Hexagonal boron nitride sheet derived with boron nitride nanotube structure as well as preparation method and application of hexagonal boron nitride sheet

Through the reaction of the precursor of the hexagonal boron nitride flakes modified by ZIF-67 and MgCo-ZIF with boric acid aqueous solution and ammonia ammonization treatment, hexagonal boron nitride flakes with high thermal conductivity were prepared. The problems of limited thermal conductivity and complex process in traditional methods are solved, and efficient thermal conductivity improvement and industrial production are achieved.

CN119079939AActive Publication Date: 2024-12-06LANZHOU INSTITUTE OF CHEMICAL PHYSICS CHINESE ACADEMY OF SCIENCES +2
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202411180674.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-27
Publication Date
2024-12-06
Estimated Expiration
2044-08-27

AI Technical Summary

Technical Problem

In the prior art, the thermal conductivity enhancement of the hexagonal boron nitride sheet is limited. The traditional chemical vapor deposition method requires external addition of catalysts and boron sources, which is difficult to grow and product uniformity is difficult to control.

Method used

Hexagonal boron nitride sheet precursor modified by ZIF-67 and MgCo-ZIF were prepared by heating with boric acid aqueous solution and ammonia ammonization treatment to produce hexagonal boron nitride sheets derived from boron nitride nanotube structures, avoiding the External addition of catalysts simplifies the process and reduces equipment costs.

Benefits of technology

The thermal conductivity is significantly improved, and by enhancing the contact area between the nanofiller and the matrix, a complete thermal conductivity network is built, the interface thermal resistance is reduced, and large-scale preparation of high-quality, high-purity boron nitride nanotubes is achieved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119079939A_ABST
    Figure CN119079939A_ABST
Patent Text Reader

Abstract

The invention discloses a hexagonal boron nitride sheet derived with a boron nitride nanotube structure as well as a preparation method and application of the hexagonal boron nitride sheet. The method comprises the following steps: (1) preparing a ZIF-67 modified hexagonal boron nitride sheet; (2) preparing an MgCo-ZIF modified hexagonal boron nitride sheet; (3) preparing a hexagonal boron nitride sheet-boron nitride nanotube precursor; and (4) ammoniation of the hexagonal boron nitride sheet-boron nitride nanotube precursor: heating the hexagonal boron nitride sheet-boron nitride nanotube precursor in an inert atmosphere to 1100-1600 DEG C, then introducing ammonia gas for ammoniation treatment, carrying out a reaction, and then naturally cooling to room temperature to obtain the hexagonal boron nitride sheet derived with the boron nitride nanotube structure. According to the method, an external boron source does not need to be additionally added as a catalyst, the preparation process is simple, the requirement on equipment is low, industrialization is easy to realize, and the equipment cost is greatly saved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a hexagonal boron nitride thin sheet, in particular to a hexagonal boron nitride thin sheet with a boron nitride nanotube structure derived therefrom and a preparation method and application thereof. Background Art

[0002] With the rapid development of electronic devices, nanomaterials are increasingly used in smartphones, wearable devices, tablets, and battery packaging. Boron nitride nanomaterials exhibit unique physical and chemical properties, such as electrical insulation, high specific surface area, low dielectric constant, good thermal and chemical stability, and excellent thermal conductivity. Boron nitride nanomaterials not only give polymers high thermal conductivity, but also enable the filled composite materials to remain electrically insulating. They have been widely used in electronics / optoelectronics, catalysis, energy storage and conversion, sensor and electronic product development, nanocomposites, and other fields.

