Method for preparing titanium-doped iron phosphate from metatitanic acid and titanium dioxide by-products
By combining metatitanium acid with titanium dioxide by-products, the pH is controlled by using the co-flow of high-temperature concentrated sulfuric acid and sodium hexametaphosphate, the problem of poor uniformity of titanium doping is solved, and the uniform distribution of titanium and impurity removal is achieved, and low impurity doping is obtained. Titanium iron phosphate meets battery grade requirements.
Patent Information
- Application Number
- CN202411223959.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-03
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2044-09-03
AI Technical Summary
The titanium doping in the existing iron phosphate-doped titanium is poor in uniformity, resulting in uneven distribution of titanium and it is difficult to meet the battery level requirements.
The method of preparing titanium doped titanium phosphate by hydrolyzing metatitanium acid and titanium dioxide by-products is used to control pH by hydrolyzing metatitanium acid by solid-liquid separation, beating and washing, treatment with high-temperature concentrated sulfuric acid, adding ferrous sulfate and sodium hexametaphosphate, and flow control of pH , ensure that the titanium is evenly distributed in ion form, and after washing and calcining, iron doped titanium phosphate with low impurity ion content is obtained.
The uniform distribution of titanium and the effective removal of impurity ions are achieved, and the finished titanium doped iron phosphate products with very low impurity ion content are obtained, meeting the battery grade requirements.
Smart Images

Figure CN119079966A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of preparation of ferric phosphate-doped titanium, and in particular to a method for preparing titanium-doped ferric phosphate by utilizing metatitanic acid and titanium dioxide byproducts. Background Art
[0002] Most of the currently known methods for preparing titanium doped with iron phosphate are to ball-mill calcined titanium dioxide together with iron phosphate, a carbon source, and a lithium source to a certain particle size, and then calcine under the protection of an inert gas. The uniformity of titanium doping obtained by this preparation method is not as good as that obtained by directly doping it in iron phosphate. The reason is that during the grinding process, the titanium dioxide particles are uneven. Although some grinding equipment can achieve a particle size distribution as narrow as possible before the calcination process, the size gap is still large at both ends of the particle size distribution.
[0003] The existing process is to add nano-titanium dioxide to ferrous sulfate. In the process of synthesizing iron phosphate, the nano-titanium dioxide is used as a nucleation seed, so that the precipitate phase is attached to the nano-titanium dioxide. The problem that arises in this type of process is still the huge difference between the two ends of the particle size distribution, which is not conducive to the later uniform distribution of Ti in the lithium iron phosphate, such as patent CN202211595974.X. There are also some processes that directly mix the ferrous sulfate of titanium-containing liquid (titanic sulfate) with ferrous sulfate without titanium liquid, and then oxidize to synthesize iron phosphate, such as patent CN202311785880.3. The manganese and magnesium ions in the ferrous sulfate of titanium-containing liquid are generally high. Even if it is mixed with ferrous sulfate without titanium liquid, it is difficult to meet the requirements of battery-grade iron phosphate (metal impurity content ≤ 100ppm) after purification of impurities. If the titanium liquid attached to the titanium dioxide by-product ferrous sulfate after freeze filtration is directly used as a titanium-doped raw material without purification, the disadvantage is that there are too many impurity ions; if purified, the disadvantage is that during the purification process, Ti will precipitate with impurities, and the solubility product constant Ksp of titanium phosphate is much smaller than the solubility product constant Ksp of manganese phosphate and magnesium phosphate. There are also some that directly use hydrolyzed metatitanic acid as a titanium source for doping. At this time, the metatitanic acid is already uneven in particle size, and this method cannot evenly distribute titanium. Summary of the invention
[0004] 1. Technical issues to be solved
[0005] The purpose of the present invention is to solve the problem of poor uniformity of titanium doping caused by the preparation method of titanium doped ferric phosphate in the prior art, and to propose a method for preparing titanium doped ferric phosphate using metatitanic acid and titanium dioxide byproduct.
