Method for producing silicon oxide aerogel by using mineral solid waste raw material with carbon dioxide as regulator

By using carbon dioxide regulators in the production process of silicon-based aerogels, silicon oxide is activated from mineral solid waste, the problems of high energy consumption and serious pollution in the production process of silicon-based aerogels are solved, and high-efficiency and low-pollution oxidation is achieved Silicon aerogel extraction has promoted the development of the silicon aerosol industry and the sustainable utilization of resources.

CN119080009AInactive Publication Date: 2024-12-06GUANGZHOU INST OF ENERGY CONVERSION CHINESE ACAD OF SCI
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202310657247.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-06-05
Publication Date
2024-12-06
Estimated Expiration
Not applicable · inactive patent
Patent Text Reader

Abstract

The invention discloses a method for producing silicon oxide aerogel from a mineral solid waste raw material by using carbon dioxide as a regulator. The method comprises the following steps: activating silicon-containing mineral solid waste to leach silicon oxide, adjusting the pH value by carbon dioxide, and replacing strong alkali carbonate in one step. The silicon oxide aerogel prepared by the invention has a developed pore structure, a high specific surface area and excellent heat insulation performance, can be used as a high-performance heat insulation material, a catalyst carrier and the like, and is widely applied to emerging industries such as building materials, traffic, new materials, Wentu and the like. The mineral solid waste is used as a silicon source, spontaneous carbon dioxide in the process is used as a regulator, inorganic acid consumption and subsequent acid radical pollution are avoided, application of micro-toxic organic silicon is reduced, the resource utilization rate is increased, the mineral solid waste is compatibly reduced, and the method serves a macro energy-saving and carbon-reducing target.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of mineral solid waste utilization and lightweight porous silicon-based materials, and in particular to a method for producing silicon oxide aerogel from mineral solid waste raw materials using carbon dioxide as a regulator. Background Art

[0002] Silicon is a key raw material in the semiconductor material industry. Silicon resources in nature mainly exist in the form of silicon oxide. The conversion of silicon oxide into silicon consumes a lot of energy, so the grade of resource silicon is required to be very high. However, although the amount of silicon oxide in natural minerals is large, it is usually of low grade. For example, the bulk solid waste produced in the production of other elements includes low-grade silicon oxide, which is generally used for simple landfill or paving. It has low economic value and limited consumption. The unconsumed mineral solid waste is piled up in large quantities, encroaching on land and polluting the environment. Silica-based aerogel is a new type of porous silicon material with high specific surface area, high porosity and low thermal conductivity. It shows wide application potential in the fields of thermal insulation, catalysis, sound absorption, biomedicine, adsorption, etc., especially in the field of building thermal insulation. The low thermal conductivity and lightweight characteristics of silica aerogel will have a large-scale application potential, which is of great significance to energy saving, reducing dead weight and reducing steel consumption, and will have a revolutionary impact on the building materials industry; at the same time, its unique microporous structure also makes it an excellent carrier for chemical reactions, and the catalyst loaded will greatly improve the reaction effect, save energy and reduce emissions. The development of this emerging material in the future involves a large supply of silicon oxide raw materials. The use of expensive pure silicon sources limits its wider application. The silicon oxide source provided by mineral solid waste has become a promising raw material supply channel. At the same time, the traditional silica aerosol technology process is lengthy, involves the use of inorganic strong acids, and is prone to chemical pollution, which greatly increases the production cost of silica aerosol and its high carbon emissions. At present, there is no silica aerogel production technology starting from mineral solid waste raw materials. Therefore, the large-scale use of silica components in mineral solid waste to develop the future silica aerosol industry will not only directly reduce production costs and promote its large-scale and wide application, but also achieve energy conservation and reduction, and effectively reduce the capacity of mineral solid waste and promote the sustainable development of the mining industry. Summary of the invention

[0003] The purpose of the present invention is to provide a method for producing silicon oxide aerogel from mineral solid waste raw materials using carbon dioxide as a regulator. The method proposed by the present invention can extract silicon oxide raw materials from mineral solid waste with high efficiency and low pollution, and at the same time utilize the carbon dioxide produced by the process itself to reduce the application of inorganic acid, subsequent pollution control and process carbon emissions, and form oxidized high-performance silicon aerogel in one step with high efficiency dehydration. The waste heat of the process serves the dehydration energy consumption, and better realizes the high-value utilization of solid waste while achieving energy conservation, emission reduction and efficient utilization of solid waste.