[0003] Like carbon nanomaterials including graphene and carbon nanotubes, boron nitride also has structures of different dimensions. A series of boron nitride nanostructures have been synthesized, including: zero-dimensional boron nitride nanospheres; one-dimensional boron nitride nanostructures, mainly including boron nitride nanowires, boron nitride nanorods, and boron nitride nanofibers; two-dimensional boron nitride nanostructures, mainly including boron nitride nanosheets (BNNSs), boron nitride nanobelts (BNNRs), boron nitride nanotubes (BNNTs) and three-dimensional nanostructured porous boron nitride fullerenes. Boron nitride structures of different dimensions have different properties. Since single-dimensional fillers have similar sizes and morphologies, there are a large number of gaps between fillers, resulting in severe interface phonon scattering. The synergistic effect between multi-dimensional fillers can increase the overall filling density of the composite material, thereby building bridges between fillers to form a large thermal conductive network and improve thermal conductivity.

[0004] According to the existing chemical synthesis method, that is, annealing boron- and nitrogen-containing precursors at normal pressure and high temperature in a tubular furnace, the surface of the prepared hexagonal boron nitride sheet is smooth. When used in composite materials, the contact area with the matrix material is small, which leads to limited enhancement of thermal conductivity.

[0005] In addition, the traditional chemical vapor deposition method for growing boron nitride nanotubes requires the addition of catalysts and boron sources from the outside during the preparation process. Many factors such as boron sources and catalysts have a great influence on the structure, morphology and yield of BNNTs. In addition, the growth is difficult and the product uniformity is difficult to control. Summary of the invention

[0006] The purpose of the present invention is to provide a hexagonal boron nitride sheet derived with a boron nitride nanotube structure and a preparation method and application thereof, which does not require the addition of an external boron source as a catalyst, has a simple preparation process, low equipment requirements, is easy to industrialize, and greatly saves equipment costs.

[0007] In order to achieve the above object, the present invention provides a method for preparing a hexagonal boron nitride sheet having a boron nitride nanotube structure, the method comprising the following steps:

[0008] (1) Preparation of ZIF-67 modified hexagonal boron nitride flakes

[0009] The hexagonal boron nitride sheet is immersed in methanol and mixed with a 2-methylimidazole methanol solution to obtain a mixed solution A;

[0010] The mixed solution A is mixed with the cobalt nitrate hexahydrate methanol solution, and the mixture is stirred sufficiently to react to obtain a mixed solution B, and the mixed solution is allowed to stand;

[0011] The mixed solution B is separated and dried to obtain a ZIF-67 modified hexagonal boron nitride flake precursor, which is referred to as ZIF-67@BNFs;

[0012] (2) Preparation of MgCo-ZIF modified hexagonal boron nitride flakes

[0013] The ZIF-67@BNFs and the magnesium chloride hexahydrate methanol solution were mixed, stirred sufficiently to react, and a mixed solution C was obtained, and allowed to stand;

[0014] The mixed solution C is separated and dried to obtain a MgCo-ZIF modified hexagonal boron nitride flake precursor, which is recorded as MgCo-ZIF@BNFs;

[0015] (3) Preparation of hexagonal boron nitride flakes-boron nitride nanotube precursors

[0016] The MgCo-ZIF@BNFs are added to a boric acid aqueous solution, heated and stirred at 30 to 100° C. to obtain a slurry precursor;

[0017] Drying the slurry precursor to obtain a hexagonal boron nitride flake-boron nitride nanotube precursor;

[0018] (4) Amination of hexagonal boron nitride flakes and boron nitride nanotube precursors

[0019] The hexagonal boron nitride sheet-boron nitride nanotube precursor is heated to 1100-1600° C. in an inert atmosphere, and then ammonia gas is introduced for ammoniation treatment to react, and then naturally cooled to room temperature to obtain a hexagonal boron nitride sheet with a derived boron nitride nanotube structure.

[0020] Preferably, in step (1), the molar ratio of the hexagonal boron nitride flakes to 2-methylimidazole is (1-5):(2-1).

[0021] More preferably, in step (1), the molar ratio of the hexagonal boron nitride flakes to 2-methylimidazole is 2:1.5.

