Preparation method of porous silicon-carbon composite negative electrode material
By reacting silicon tetrachloride with ferrosilicon powder at high temperature and coating carbon nanotubes using chemical vapor deposition method, forming porous silicon-carbon composite negative electrode material, solving the problems of short cycle life and poor conductivity caused by volume changes of silicon material, significantly improving The conductivity and cycle stability of lithium-ion batteries are achieved.
Patent Information
- Application Number
- CN202411282048.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-13
- Publication Date
- 2024-12-06
AI Technical Summary
The volume change of silicon material during charging and discharging of lithium-ion batteries leads to a short cycle life and poor conductivity, which affects the application of materials.
After high-temperature reaction of silicon tetrachloride and ferrosilicon powder, carbon nanotubes were coated by chemical vapor deposition to form porous silicon-carbon composite anode material, improving the conductive network and alleviating the influence of volume expansion.
It improves the conductivity and cycle stability of the negative electrode material of lithium-ion battery and extends the service life of the battery.
Smart Images

Figure CN119080004A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of secondary batteries, and in particular relates to a method for preparing a porous silicon-carbon composite negative electrode material. Background Art
[0002] At present, the theoretical capacity of graphite negative electrodes in commercial lithium-ion batteries is about 372mAh / g, which is far from meeting the growing demand for energy storage device capacity in the energy storage field. Among the many candidate negative electrode materials, the theoretical capacity of silicon materials is more than 10 times that of graphitized carbon materials. In addition, they are environmentally friendly, have abundant reserves, and are cheap. They have the advantages of high mass-to-capacity, low charge and discharge platform, abundant resources, and good safety. They have become one of the most promising negative electrode materials for lithium-ion batteries. However, silicon materials undergo severe volume changes during the charge and discharge process, resulting in a short cycle life and poor conductivity, which brings huge difficulties to the application of materials.
[0003] Among them, amorphous silicon has an ultra-high capacity close to that of crystalline silicon, and the volume expansion of the electrode material during the charge and discharge process is also smaller than that of crystalline silicon; and amorphous silicon has better mechanical stability and can withstand greater stress before structural damage, which can alleviate the adverse effects caused by volume expansion. Therefore, amorphous silicon is also a relatively promising silicon negative electrode material. However, amorphous silicon has poor conductivity and has a certain limit to buffering the negative impact of volume expansion. Therefore, it is still necessary to develop a negative electrode material with good conductivity that can better alleviate the volume expansion of amorphous silicon. Summary of the invention
[0004] The purpose of the present invention is to provide a method for preparing a porous silicon-carbon composite negative electrode material in order to solve the above problems. The obtained porous silicon-carbon composite negative electrode material is used for the negative electrode plate of a lithium-ion battery, has a relatively stable structure, and exhibits excellent conductivity and cycle stability.
[0005] The method for preparing the porous silicon-carbon composite negative electrode material in the technical solution of the present invention comprises the following steps: stirring and mixing silicon tetrachloride and iron silicon powder, washing and drying the obtained mixture after high temperature reaction to obtain composite silicon, and then chemically vapor depositing the composite silicon.
[0006] After silicon tetrachloride and iron silicon powder are mixed, they are subjected to a high-temperature reaction to obtain a composite silicon composed of porous silicon and amorphous silicon. The ferric chloride generated by the reaction is washed away, and then carbon nanotubes are coated by chemical vapor deposition (CVD) to finally obtain a porous silicon-carbon composite negative electrode material. The pore structure not only improves the conductive network of the negative electrode material and improves its conductive performance, but also can bind amorphous silicon in the pores, strengthening the buffering effect on the volume expansion of the negative electrode material.
[0007] Furthermore, the weight ratio of silicon tetrachloride to iron silicon powder is 1:3 to 1:5.
[0008] Furthermore, the iron silicon powder is a mixture of iron disilicide (FeSi2) phase and Si phase.
[0009] The FeSi2 phase in the iron silicon powder can induce the in-situ growth of carbon nanotubes, improve the coating effect of the carbon nanotube re-composite silicon surface, enhance the structural stability of the silicon-carbon composite negative electrode material, and thus improve the cycle stability of lithium-ion batteries.