[0006] 2. Technical solution
[0007] In order to achieve the above object, the present invention adopts the following technical solutions:
[0008] A method for preparing titanium-doped ferric phosphate using metatitanic acid and titanium dioxide byproducts comprises the following steps:
[0009] Step 1: Separate the hydrolyzed metatitanic acid into solid and liquid, and the filter cake is metatitanic acid, which is pulped and washed twice by a leaf filter to obtain purified metatitanic acid;
[0010] Step 2: Beat the titanic acid to 300-350 g / L, transfer it into a reactor, add 98% concentrated sulfuric acid, turn on the jacket for heating, and observe through the observation window that the titanic acid turns into a dark brown transparent titanyl sulfate liquid under the action of high temperature concentrated sulfuric acid;
[0011] Step 3: adding the prepared titanyl sulfate to the prepared ferrous sulfate solution, stirring evenly in the reactor until the liquid is clear, so that the doped titanium is evenly distributed in the entire reactor in the form of ions;
[0012] Step 4: prepare a predetermined amount of sodium hexametaphosphate and hydrogen peroxide mixture, add the mixture into the reactor, and simultaneously add sulfuric acid and sodium hexametaphosphate in parallel to maintain the pH between 1.2 and 1.5;
[0013] Step 5: Slowly introduce 28% ammonia water into the reactor, control the pH of the reactor system to be between 1.5-1.8, and precipitate the iron source and titanium source;
[0014] Step 6: Wash the yellow iron phosphate precursor until the filtrate conductivity is below 1000us / cm, add a phosphorus source for aging, and a light pink iron phosphate is generated after a few hours. After subsequent washing, drying and calcination, a titanium-doped iron phosphate product with a very low content of other impurity ions is obtained.
[0015] Preferably, the content of Mn and Mg in the metatitanate purified in step 1 is less than 20 ppm.
[0016] Preferably, in step 2, the mass ratio of concentrated sulfuric acid to titanic acid is 6:8.
[0017] Preferably, in step 2, the jacket is heated to 130-150° C. and kept warm for 2-3 hours.
[0018] Preferably, in step 4, the molar ratio of P:Fe is 1-1.2:1, and H 2 O 2 :Fe substance ratio is 0.55-0.65:1, and the mixed liquid is added into the reactor.
[0019] Preferably, in step 4, sulfuric acid is added in parallel and the pH is maintained to prevent the local pH from being too high and causing iron hydroxide precipitation.
[0020] Preferably, in step 5, it is necessary to ensure that other impurities remain in the solution in the form of ions.
[0021] Preferably, the phosphorus source in step 6 is sodium phosphate, ammonium phosphate or phosphoric acid.
[0022] 3. Beneficial effects
[0023] Compared with the prior art, the advantages of the present invention are:
[0024] In the present invention, the step of purifying titanium is placed in the first step so that it will not be consumed by the subsequent purification process; the washed solid titanium is dissolved into an ionic state without adding other metal impurities, and sodium hexametaphosphate and hydrogen peroxide are flowed in parallel with sulfuric acid to control the pH, so as to prevent the local pH from being too high to generate iron hydroxide precipitation and being unable to be evenly dispersed in the slurry; the pH is controlled by ammonia water to only precipitate iron and titanium, and other metal impurity ions are washed away, thereby obtaining a titanium-doped iron phosphate product with a very low impurity ion content. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 The present invention provides a process flow chart of a method for preparing titanium-doped ferric phosphate by utilizing metatitanic acid and titanium dioxide byproduct. DETAILED DESCRIPTION
[0026] The technical solutions in the embodiments of the present invention will be described clearly and completely below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all the embodiments.