[0022] Preferably, in step (1), the molar ratio of cobalt nitrate hexahydrate to 2-methylimidazole is 1:(2-50).

[0023] More preferably, in step (1), the molar ratio of cobalt nitrate hexahydrate to 2-methylimidazole is 1:5.0-5.2.

[0024] Preferably, in any one or both of steps (1) to (2), the standing time is 2 to 48 hours; or / and,

[0025] In any one or more of steps (1) to (3), the drying temperature is 40 to 200°C.

[0026] Preferably, in step (2), the mass ratio of magnesium chloride hexahydrate to ZIF-67@BNFs is (1-10): (0.1-5).

[0027] More preferably, in step (2), the mass ratio of magnesium chloride hexahydrate to ZIF-67@BNFs is 6 to 7:5.

[0028] Preferably, in step (1), the concentration of the methanol solution of hexagonal boron nitride flakes is 1 to 20 mol / L; the concentration of the methanol solution of 2-methylimidazole is 1 to 20 mol / L; or / and, in step (1), the concentration of the methanol solution of cobalt nitrate hexahydrate is 0.1 to 10 mol / L; or / and, in step (2), the concentration of the methanol solution of magnesium chloride hexahydrate is 0.1 to 10 mol / L; or / and, in step (3), the concentration of the aqueous boric acid solution is 0.1 to 10 mol / L.

[0029] More preferably, in step (1), the concentration of the methanol solution of hexagonal boron nitride flakes is 2 mol / L; the concentration of the methanol solution of 2-methylimidazole is 3 mol / L; or / and, in step (1), the concentration of the methanol solution of cobalt nitrate hexahydrate is 0.58 mol / L; or / and, in step (2), the concentration of the methanol solution of magnesium chloride hexahydrate is 0.3 mol / L; or / and, in step (3), the concentration of the aqueous boric acid solution is 0.5 mol / L.

[0030] Preferably, in step (4), the temperature is heated to 1300-1400° C. and then ammonia gas is introduced for ammoniation treatment.

[0031] Preferably, in step (4), the gas of the inert atmosphere is selected from any one or more of nitrogen, argon, helium, neon and radon; or / and, the heating is carried out at a rate of 1 to 15°C / min to a temperature of 1100 to 1600°C; or / and, the ammoniation treatment time is 1 to 10 hours. The present invention controls the ammoniation conditions to obtain hexagonal boron nitride flakes with a boron nitride nanotube structure.

[0032] More preferably, in step (4), the heating is increased to 1300-1400° C. at a rate of 1-2° C. / min; or / and the ammoniation treatment is performed for 1-3 h.

[0033] More preferably, in step (4), the hexagonal boron nitride sheet-boron nitride nanotube precursor is heated to 1100-1600° C. in a 100 sccm inert atmosphere, and then 100 sccm ammonia gas is introduced for ammonia treatment to carry out a reaction, and the ammonia gas is switched to a 100 sccm inert atmosphere, and the mixture is naturally cooled to room temperature to obtain a hexagonal boron nitride sheet with a boron nitride nanotube structure.

[0034] Preferably, in step (4), the precursor is placed in a crucible, and the crucible used may be, but is not limited to, an alumina crucible, a silicon nitride crucible or a boron nitride crucible.

[0035] Another object of the present invention is to provide a hexagonal boron nitride sheet having a boron nitride nanotube structure derived therefrom obtained by the preparation method.

[0036] Another object of the present invention is to provide the application of the hexagonal boron nitride sheet derived with the boron nitride nanotube structure in the field of heat conduction.