[0010] Furthermore, the mass percentage of the iron disilicide phase in the iron silicon powder is 20-25%.
[0011] Preferably, the stirring and mixing of silicon tetrachloride and iron silicon powder is carried out in nitrogen or argon.
[0012] Furthermore, the temperature of the high temperature reaction is 150-250° C., and the time is 6-12 hours.
[0013] Preferably, the high temperature reaction is carried out in a hydrothermal reactor.
[0014] Preferably, after the high temperature reaction, the mixture is washed with dilute hydrochloric acid and ethanol in sequence, and then dried at 60-100°C.
[0015] Furthermore, the chemical vapor deposition is performed in an acetylene gas atmosphere.
[0016] Furthermore, the temperature of chemical vapor deposition is 800-1000° C., and the time is 4-12 hours.
[0017] The present invention also provides a porous silicon-carbon composite negative electrode material, which is prepared by the above-mentioned method for preparing the porous silicon-carbon composite negative electrode material.
[0018] The present invention also provides a lithium ion battery negative electrode plate, comprising the above-mentioned porous silicon-carbon composite negative electrode material, a binder and a conductive agent.
[0019] The binder in the present invention is not limited, and any binder that can be applied to lithium-ion batteries can be used. The binder is one or more of polyvinylidene fluoride, sodium alginate, sodium carboxymethyl cellulose, polyacrylonitrile binders, polyurethane binders, and polyimide binders.
[0020] The conductive agent in the present invention is not limited, and any conductive agent that can be applied to lithium-ion batteries can be used. The conductive agent can be one or more of conductive carbon black, conductive graphite, carbon fiber, and carbon nanotubes.
[0021] Furthermore, the amounts of the porous silicon-carbon composite negative electrode material, the binder and the conductive agent in the negative electrode plate of the lithium-ion battery are 7.0 to 9.0 parts, 0.5 to 1.5 parts and 0.5 to 1.5 parts respectively.
[0022] Compared with the prior art, the technical solution of the present invention has the following beneficial effects:
[0023] (1) Silicon tetrachloride and iron silicon powder are mixed and reacted at high temperature, and then carbon-coated by chemical vapor deposition (CVD) to obtain a porous silicon-carbon composite negative electrode material;
[0024] (2) The pore structure in the obtained porous silicon-carbon composite negative electrode material not only improves the conductive network of the negative electrode material and improves its conductive performance, but also can bind amorphous silicon in the pores, thereby enhancing the buffering effect on the volume expansion of the negative electrode material;
[0025] (3) The FeSi2 phase in the iron silicon powder can induce the in-situ growth of carbon nanotubes, improve the coating effect of the carbon nanotube recombinant silicon surface, enhance the structural stability of the silicon-carbon composite negative electrode material, and thus improve the cycle stability of the lithium-ion battery;
[0026] (4) The obtained porous silicon-carbon composite negative electrode material is used for the negative electrode plate of lithium-ion batteries, has a relatively stable structure, and exhibits excellent conductivity and cycle stability;
[0027] (5) The preparation method of porous silicon-carbon composite negative electrode material is simple and easy to operate, and is suitable for large-scale industrial application. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] Figure 1 This is the XRD pattern of the porous silicon-carbon composite negative electrode material obtained in Example 1;
[0029] Figure 2 This is a cycle performance diagram of the porous silicon-carbon composite negative electrode material obtained in Example 1; DETAILED DESCRIPTION
[0030] The technical scheme of the present invention is further described below by specific examples and accompanying drawings. It should be understood that the specific examples described herein are only used to help understand the present invention and are not intended for specific limitations of the present invention. The accompanying drawings used herein are only for better illustrating the disclosed content of the present invention and do not have a limiting effect on the scope of protection. If not otherwise specified, the raw materials used in the embodiments of the present invention are all commonly used raw materials in the art, and the methods used in the embodiments are all conventional methods in the art.