[0027] Embodiment 1:
[0028] Reference Figure 1 A method for preparing titanium-doped ferric phosphate using metatitanic acid and titanium dioxide byproducts comprises the following steps:
[0029] Step 1: Separate the hydrolyzed metatitanic acid into solid and liquid, and the filter cake is metatitanic acid, which is washed twice by a leaf filter to obtain purified metatitanic acid, wherein the content of Mn and Mg in the purified metatitanic acid is less than 20 ppm;
[0030] Step 2: Beat the titanic acid to 300-350 g / L, transfer it into a reactor, add 98% concentrated sulfuric acid, the mass ratio of concentrated sulfuric acid to titanic acid is 6-8:1, turn on the jacket heating, raise the temperature to 130-150°C, keep it warm for 2-3 hours, and observe through the observation window that the titanic acid turns into a dark brown transparent titanyl sulfate liquid under the action of high-temperature concentrated sulfuric acid;
[0031] Step 3: adding the prepared titanyl sulfate to the prepared ferrous sulfate solution, stirring evenly in the reactor until the liquid is clear, so that the doped titanium is evenly distributed in the entire reactor in the form of ions;
[0032] Step 4: Prepare a mixture of sodium hexametaphosphate and hydrogen peroxide, with a molar ratio of P:Fe of 1-1.2:1 and H 2 O 2 The molar ratio of Fe: Fe is 0.55-0.65:1, the mixed solution is added into the reactor, and sulfuric acid and sodium hexametaphosphate are added in parallel to maintain the pH between 1.2-1.5;
[0033] Step 5: Slowly introduce 28% ammonia water into the reactor, control the pH of the reactor system to be between 1.5-1.8, and precipitate the iron source and titanium source;
[0034] Step 6: Wash the yellow iron phosphate precursor until the filtrate conductivity is below 1000us / cm, add a phosphorus source for aging, the phosphorus source type is sodium phosphate, ammonium phosphate or phosphoric acid, and after a few hours, a light pink iron phosphate is generated, followed by washing, drying and calcining to obtain a titanium-doped iron phosphate product with very low content of other impurity ions.
[0035] In this embodiment, the step of purifying titanium is placed in the first step so that it will not be consumed by the subsequent purification process; the washed solid titanium is dissolved into an ionic state without adding other metal impurities, and sodium hexametaphosphate and hydrogen peroxide are flowed in parallel with sulfuric acid to control the pH to prevent the local pH from being too high to form iron hydroxide precipitation, which cannot be evenly dispersed in the slurry; the pH is controlled by ammonia water to only precipitate iron and titanium, and other metal impurity ions are washed away, thereby obtaining a titanium-doped iron phosphate product with a very low impurity ion content.
[0036] Embodiment 2:
[0037] In this embodiment, a method for preparing titanium-doped ferric phosphate using metatitanic acid and titanium dioxide byproducts comprises the following steps:
[0038] Step 1: Separate the hydrolyzed metatitanic acid into solid and liquid, and the filter cake is metatitanic acid, which is washed twice by a leaf filter to obtain purified metatitanic acid with Mn and Mg contents less than 20 ppm;
[0039] Step 2: Beat the titanic acid to 350g / l, transfer it into a reactor, add 98% concentrated sulfuric acid at a mass ratio of 6:1, turn on the jacket heating, raise the temperature to 150°C, and keep it warm for 3 hours. Through the observation window, it can be seen that the titanic acid turns into a dark brown titanyl sulfate liquid under the action of high-temperature concentrated sulfuric acid;
[0040] Step 3: Add the prepared titanyl sulfate to the prepared ferrous sulfate solution and stir evenly in the reactor. This is a clear liquid, so the doped titanium is evenly distributed in the entire reactor in the form of ions;
[0041] Step 4: prepare a mixture of sodium hexametaphosphate and hydrogen peroxide, according to the molar ratio of P:Fe being 1.2:1 and the molar ratio of H2O2:Fe being 0.55:1, add the mixed solution into the reactor, and add sulfuric acid and sodium hexametaphosphate in parallel, maintaining the pH at about 1.5;
[0042] Step 5: Slowly introduce 28% ammonia water into the reactor, control the pH of the reactor system to be between 1.8, precipitate the iron source and titanium source, and ensure that other impurities remain in the solution in the form of ions;
[0043] Step 6: Wash the yellow iron phosphate precursor until the conductivity of the filtrate is below 1000us / cm, add a phosphorus source for aging, and a light pink iron phosphate is generated after a few hours. After subsequent washing, drying and calcination, a titanium-doped iron phosphate product with very low content of other impurity ions is obtained.