[0037] The hexagonal boron nitride sheet with a boron nitride nanotube structure derived from the present invention and the preparation method and application thereof have the following advantages:

[0038] Compared with traditional hexagonal boron nitride sheets and BNNTs nanofillers, the boron nitride sheet-boron nitride nanotube structure prepared by the present invention utilizes a magnesium-cobalt bimetallic organic framework to derive boron nitride nanotubes on hexagonal boron nitride sheets, which can give full play to the synergistic effect of the sheets and tubes, improve the interface characteristics, and significantly increase the contact area. The bridging structure formed by BNNTs and the boron nitride sheets makes it easier to overlap, thereby improving the conduction efficiency of phonons. A complete and continuous thermal conductive network can be constructed inside the polymer matrix at a lower filling amount, thereby generating an efficient thermal network by increasing the nanofiller / matrix contact area and reducing the interface thermal resistance, which can effectively broaden the application of boron nitride in the field of functional composite materials.

[0039] Compared with the prior art, the present invention does not need to add an external boron source as a catalyst. The traditional chemical vapor deposition method for growing boron nitride nanotubes requires the addition of catalysts and boron sources from the outside, which is difficult to grow and difficult to control product uniformity. Compared with the commonly used method, the present invention has a simple preparation process, solves the problems of expensive equipment and complex process, has low requirements for equipment, is easy to realize industrialization, greatly saves equipment costs, and the chemical raw materials used are cheap and easy to obtain. The prepared hexagonal boron nitride sheet-boron nitride nanotube structure has important application prospects in the field of thermal conductivity, and provides a basis for realizing large-scale preparation of high-quality and high-purity boron nitride nanotubes. BRIEF DESCRIPTION OF THE DRAWINGS

[0040] Figure 1 This is a SEM photograph of the sample prepared in Example 1 of the present invention.

[0041] Figure 2 This is the X-ray diffraction (XRD) pattern of the sample prepared in Example 1 of the present invention.

[0042] Figure 3 This is a SEM photograph of the sample prepared in Example 2 of the present invention.

[0043] Figure 4 This is a SEM photograph of the sample prepared in Example 3 of the present invention.

[0044] Figure 5 This is a SEM photograph of the sample prepared in Comparative Example 1 of the present invention. DETAILED DESCRIPTION

[0045] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0046] A hexagonal boron nitride sheet having a boron nitride nanotube structure is prepared by a method comprising:

[0047] (1) Preparation of ZIF-67 modified hexagonal boron nitride flakes

[0048] The hexagonal boron nitride flake powder is soaked in methanol and mixed with 2-methylimidazole methanol solution to ensure complete adsorption and assembly on its surface. Subsequently, the mixed solution is further mixed with cobalt nitrate hexahydrate methanol solution, stirred thoroughly to achieve full reaction, and a mixed solution is obtained, which is allowed to stand. The mixed solution is centrifuged and dried to obtain a ZIF-67 modified hexagonal boron nitride flake precursor powder, recorded as ZIF-67@BNFs.

[0049] (2) Preparation of MgCo-ZIF modified hexagonal boron nitride flakes

[0050] The obtained ZIF-67@BNFs powder and the magnesium chloride hexahydrate methanol solution were mixed, and the components were uniformly dispersed and fully reacted by stirring to obtain a mixed solution, which was allowed to stand. The mixed solution was centrifuged and dried to obtain a MgCo-ZIF modified hexagonal boron nitride flake precursor powder, which was recorded as MgCo-ZIF@BNFs.

[0051] (3) Preparation of hexagonal boron nitride flakes-boron nitride nanotube precursors

[0052] Boric acid was dissolved in deionized water, and the obtained MgCo-ZIF@BNFs powder was added to the boric acid aqueous solution, heated and stirred in a water bath, and a slurry precursor was obtained. The precursor solution was dried to obtain hexagonal boron nitride flakes-boron nitride nanotube precursor powder.

[0053] (4) Precursor powder amination

[0054] The hexagonal boron nitride flake-boron nitride nanotube precursor powder is placed in a crucible, and is continuously heated to a certain temperature in an inert atmosphere, and then ammonia gas is introduced for a period of time for ammonia treatment to react, and then naturally cooled to room temperature to obtain a hexagonal boron nitride flake-boron nitride nanotube structure powder, on which a boron nitride nanotube structure is derived.