[0031] Example 1
[0032] The method for preparing the porous silicon-carbon composite negative electrode material of this embodiment comprises the following steps:
[0033] (1) Silicon tetrachloride and iron silicon powder (Ningbo Guangxin Nanomaterial Co., Ltd.) were stirred and mixed in an argon atmosphere at a mass ratio of 1:4, wherein the content of FeSi2 phase in the iron silicon powder was 20%, and the obtained mixture was transferred to a hydrothermal reactor, reacted at 200° C. for 8 h, washed with dilute hydrochloric acid and ethanol in turn, and dried at 80° C. to obtain composite silicon;
[0034] (2) placing the composite silicon in a CVD furnace tube, introducing acetylene gas, heating to 1000°C and reacting for 6 hours to obtain a porous silicon-carbon composite negative electrode material; Figure 1 As shown, the obtained porous silicon-carbon composite negative electrode material contains crystalline silicon and FeSi2 phase.
[0035] The porous silicon-carbon composite negative electrode material, polyacrylic acid binder and conductive carbon black (Super P) were mixed evenly in a mass ratio of 8:1:1, coated on a copper foil, punched into discs after drying, and vacuum dried at 90° C. for 8 h to obtain a negative electrode sheet for a lithium-ion battery.
[0036] Example 2
[0037] The method for preparing the porous silicon-carbon composite negative electrode material of this embodiment comprises the following steps:
[0038] (1) Silicon tetrachloride and iron silicon powder (Ningbo Guangxin Nanomaterial Co., Ltd.) were stirred and mixed in an argon atmosphere at a mass ratio of 1:4, wherein the content of FeSi2 phase in the iron silicon powder was 25%, and the obtained mixture was transferred to a hydrothermal reactor, reacted at 180° C. for 8 h, washed with dilute hydrochloric acid and ethanol in turn, and dried at 80° C. to obtain composite silicon;
[0039] (2) The composite silicon is placed in a CVD furnace tube, acetylene gas is introduced, the temperature is raised to 950° C. and the reaction is carried out for 8 hours to obtain a porous silicon-carbon composite negative electrode material.
[0040] The porous silicon-carbon composite negative electrode material, polyacrylic acid binder and conductive carbon black (Super P) were mixed evenly in a mass ratio of 7.5:1.0:1.5, coated on a copper foil, punched into discs after drying, and vacuum dried at 90° C. for 8 h to obtain a negative electrode sheet for a lithium-ion battery.
[0041] Example 3
[0042] The method for preparing the porous silicon-carbon composite negative electrode material of this embodiment comprises the following steps:
[0043] (1) Silicon tetrachloride and iron silicon powder (Ningbo Guangxin Nanomaterial Co., Ltd.) were stirred and mixed in an argon atmosphere at a mass ratio of 1:4, wherein the content of FeSi2 phase in the iron silicon powder was 25%, and the obtained mixture was transferred to a hydrothermal reactor, reacted at 230° C. for 8 h, washed with dilute hydrochloric acid and ethanol in turn, and dried at 80° C. to obtain composite silicon;
[0044] (2) The composite silicon is placed in a CVD furnace tube, acetylene gas is introduced, the temperature is raised to 900° C. and the reaction is carried out for 10 hours to obtain a porous silicon-carbon composite negative electrode material.
[0045] The porous silicon-carbon composite negative electrode material, polyacrylic acid binder and conductive carbon black (Super P) were mixed evenly in a mass ratio of 7.5:1.5:1.0, coated on a copper foil, punched into discs after drying, and vacuum dried at 90° C. for 8 h to obtain a negative electrode sheet for a lithium-ion battery.
[0046] Example 4
[0047] The difference between this embodiment and embodiment 1 is that in step (1), silicon tetrachloride and iron silicon powder are stirred and mixed in an argon atmosphere in a mass ratio of 1:3, and the content of FeSi2 phase in the iron silicon powder is 25%. The obtained mixture is transferred to a hydrothermal reactor, reacted at 200°C for 8h, washed with dilute hydrochloric acid and ethanol in turn, and dried at 80°C to obtain composite silicon.
[0048] Example 5
[0049] The difference between this embodiment and embodiment 1 is that in step (1), silicon tetrachloride and iron silicon powder are stirred and mixed in an argon atmosphere at a mass ratio of 1:5, the content of FeSi2 phase in the iron silicon powder is 20%, and the obtained mixture is transferred to a hydrothermal reactor, reacted at 200°C for 8h, washed with dilute hydrochloric acid and ethanol in turn, and dried at 80°C to obtain composite silicon.