[0004] The present invention is achieved through the following technical solutions:

[0005] A method for producing silicon oxide aerogel using mineral solid waste raw materials with carbon dioxide as a regulator comprises the following steps:

[0006] (1) Activation and leaching of silicon oxide from mineral solid waste: At a temperature of 200°C to 1500°C and a pressure of 0.1 to 10 MPa, the silicon-containing mineral solid waste reacts with a strong alkali and weak acid salt solution or a strong alkali solution to activate and deconstruct the silicon oxide in the mineral solid waste to obtain a liquid phase product containing silicon oxide and a gas phase product containing carbon dioxide; at a temperature of 25°C to 500°C and a pressure of 0.1 to 10 MPa, the liquid phase product is immersed in water to dissolve the deconstructed silicon oxide to obtain a solution containing silicon oxide sol;

[0007] (2) adjusting the pH with carbon dioxide: introducing the carbon dioxide obtained in step (1) into the solution containing the silica sol obtained in step (1) at a temperature of 20° C. to 180° C. and a pressure of 0.1 to 10 MPa to adjust the pH of the solution containing the silica sol to 1 to 12, thereby forming a mixture of silica gel and a strong alkaline carbonate solution;

[0008] (3) One-step replacement of strong alkali carbonate: Adding a water-insoluble solvent A and a water-soluble solvent B soluble in solvent A to the mixture of step (2) at a temperature of 20°C to 200°C and a pressure of 0.1 to 10 MPa to replace the strong alkali carbonate solution in the silica gel, and drying the silica gel to obtain silica aerogel. Silica aerosol is a new material with large porosity, low thermal conductivity and extremely low density.

[0009] The deconstruction and activation of solid waste in step (1) creates conditions for efficient extraction of silicon oxide, and the subsequent water immersion treatment helps to improve the yield of silicon oxide. The carbon dioxide in step (2) comes from the carbon emissions generated in step (1), which enters the silica sol to form a strong alkaline carbonate; if the generated strong alkaline carbonate is not recycled back to step (1), it will play a role in carbon fixation. The replacement of the alkaline carbonate solution in step (3) creates conditions for the formation of silicon oxide aerogel with better performance. After replacement, the silicon oxide gel can be directly dried to obtain an aerogel.

[0010] The present invention constructs technical routes such as activated leaching of silicon oxide from mineral solid waste, adjustment of pH by carbon dioxide, fixation of carbon dioxide, one-step replacement of strong alkaline carbonate, and preparation of silicon-based aerosol, which improves process energy efficiency and product output value, consumes and utilizes mineral solid waste on a large scale, improves resource utilization efficiency, and is of great significance to environmental ecology and carbon emission reduction.

[0011] Preferably, the mass ratio of the silicon-containing mineral solid waste to the strong base weak acid salt solution or the strong base solution in step (1) is 1 to 5:1, and the mass fraction of the strong base weak acid salt solution or the strong base solution is 5%-100%, and 100% refers to the saturated state of the aqueous solution of the substance involved, the saturated solution. Further preferably, the mass ratio of the mineral solid waste to the strong base weak acid salt solution or the strong base solution is 1 to 3:1.

[0012] Preferably, the conditions for activating and deconstructing silicon oxide in mineral solid waste in step (1) are: temperature 450°C to 1200°C, pressure 0.1 to 1.0 MPa; the conditions for forming silicon oxide sol are: temperature 80°C to 150°C, pressure 0.1 to 0.6 MPa.

[0013] Preferably, the silicon-containing mineral solid waste described in step (1) includes coal-based solid waste and waste tailings, the coal-based solid waste is selected from at least one of fly ash, coal slime, coal gangue and gasification slag, and the waste tailings is selected from at least one of iron ore slag, steelmaking and ironmaking slag, manganese slag, tungsten slag, aluminum red mud and composite associated slag.

[0014] Preferably, the strong base and weak acid salt described in step (1) is an alkali metal carbonate or an alkaline earth metal carbonate, and the strong base is a strong alkali metal base or an alkaline earth metal base.

[0015] More preferably, the strong base and weak acid salt in step (1) is sodium carbonate or potassium carbonate, and the strong base is sodium hydroxide or potassium hydroxide.

[0016] Preferably, the pH adjustment conditions in step (2) are: temperature 20°C to 80°C, pressure 0.1 to 0.6 MPa, and the pH of the silica sol is adjusted to 5 to 8.

[0017] Preferably, the reaction conditions in step (3) are: temperature 80°C to 160°C, and pressure 0.2 to 3 MPa.