[0055] Compared with the prior art, the present invention does not require the addition of an external boron source as a catalyst. The traditional chemical vapor deposition method for growing boron nitride nanotubes requires the addition of catalysts and boron sources from the outside, which makes growth difficult and the product uniformity difficult to control. Moreover, compared with the existing methods, the existing methods usually require multiple temperature zone heating equipment, and the technology of heating the external boron source at high temperature so that gaseous B is formed or the precursor containing solid B is decomposed to form an active B reactant. However, this will cause the synthesis of BNNTs to be dispersed throughout the container, resulting in a decrease in the efficiency of collecting BNNTs. The preparation process of the present invention is simple, and only the treated sample needs to be heated and aminated to obtain hexagonal boron nitride flakes loaded with boron nitride nanotubes, which solves the problems of complex process and reduced efficiency of collecting BNNTs. The present invention has low equipment requirements and is easy to industrialize, greatly saving equipment costs. The chemical raw materials used are cheap and easy to obtain. The prepared hexagonal boron nitride flake-boron nitride nanotube structure has important application prospects in the field of thermal conductivity, and provides a basis for large-scale preparation of high-quality and high-purity boron nitride nanotubes. In addition, hexagonal boron nitride flakes loaded with boron nitride nanotubes have not been reported in the literature.

[0056] The boron nitride nanotube structure derived from the hexagonal boron nitride flakes prepared by the present invention, when applied to composite materials, can give full play to the synergistic effect of the flakes and the tubes, improve the interface characteristics, and significantly increase the contact area. The bridging structure formed by BNNTs and the hexagonal boron nitride flakes makes it easier to overlap and improves the conduction efficiency of phonons. A complete and continuous thermal conductive network can be constructed inside the polymer matrix at a relatively low filling amount, thereby improving the thermal conductivity.

[0057] Furthermore, in the step of preparing the ZIF-67 modified hexagonal boron nitride flakes, the concentration of the methanol solution of the hexagonal boron nitride flakes is 1 to 20 mol / L.

[0058] Furthermore, in the step of preparing the ZIF-67 modified hexagonal boron nitride flakes, the concentration of the methanol solution of the hexagonal boron nitride flakes is 2 mol / L.

[0059] Furthermore, in the step of preparing the ZIF-67 modified hexagonal boron nitride flakes, the concentration of the 2-methylimidazole methanol solution is 1 to 20 mol / L.

[0060] Furthermore, in the step of preparing the ZIF-67 modified hexagonal boron nitride flakes, the concentration of the methanol solution of 2-methylimidazole is 3 mol / L.

[0061] Furthermore, in the step of preparing the ZIF-67 modified hexagonal boron nitride flakes, the molar ratio of the hexagonal boron nitride flakes to 2-methylimidazole is (1-5): (2-1).

[0062] Furthermore, in the step of preparing the ZIF-67 modified hexagonal boron nitride flakes, the concentration of the methanol solution of cobalt nitrate hexahydrate is 0.1 to 10 mol / L.

[0063] Furthermore, in the step of preparing the ZIF-67 modified hexagonal boron nitride flakes, the concentration of the methanol solution of cobalt nitrate hexahydrate is 0.58 mol / L.

[0064] Furthermore, in the step of preparing the ZIF-67 modified hexagonal boron nitride flakes, the molar ratio of cobalt nitrate hexahydrate to 2-methylimidazole is 1:(2-50).

[0065] Furthermore, in the step of preparing the ZIF-67 modified hexagonal boron nitride flakes, the standing time is 2 to 48 hours and the drying temperature is 40 to 200°C.

[0066] Furthermore, in the step of preparing the hexagonal boron nitride flakes modified by MgCo-ZIF, the mass ratio of magnesium chloride hexahydrate to ZIF-67@BNFs is (1-10): (0.1-5).