[0044] Embodiment 3:
[0045] In this embodiment, a method for preparing titanium-doped ferric phosphate using metatitanic acid and titanium dioxide byproducts comprises the following steps:
[0046] Step 1: Separate the hydrolyzed metatitanic acid into solid and liquid, and the filter cake is metatitanic acid, which is washed twice by a leaf filter to obtain purified metatitanic acid with Mn and Mg contents less than 20 ppm;
[0047] Step 2: Beat the titanic acid to 330 g / l, transfer it into a reactor, add 98% concentrated sulfuric acid at a mass ratio of 7:1, turn on the jacket heating, raise the temperature to 140°C, keep it warm for 2 hours, and observe through the observation window that the titanic acid turns into dark brown titanyl sulfate liquid under the action of high-temperature concentrated sulfuric acid;
[0048] Step 3: Add the prepared titanyl sulfate to the prepared ferrous sulfate solution and stir evenly in the reactor. This is a clear liquid, so the doped titanium is evenly distributed in the entire reactor in the form of ions;
[0049] Step 4: prepare a mixture of sodium hexametaphosphate and hydrogen peroxide, according to the molar ratio of P:Fe being 1.1:1 and the molar ratio of H2O2:Fe being 0.6:1, add the mixed solution into the reactor, and add sulfuric acid and sodium hexametaphosphate in parallel, maintaining the pH at about 1.35;
[0050] Step 5: Slowly introduce 28% ammonia water into the reactor, control the pH of the reactor system to be between 1.65, precipitate the iron source and titanium source, and ensure that other impurities remain in the solution in the form of ions;
[0051] Step 6: Wash the yellow iron phosphate precursor until the conductivity of the filtrate is below 1000us / cm, add a phosphorus source for aging, and a light pink iron phosphate is generated after a few hours. After subsequent washing, drying and calcination, a titanium-doped iron phosphate product with very low content of other impurity ions is obtained.
[0052] Embodiment 4:
[0053] In this embodiment, a method for preparing titanium-doped ferric phosphate using metatitanic acid and titanium dioxide byproducts comprises the following steps:
[0054] Step 1: Separate the hydrolyzed metatitanic acid into solid and liquid, and the filter cake is metatitanic acid, which is washed twice by a leaf filter to obtain purified metatitanic acid with Mn and Mg contents less than 20 ppm;
[0055] Step 2: Beat the titanic acid to 300 g / l, transfer it into a reactor, add 98% concentrated sulfuric acid at a mass ratio of 8:1, turn on the jacket heating, raise the temperature to 130°C, and keep it warm for 2 hours. Through the observation window, it can be seen that the titanic acid turns into a dark brown titanyl sulfate liquid under the action of high-temperature concentrated sulfuric acid;
[0056] Step 3: Add the prepared titanyl sulfate to the prepared ferrous sulfate solution and stir evenly in the reactor. This is a clear liquid, so the doped titanium is evenly distributed in the entire reactor in the form of ions;
[0057] Step 4: prepare a mixture of sodium hexametaphosphate and hydrogen peroxide, according to the molar ratio of P:Fe being 1:1 and the molar ratio of H2O2:Fe being 0.65:1, add the mixed solution into the reactor, and add sulfuric acid and sodium hexametaphosphate in parallel, maintaining the pH at about 1.2;
[0058] Step 5: Slowly introduce 28% ammonia water into the reactor, control the pH of the reactor system to be between 1.5, precipitate the iron source and titanium source, and ensure that other impurities remain in the solution in the form of ions;
[0059] Step 6: Wash the yellow iron phosphate precursor until the conductivity of the filtrate is below 1000us / cm, add a phosphorus source for aging, and a light pink iron phosphate is generated after a few hours. After subsequent washing, drying and calcination, a titanium-doped iron phosphate product with very low content of other impurity ions is obtained.