[0018] Preferably, the solvent A in step (3) is n-hexane, n-heptane or hexamethyldisiloxane with low surface tension, the solvent B is acetonitrile, ethanol or methanol, and the mass ratio of solvent A to solvent B is 2 to 20:1. Solvent B is an amphiphilic solvent. Solvent A and solvent B are chemically pure or industrial grade pure material raw materials, generally the industrial grade purity is 95-99.9%, and the chemical purity is 99.99%.

[0019] Preferably, the drying conditions in step (3) are: temperature -20°C to 500°C.

[0020] Compared with the prior art, the present invention has the following beneficial effects:

[0021] (1) The present invention extracts silicon oxide from mineral solid waste that usually contains a high proportion of silicon oxide through an activation step to form a silicon oxide sol, and uses the carbon dioxide generated in the activation process to adjust the pH of the silicon oxide sol, thereby saving the cost of conventional inorganic acid and avoiding subsequent pollution by acid radical ions; further, during the curing process, the silicon oxide sol is subjected to a silicon oxide microstructure to form a gel form, and finally, the weak base carbonate in the gel is replaced in a one-step method and dried to obtain a silicon oxide aerogel product.

[0022] (2) The silica aerogel proposed in the present invention has a developed pore structure, a high specific surface area and excellent thermal insulation performance, and can be used as a high-performance thermal insulation material and catalyst carrier, etc., and is widely used in emerging industries such as building materials, transportation, new materials, and cultural tourism. The present invention uses mineral solid waste as a silicon source and spontaneous carbon dioxide in the process as a regulator, avoiding inorganic acid consumption and subsequent acid radical pollution, reducing the application of micro-toxic organic silicon, improving resource utilization, and being compatible with and reducing mineral solid waste, serving the grand goal of energy conservation and carbon reduction. DETAILED DESCRIPTION

[0023] The present invention is further described in detail below with reference to the examples. These examples are only used to illustrate the present invention and are not intended to limit the scope of the present invention. The experimental methods in the following examples where specific conditions are not specified are generally based on conventional conditions in the art or conditions recommended by the manufacturer; the raw materials, reagents, etc. used, unless otherwise specified, are considered to be raw materials and reagents that can be obtained through commercial channels such as conventional markets.

[0024] Example 1

[0025] A method for producing silicon oxide aerogel using mineral solid waste raw materials with carbon dioxide as a regulator comprises the following steps:

[0026] (1) Activation leaching of silica from mineral solid waste: At a temperature of 450°C and a pressure of 0.1 MPa, fly ash in a mass ratio of 1:1 reacts with a potassium hydroxide solution with a mass fraction of 10% to activate and decompose the silica therein, thereby obtaining a liquid product containing silica and a gas product containing carbon dioxide; at a temperature of 120°C and a pressure of 0.2 MPa, the liquid product is immersed in clean water to dissolve the decomposed silica sol, thereby obtaining a solution containing silica sol.

[0027] (2) Adjusting pH with carbon dioxide: introducing carbon dioxide into the solution containing silica sol obtained in step (1) at a temperature of 50° C. and a pressure of 0.5 MPa to adjust the pH of the solution to 6, thereby forming a mixture of silica gel and strong alkaline carbonate solution.

[0028] (3) One-step replacement of strong base carbonate: adding n-hexane and methanol in a mass ratio of 10:1 to the mixture obtained in step (2) at a temperature of 80° C. and a pressure of 0.3 MPa to replace the strong base carbonate solution in the gel, and finally drying at a temperature of 120° C. to obtain silica aerogel.

[0029] Silica aerogel yield 62%, specific surface area 680m 2 / g.

[0030] Example 2

[0031] A method for producing silicon oxide aerogel using mineral solid waste raw materials with carbon dioxide as a regulator comprises the following steps:

[0032] (1) Activation leaching of silica from mineral solid waste: At a temperature of 550°C and a pressure of 1 MPa, rare earth slag in a mass ratio of 2:1 reacts with a sodium hydroxide solution with a mass fraction of 10% to activate and decompose the silica therein, thereby obtaining a liquid product containing silica and a gas product containing carbon dioxide; at a temperature of 120°C and a pressure of 0.2 MPa, the liquid product is immersed in clean water to dissolve the decomposed silica sol, thereby obtaining a solution containing silica sol.

[0033] (2) Adjusting pH with carbon dioxide: introducing carbon dioxide into the solution containing silica sol obtained in step (1) at a temperature of 30° C. and a pressure of 0.4 MPa to adjust the pH of the solution to 7, thereby forming a mixture of silica gel and strong alkaline carbonate solution.