[0067] Furthermore, in the step of preparing the hexagonal boron nitride flakes modified with MgCo-ZIF, the concentration of the methanol solution of magnesium chloride hexahydrate is 0.1 to 10 mol / L.

[0068] Furthermore, in the step of preparing the hexagonal boron nitride flakes modified with MgCo-ZIF, the concentration of the methanol solution of magnesium chloride hexahydrate is 0.3 mol / L.

[0069] Furthermore, in the step of preparing the MgCo-ZIF modified hexagonal boron nitride flakes, the standing time is 2 to 48 hours and the drying temperature is 40 to 200°C.

[0070] Furthermore, in the step of preparing the hexagonal boron nitride sheet-boron nitride nanotube precursor, the concentration of the boric acid aqueous solution is 0.1-10 mol / L.

[0071] Furthermore, in the step of preparing the hexagonal boron nitride sheet-boron nitride nanotube precursor, the concentration of the boric acid aqueous solution is 0.5 mol / L.

[0072] Furthermore, in the step of preparing the hexagonal boron nitride sheet-boron nitride nanotube precursor, the water bath stirring temperature is 30-100°C, and the drying temperature is 40-200°C.

[0073] Furthermore, in the precursor powder ammoniation treatment step, the inert gas used is selected from any one or more of nitrogen, argon, helium, neon and radon; or / and, the temperature is raised to 1100-1600°C at a rate of 1-15°C / min; or / and, the ammoniation time is 1-10h.

[0074] Furthermore, in the step of ammoniation treatment of the precursor powder, the temperature is raised to 1300-1400° C. at a rate of 1-2° C. / min; or / and the ammoniation treatment time is 1-3 hours.

[0075] Furthermore, in the precursor powder ammoniation treatment step, the hexagonal boron nitride flake-boron nitride nanotube precursor is heated to 1100-1600° C. in a 100 sccm inert atmosphere, and then 100 sccm ammonia gas is introduced for ammoniation treatment to carry out a reaction. The ammonia gas is switched to a 100 sccm inert atmosphere, and the mixture is naturally cooled to room temperature to obtain a hexagonal boron nitride flake with a boron nitride nanotube structure derived therefrom.

[0076] Furthermore, in the precursor powder ammoniation treatment step, the crucible used may be, but is not limited to, an alumina crucible, a silicon nitride crucible, or a boron nitride crucible.

[0077] In order to better illustrate the technical solution of the present invention, the present invention will be further described below in conjunction with the following Example 1. It should be noted here that the example is only a detailed description of the technical solution and does not limit the protection scope of the present invention.

[0078] Example 1

[0079] A boron nitride nanotube structure derived from a hexagonal boron nitride sheet, the preparation method of which is as follows:

[0080] (1) Preparation of ZIF-67 modified hexagonal boron nitride flakes (ZIF-67@BNFs)

[0081] 0.50g (0.02mol) of hexagonal boron nitride flakes were soaked in 10mL of methanol. Then, 5mL of a methanol solution containing 1.23g (0.015mol) of 2-methylimidazole was added to ensure that it was completely adsorbed and assembled on the surface of the boron nitride flakes. Then, 5mL of a methanol solution containing 0.83g (0.0029mol) of cobalt nitrate hexahydrate was added, and the mixed solution was obtained after sufficient stirring and allowed to stand for 12 hours. The mixed solution was then centrifuged at 5000 rpm for 5min, the obtained precipitate was washed 3 times with methanol, and then dried at 65°C for 12h to obtain ZIF-67@BNFs.

[0082] (2) Preparation of MgCo-ZIF modified hexagonal boron nitride flakes (MgCo-ZIF / BNFs)

[0083] 0.5 g ZIF-67@BNFs was placed in 10 mL 0.3 mol / L magnesium chloride hexahydrate methanol solution, stirred thoroughly, and allowed to stand for 12 h. The mixed solution was then centrifuged at 5000 rpm for 5 min, washed with methanol three times, and dried at 65 °C for 12 h to obtain MgCo-ZIF / BNFs.