[0050] Example 6
[0051] The difference between this embodiment and embodiment 1 is that in step (1), silicon tetrachloride and iron silicon powder are stirred and mixed in an argon atmosphere in a mass ratio of 1:2, and the content of FeSi2 phase in the iron silicon powder is 20%. The obtained mixture is transferred to a hydrothermal reactor, reacted at 200°C for 8h, washed with dilute hydrochloric acid and ethanol in turn, and dried at 80°C to obtain composite silicon.
[0052] Example 7
[0053] The difference between this embodiment and embodiment 1 is that in step (1), silicon tetrachloride and iron silicon powder are stirred and mixed in an argon atmosphere at a mass ratio of 1:6, the content of FeSi2 phase in the iron silicon powder is 20%, and the obtained mixture is transferred to a hydrothermal reactor, reacted at 200°C for 8h, washed with dilute hydrochloric acid and ethanol in turn, and dried at 80°C to obtain composite silicon.
[0054] Example 8
[0055] The difference between this embodiment and embodiment 1 is that in step (1), silicon tetrachloride and iron silicon powder are stirred and mixed in an argon atmosphere in a mass ratio of 1:3, and the content of FeSi2 phase in the iron silicon powder is 5%. The obtained mixture is transferred to a hydrothermal reactor, reacted at 200°C for 8h, washed with dilute hydrochloric acid and ethanol in turn, and dried at 80°C to obtain composite silicon.
[0056] Example 9
[0057] The difference between this embodiment and embodiment 1 is that in step (1), silicon tetrachloride and iron silicon powder are stirred and mixed in an argon atmosphere in a mass ratio of 1:3, the content of FeSi2 phase in the iron silicon powder is 40%, and the obtained mixture is transferred to a hydrothermal reactor, reacted at 200°C for 8h, washed with dilute hydrochloric acid and ethanol in turn, and dried at 80°C to obtain composite silicon.
[0058] Comparative Example 1
[0059] The difference between this comparative example and Example 1 is that in step (1), silicon tetrachloride and a mixture of iron powder and silicon powder are stirred and mixed in an argon atmosphere in a mass ratio of 1:3, the content of iron powder in the mixture of iron powder and silicon powder is 5%, and the obtained mixture is transferred to a hydrothermal reactor, reacted at 200° C. for 8 h, washed with dilute hydrochloric acid and ethanol in turn, and dried at 80° C. to obtain composite silicon.
[0060] Comparative Example 2
[0061] The difference between this comparative example and Example 1 is that in step (2), the composite silicon and carbon nanotubes are placed in a high-temperature reaction tube, argon gas is introduced, the temperature is raised to 1000° C. and reacted for 6 hours to obtain a silicon-carbon composite negative electrode material.
[0062] Comparative Example 3
[0063] The preparation method of the silicon-carbon composite negative electrode material in this comparative example comprises the following steps: placing silicon powder in a CVD furnace tube, introducing acetylene gas, heating to 1000° C. and reacting for 6 hours to obtain the silicon-carbon composite negative electrode material.
[0064] The negative electrode of the lithium-ion battery obtained in the above embodiments and comparative examples is the working electrode, the metal lithium is the counter electrode, and the electrolyte is 1 mol / L LiPF6 / DMC:EC (V:V=7:3) containing 5% FEC electrolyte additive; button batteries are assembled in a glove box protected by argon atmosphere. The battery tester of Wuhan Blue Electric Electronics Co., Ltd. is used for electrochemical performance testing. The charge and discharge voltage range is 0.01V~1.5V (vs.Li+ / Li), and the test temperature is 30°C. The obtained performance data are shown in Table 1.