[0060] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.
Claims
1. A method for preparing titanium-doped ferric phosphate using metatitanic acid and titanium dioxide byproducts, characterized in that: The following steps are involved: Step 1: Separate the hydrolyzed metatitanic acid into solid and liquid, and the filter cake is metatitanic acid, which is pulped and washed twice by a leaf filter to obtain purified metatitanic acid; Step 2: Beat the titanic acid to 300-350 g / L, transfer it into a reactor, add 98% concentrated sulfuric acid, turn on the jacket for heating, and observe through the observation window that the titanic acid turns into a dark brown transparent titanyl sulfate liquid under the action of high temperature concentrated sulfuric acid; Step 3: adding the prepared titanyl sulfate to the prepared ferrous sulfate solution, stirring evenly in the reactor until the liquid is clear, so that the doped titanium is evenly distributed in the entire reactor in the form of ions; Step 4: prepare a predetermined amount of sodium hexametaphosphate and hydrogen peroxide mixture, add the mixture into the reactor, and simultaneously add sulfuric acid and sodium hexametaphosphate in parallel to maintain the pH between 1.2 and 1.5; Step 5: Slowly introduce 28% ammonia water into the reactor, control the pH of the reactor system to be between 1.5-1.8, and precipitate the iron source and titanium source; Step 6: Wash the yellow iron phosphate precursor until the filtrate conductivity is below 1000us / cm, add a phosphorus source for aging, and a light pink iron phosphate is generated after a few hours. After subsequent washing, drying and calcination, a titanium-doped iron phosphate product with a very low content of other impurity ions is obtained.
2. The method for preparing titanium-doped ferric phosphate by using metatitanic acid and titanium dioxide byproduct according to claim 1, characterized in that: The content of Mn and Mg in the metatitanate purified in step 1 is less than 20 ppm.
3. The method for preparing titanium-doped ferric phosphate by using metatitanic acid and titanium dioxide byproduct according to claim 1, characterized in that: In step 2, the mass ratio of concentrated sulfuric acid to titanic acid is 6:
8.
4. The method for preparing titanium-doped ferric phosphate using metatitanic acid and titanium dioxide byproduct according to claim 1, characterized in that: In the step 2, the jacket is heated to 130-150° C. and kept warm for 2-3 hours.
5. The method for preparing titanium-doped ferric phosphate by using metatitanic acid and titanium dioxide byproduct according to claim 1, characterized in that: In the step 4, the mixed solution is added into the reactor according to the molar ratio of P:Fe being 1-1.2:1 and the molar ratio of H2O2:Fe being 0.55-0.65:
1.
6. The method for preparing titanium-doped ferric phosphate by using metatitanic acid and titanium dioxide byproduct according to claim 1, characterized in that: In step 4, sulfuric acid is added in parallel and the pH is maintained to prevent the local pH from being too high and causing iron hydroxide precipitation.
7. The method for preparing titanium-doped ferric phosphate using metatitanic acid and titanium dioxide byproduct according to claim 1, characterized in that: In step 5, it is necessary to ensure that other impurities remain in the solution in the form of ions.
8. The method for preparing titanium-doped ferric phosphate by using metatitanic acid and titanium dioxide byproduct according to claim 1, characterized in that: In step 6, the phosphorus source is sodium phosphate, ammonium phosphate or phosphoric acid.
Citation Information
Patent Citations
Preparation method of ferric phosphate
CN107317029A
Method for preparing lithium titanate from inorganic titanium source, product and application
CN108529666A
Preparation method of battery-grade titanium-doped iron phosphate
CN118495494A
Cited By
Positive electrode material and preparation method thereof, positive electrode plate and secondary battery
CN120864466A
Process method for producing titanium-doped iron phosphate through continuous reaction
CN120987292A