[0084] (3) Preparation of hexagonal boron nitride flakes-boron nitride nanotube precursor powder

[0085] 0.5 g of MgCo-ZIF / BNFs was placed in 5 mL of 0.5 mol / L boric acid aqueous solution, stirred in a water bath at 80° C. to obtain a slurry precursor, which was dried at 65° C. for 12 h to obtain a boron nitride sheet-boron nitride nanotube precursor powder.

[0086] (4) Precursor powder amination

[0087] The prepared hexagonal boron nitride flake-boron nitride nanotube precursor powder was placed in an alumina crucible, and continuously heated to 1300°C at a heating rate of 2°C / min in a 100sccm nitrogen atmosphere. The nitrogen was then switched to 100sccm ammonia for ammonia treatment for 1h. After the reaction was completed, the ammonia was switched to 100sccm nitrogen, cooled to room temperature, and then taken out to obtain hexagonal boron nitride flake-boron nitride nanotube powder.

[0088] like Figure 1 As shown in the electron microscope photograph, the hexagonal boron nitride flakes obtained in Example 1 are loaded with a large number of boron nitride nanotubes, the length of the boron nitride nanotubes is greater than 20 μm, and the diameter is 20 to 80 nm.

[0089] like Figure 2 As shown in the XRD spectrum of the hexagonal boron nitride flakes-boron nitride nanotubes obtained in Example 1, the peaks at 26.7°, 41.7°, 55.2° and 75.9° correspond to the (002), (100), (004) and (110) planes of h-BN, respectively, proving that the prepared product is a h-BN structure with higher purity.

[0090] Example 2

[0091] In this embodiment, in step (4) the ammoniation treatment, the ammoniation temperature is 1400° C., and the rest is the same as in Example 1.

[0092] like Figure 3 As shown, it is a SEM photograph of the product obtained in Example 2 of the present invention. The obtained hexagonal boron nitride flakes are loaded with a large number of boron nitride nanotubes. As the temperature increases, the diameter of the obtained boron nitride nanotubes increases and the length increases.

[0093] Example 3

[0094] In this embodiment, in the ammoniation treatment of step (4), the ammoniation time is 3 hours, and the rest is the same as in Example 1.

[0095] like Figure 4 As shown, it is a SEM photograph of the product obtained in Example 3 of the present invention. The obtained hexagonal boron nitride flakes are loaded with a large amount of boron nitride nanotubes. As the amination time is prolonged, the diameter of the obtained boron nitride nanotubes becomes larger.

[0096] Comparative Example 1

[0097] In this comparative example, step (2) in Example 1 is omitted, and ZIF-67@BNFs is directly subjected to step (3), and the other steps are the same as in Example 1.

[0098] like Figure 5As shown, it is a SEM photograph of the boron nitride nanotubes obtained in Comparative Example 1 of the present invention. It is found through testing that only some particles of the obtained product are loaded on the hexagonal boron nitride flakes, and the hexagonal boron nitride flakes loaded boron nitride nanotube structure cannot be obtained.

[0099] Although the content of the present invention has been described in detail through the above preferred embodiments, it should be appreciated that the above description should not be considered as a limitation of the present invention. After reading the above content, it will be apparent to those skilled in the art that various modifications and substitutions of the present invention will occur. Therefore, the protection scope of the present invention should be limited by the appended claims.