[0065] Table 1 Lithium-ion battery electrochemical performance data
[0066]
[0067] according to Figure 2 As can be seen from Table 1, the porous silicon-carbon composite negative electrode materials obtained in Examples 1-5 have a relatively stable structure and show excellent conductivity and cycle stability; Example 6 uses more silicon tetrachloride and less iron silicon powder to mix to obtain composite silicon, and the FeSi2 in the iron silicon powder reacts completely, so that during the chemical vapor deposition process, there is a lack of FeSi2 phase to induce the in-situ growth of carbon nanotubes, causing an incomplete conductive carbon network, which significantly reduces the material cycle performance; Example 7 uses less silicon tetrachloride and more iron silicon powder to mix to obtain composite silicon, wherein the silicon tetrachloride reacts completely, and more FeSi2 phase remains, the pore structure after cleaning is reduced, the overall capacity is low, and the reversible capacity after the cycle is reduced; Example 8 uses less FeSi2 phase in the iron silicon powder, the amorphous silicon obtained by reduction is less, the content of in-situ grown carbon nanotubes is also less, the structural stability of the silicon-carbon composite negative electrode material is reduced, and the cycle stability is poor; Example 9 The content of FeSi2 phase in the iron silicon powder used is relatively high, the proportion of unreacted FeSi2 is relatively high, the overall capacity of the material is relatively low, and the reversible capacity after the cycle is reduced; Comparative Example 1 uses silicon tetrachloride to mix with iron powder and silicon powder to prepare composite silicon. There is no uniform and effective pore structure in the composite silicon, and the carbon nanotubes generated by the CVD method are arranged in a disorderly manner, and the mitigation effect on volume expansion is reduced. The conductivity and cycle performance of the resulting negative electrode material are both reduced; Comparative Example 2 uses composite silicon and carbon nanotubes to react at high temperature to prepare silicon-carbon composite materials. The carbon nanotubes have poor dispersion effect and cannot be well attached to the surface of the composite silicon. The conductive network is imperfect, the conductivity is reduced, the support and mitigation effect on volume expansion is also reduced, and the cycle performance is also reduced; Comparative Example 3 places silicon powder in a CVD furnace tube for chemical vapor deposition to prepare a silicon-carbon composite material. There is no pore structure in the composite material, the surface carbon layer is easily broken when the silicon volume expands, and the cycle stability is significantly reduced.
[0068] Finally, it should be noted that the specific embodiments described herein are merely examples of the spirit of the present invention, and are not intended to limit the implementation methods of the present invention. Those skilled in the art of the present invention may make various modifications or supplements to the described embodiments or replace them in similar ways. It is not necessary and impossible to provide all examples of all implementation methods here. However, these obvious changes or modifications derived from the essential spirit of the present invention still fall within the scope of protection of the present invention, and interpreting them as any additional limitation is contrary to the spirit of the present invention.
Claims
1. A method for preparing a porous silicon-carbon composite negative electrode material, It is characterized in that The method comprises the following steps: mixing silicon tetrachloride and iron silicon powder, subjecting the obtained mixture to high temperature reaction, washing and drying to obtain composite silicon, and then subjecting the composite silicon to chemical vapor deposition.
2. The preparation method according to claim 1, It is characterized in that The weight ratio of silicon tetrachloride to iron silicon powder is 1:3 to 1:
5.
3. The preparation method according to claim 1, It is characterized in that Iron silicon powder is a mixture of iron disilicide phase and Si phase.
4. The preparation method according to claim 3, It is characterized in that The mass percentage of the iron disilicide phase in the iron silicon powder is 20-25%.
5. The preparation method according to claim 1, It is characterized in that The temperature of the high temperature reaction is 150-250°C and the time is 6-12 hours.
6. The preparation method according to claim 1, It is characterized in that Chemical vapor deposition is carried out in an acetylene atmosphere.
7. The preparation method according to claim 1, It is characterized in that The temperature of chemical vapor deposition is 800-1000°C and the time is 4-12 hours.
8. A porous silicon-carbon composite negative electrode material, It is characterized in that The method is prepared according to claim 1.
9. A negative electrode plate for a lithium-ion battery, comprising the porous silicon-carbon composite negative electrode material according to claim 8, a binder and a conductive agent.
10. The negative electrode plate of a lithium-ion battery according to claim 9, It is characterized in that The usage of the porous silicon-carbon composite negative electrode material, the binder and the conductive agent are 7.0-9.0 parts, 0.5-1.5 parts and 0.5-1.5 parts respectively.