] The technical solution of the present invention is described in more detail below through specific embodiments, but the present invention is not limited to these embodiments.

[0018] Nanoparticle characterization experiments: 1) Transmission Electron Microscopy (TEM) TEM was used to determine the dispersion form and size of the nano-metal oxide particles. The TEM images were obtained using a FEI Tecnai G2 20 S-twin transmission electron microscope with an accelerating voltage of 200 KV. The sample preparation method was as follows: the sample powder was dispersed in ethanol, and then a proper amount of the suspension was drawn with a capillary and dropped onto a carbon-based copper mesh to completely evaporate the ethanol for later use. Example 1

[0019] A method for preparing monodisperse nano-cerium oxide particles, comprising the following steps: taking 12 g of dicyandiamide and 1 g of Ce(NO 3 ) 3 6H 2 O was fully mixed in an agate mortar, and then polymerized at 550°C for 3 h in a tubular furnace under nitrogen atmosphere. Solid powder was obtained after natural cooling. 2 g of solid powder was weighed and calcined at 600°C for 4 h in a muffle furnace (heating rate of 3°C / min), and naturally cooled to obtain highly dispersed nano-cerium oxide particles. Example 2

[0020] A method for preparing monodisperse nano zinc oxide particles, comprising the following steps: taking 6 g melamine, 4 g cyanamide, 4 g imidazole and 2.0 g Zn(NO 3 ) 3 6H 2 O was ball-milled in a mechanical ball mill for 1 h to fully mix the mixture, and then polymerized at 550°C for 2 h in a tubular furnace under nitrogen atmosphere. Solid powder was obtained after natural cooling. 1 g of the solid powder was weighed and calcined at 600°C for 2 h in a muffle furnace (heating rate of 5°C / min), and naturally cooled to obtain highly dispersed nano zinc oxide particles. Example 3

[0021] A method for preparing monodisperse nano zirconium oxide particles, comprising the following steps: taking 10 g melamine, 2 g dimethylimidazole and 2 g Zr(NO 3 ) 4 ·3H 2 O was ball-milled in a mechanical ball mill for 2 h to fully mix the mixture, and then polymerized in a muffle furnace at 520 ° C for 3 h. After natural cooling, solid powder was obtained. 1 g of the solid powder was weighed and calcined in a muffle furnace at 580 ° C for 4 h (heating rate 5 ° C / min), and naturally cooled to obtain highly dispersed nano zirconium dioxide particles. Example 4

[0022] A method for preparing monodisperse nano iron oxide particles, comprising the following steps: taking 6 g melamine, 4 g thiourea, 4 g urea and 2.0 g FeSO 4 7H 2 O was ball-milled in a mechanical ball mill for 1 h to mix the mixture thoroughly, and then polymerized at 550 °C for 3 h in a tube furnace under nitrogen atmosphere. After natural cooling, solid powder was obtained. 1 g of solid powder was weighed and calcined at 620 °C for 3 h in a tube furnace (heating rate 5 °C / min) in an atmosphere of O 2 / N 2 Mixed gas (O 2 The volume concentration is 5 vol%) and the temperature is naturally lowered to obtain highly dispersed nano iron oxide particles. Comparative Example 1

[0023] Same as Example 1, except that the amount of dicyandiamide added is 8 g. Comparative Example 2

[0024] Same as Example 1, except that 12 g of dicyandiamide was replaced by 8 g of glucose.

[0025] Table 1 Average particle size of nano metal oxide particles Metal oxide particles Average particle size range (nm) Metal oxide particles Average particle size range (nm) Nano-cerium oxide particles prepared in Example 1 25-45 Nano-iron oxide particles prepared in Example 4 50-70 Nano zinc oxide particles prepared in Example 2 20-35 Nano cerium oxide particles prepared in Comparative Example 1 70-100 Nano-zirconia particles prepared in Example 3 35-50 Nano cerium oxide particles prepared in Comparative Example 2 Irregular block shape As attached Figure 1 As shown in the figure, the average particle size of the cerium oxide particles prepared in Example 1 is in the range of 25 to 45 nm, and the nanoparticles are highly dispersed and have uniform particle size. Figure 2 As shown, the zirconium oxide particles prepared in Example 3 are highly dispersed, with an average particle size of about 35 to 50 nm, and the particle size of the nanoparticles is uniform. This shows that the preparation method of the present invention can successfully prepare a variety of highly dispersed nano metal oxide particles. However, the cerium oxide particles synthesized in Comparative Example 2 using a preparation method other than the present invention show irregular block distribution and are in the micron level.

Claims

1. A method for preparing monodisperse nano-metal oxides, comprising the following steps: (1) uniformly mixing a polymer precursor and a metal salt in a certain proportion, and then subjecting the mixture to a high-temperature polymerization reaction; (2) calcining the reactant obtained in step (1) to obtain monodisperse nano-metal oxides.

2. The method according to claim 1, Features: The particle size of the nano metal oxide particles is 1-600 nm, preferably 20-100 nm.

3. The method according to claim 1, Features: The polymer precursor in step (1) is selected from one or more of melamine, dicyandiamide, cyanamide, urea, thiourea, imidazole, dimethylimidazole, methylimidazole and citric acid.

4. The method according to claim 1, Features: The metal in the metal salt of step (1) is one or more of Fe, Co, Ni, Cu, Ce, La, Ta, Mn, Mg, W, Mo, Al, Ti, Zr, Zn, Ga, Cr, V, In, Sn, Ag, Pt, Pd, Ir, Rh, Ru, Y or Sr.

5. The method according to claim 1, Features: The metal salt in step (1) is selected from one or more metal salts of the corresponding metal nitrates, sulfates, oxalates, acetates, phosphates, hypochlorites or halides.

6. The method according to claim 1, Features: The mass ratio of the polymer precursor to the metal salt in step (1) is 1-30:

1.

7. The method according to claim 1, Features: The mixing method in step (1) is manual grinding or mechanical ball milling, and the mixing time is 0.5 to 3 hours.

8. The method according to claim 1, Features: The high temperature polymerization reaction temperature of step (1) is 300-650°C, the heating rate can be 1-15°C / min, the reaction time is 1-5 hours, and the reaction atmosphere can be air or an inert atmosphere.

9. The method according to claim 1, Features: The calcination temperature in step (2) is 400-700°C, the heating rate can be 1-15°C / min, the calcination time is 0.5-6 hours, and the calcination atmosphere is an oxygen-containing atmosphere.

10. Use of the monodisperse nano metal oxide prepared according to any one of claims 1 to 9 in energy materials, ecological environment materials, functional coating materials and catalytic materials.

Citation Information

Patent Citations

  • Monodisperse nano-silica production process by chemical precipitation method

    CN102757053A