Claims

1. A method for preparing a hexagonal boron nitride sheet having a boron nitride nanotube structure, characterized in that: The following steps of the method include: (1) Preparation of ZIF-67 modified hexagonal boron nitride flakes The hexagonal boron nitride sheet is immersed in methanol and mixed with a 2-methylimidazole methanol solution to obtain a mixed solution A; The mixed solution A is mixed with the cobalt nitrate hexahydrate methanol solution, and the mixture is stirred sufficiently to react to obtain a mixed solution B, and the mixed solution is allowed to stand; The mixed solution B is separated and dried to obtain a ZIF-67 modified hexagonal boron nitride flake precursor, which is referred to as ZIF-67@BNFs; (2) Preparation of MgCo-ZIF modified hexagonal boron nitride flakes The ZIF-67@BNFs and the magnesium chloride hexahydrate methanol solution were mixed, stirred sufficiently to react, and a mixed solution C was obtained, and allowed to stand; The mixed solution C is separated and dried to obtain a MgCo-ZIF modified hexagonal boron nitride flake precursor, which is recorded as MgCo-ZIF@BNFs; (3) Preparation of hexagonal boron nitride flakes-boron nitride nanotube precursors The MgCo-ZIF@BNFs are added to a boric acid aqueous solution, heated and stirred at 30 to 100° C. to obtain a slurry precursor; Drying the slurry precursor to obtain a hexagonal boron nitride flake-boron nitride nanotube precursor; (4) Amination of hexagonal boron nitride flakes and boron nitride nanotube precursors The hexagonal boron nitride sheet-boron nitride nanotube precursor is heated to 1100-1600° C. in an inert atmosphere, and then ammonia gas is introduced for ammoniation treatment to react, and then naturally cooled to room temperature to obtain a hexagonal boron nitride sheet with a derived boron nitride nanotube structure.

2. The preparation method according to claim 1, characterized in that: In step (1), the molar ratio of the hexagonal boron nitride flakes to 2-methylimidazole is (1-5): (2-1).

3. The preparation method according to claim 1, characterized in that: In step (1), the molar ratio of cobalt nitrate hexahydrate to 2-methylimidazole is 1:(2-50).

4. The preparation method according to claim 1, characterized in that: In any one or both of steps (1) to (2), the standing time is 2 to 48 hours; Or / and, in any one or more of steps (1) to (3), the drying temperature is 40 to 200°C.

5. The preparation method according to claim 1, characterized in that: In step (2), the mass ratio of magnesium chloride hexahydrate to ZIF-67@BNFs is (1-10): (0.1-5).

6. The preparation method according to claim 1, characterized in that: In step (1), the concentration of the methanol solution of the hexagonal boron nitride flakes is 1 to 20 mol / L; Or / and, in step (1), the concentration of the methanol solution of 2-methylimidazole is 1 to 20 mol / L; or / and, in step (1), the concentration of the methanol solution of cobalt nitrate hexahydrate is 0.1 to 10 mol / L; Or / and, in step (2), the concentration of the methanol solution of magnesium chloride hexahydrate is 0.1 to 10 mol / L; Or / and, in step (3), the concentration of the boric acid aqueous solution is 0.1 to 10 mol / L.

7. The preparation method according to claim 1, characterized in that: In step (4), the gas of the inert atmosphere is selected from any one or more of nitrogen, argon, helium, neon and radon; Or / and, the heating is carried out at a rate of 1 to 15°C / min to a temperature of 1100 to 1600°C; Or / and, the time of the ammoniation treatment is 1 to 10 hours.

8. The preparation method according to claim 1, characterized in that: In step (4), the hexagonal boron nitride flakes-boron nitride nanotube precursor powder is placed in a crucible, and the crucible is selected from an alumina crucible, a silicon nitride crucible or a boron nitride crucible.

9. A hexagonal boron nitride sheet having a boron nitride nanotube structure derived therefrom obtained by the preparation method according to any one of claims 1 to 8.

10. Use of the hexagonal boron nitride sheet derived with a boron nitride nanotube structure as claimed in claim 9 in the field of heat conduction.

Citation Information

Patent Citations

  • Boron nitride nanotube coated optical waveguide and uses thereof

    CA3053149A1

  • Method for preparing multi-layer hexagonal boron nitride film

    WO2020057672A1