[0034] (3) One-step replacement of strong base carbonate: adding n-hexane and ethanol in a mass ratio of 12:1 to the mixture obtained in step (2) at a temperature of 90° C. and a pressure of 0.4 MPa to replace the strong base carbonate solution in the gel, and finally drying at a temperature of 100° C. to obtain silica aerogel.

[0035] Silica aerogel yield 53%, specific surface area 710m 2 / g.

[0036] Example 3

[0037] A method for producing silicon oxide aerogel using mineral solid waste raw materials with carbon dioxide as a regulator comprises the following steps:

[0038] (1) Activation leaching of silica from mineral solid waste: At a temperature of 850°C and a pressure of 0.1 MPa, fly ash with a mass ratio of 1:1 reacts with a sodium carbonate solution with a mass fraction of 10%, activating and decomposing the silica therein to obtain a liquid product containing silica and a gas product containing carbon dioxide; at a temperature of 150°C and a pressure of 0.4 MPa, the liquid product is immersed in clean water to dissolve the decomposed silica sol to obtain a solution containing silica sol.

[0039] (2) Adjusting pH with carbon dioxide: introducing carbon dioxide into the solution containing silica sol obtained in step (1) at a temperature of 20° C. and a pressure of 0.1 MPa to adjust the pH of the solution to 8, thereby forming a mixture of silica gel and strong alkaline carbonate solution.

[0040] (3) One-step replacement of strong base carbonate: adding n-heptane and methanol in a mass ratio of 10:1 to the mixture obtained in step (2) at a temperature of 150° C. and a pressure of 2 MPa to replace the strong base carbonate solution in the gel, and finally drying at a temperature of 150° C. to obtain silica aerogel.

[0041] Silica aerogel yield 44%, specific surface area 626m 2 / g.

[0042] Example 4

[0043] A method for producing silicon oxide aerogel using mineral solid waste raw materials with carbon dioxide as a regulator comprises the following steps:

[0044] (1) Activation leaching of solid waste silicon oxide: At a temperature of 1200°C and a pressure of 0.1 MPa, fly ash with a mass ratio of 3:1 reacts with a sodium carbonate solution with a mass fraction of 5%, thereby activating and decomposing the silicon oxide therein to obtain a liquid product containing silicon oxide and a gas product containing carbon dioxide; at a temperature of 100°C and a pressure of 0.1 MPa, the liquid product is immersed in clean water to dissolve the decomposed silicon oxide sol to obtain a solution containing silicon oxide sol.

[0045] (2) Adjusting pH with carbon dioxide: introducing carbon dioxide into the solution containing silica sol obtained in step (1) at a temperature of 80° C. and a pressure of 0.2 MPa to adjust the pH of the solution to 5, thereby forming a mixture of silica gel and strong alkaline carbonate solution.

[0046] (3) One-step replacement of strong base carbonate: adding n-heptane and acetonitrile in a mass ratio of 20:1 to the mixture obtained in step (2) at a temperature of 80° C. and a pressure of 3 MPa to replace the strong base carbonate solution in the gel, and finally drying at a temperature of 80° C. to obtain silica aerogel.

[0047] Silica aerogel yield 53%, specific surface area 521m2 / g.

[0048] Example 5

[0049] A method for producing silicon oxide aerogel using mineral solid waste raw materials with carbon dioxide as a regulator comprises the following steps:

[0050] (1) Activation leaching of silica from mineral solid waste: At a temperature of 850°C and a pressure of 0.1 MPa, copper slag in a mass ratio of 2:1 reacts with a potassium carbonate solution with a mass fraction of 10% to activate and decompose the silica therein, thereby obtaining a liquid product containing silica and a gas product containing carbon dioxide; at a temperature of 120°C and a pressure of 0.3 MPa, the liquid product is immersed in clean water to dissolve the decomposed silica sol, thereby obtaining a solution containing silica sol.

[0051] (2) Adjusting pH with carbon dioxide: introducing carbon dioxide into the solution containing silica sol obtained in step (1) at a temperature of 25° C. and a pressure of 0.2 MPa to adjust the pH of the solution to 6, thereby forming a mixture of silica gel and strong alkaline carbonate solution.

[0052] (3) One-step replacement of strong base carbonate: adding hexamethylsiloxane and ethanol in a mass ratio of 10:1 to the mixture obtained in step (2) at a temperature of 100° C. and a pressure of 0.5 MPa to replace the strong base carbonate solution in the gel, and finally drying at a temperature of 140° C. to obtain silica aerogel.

[0053] Silica aerogel yield 57%, specific surface area 823m 2 / g.

[0054] Example 6

[0055] A method for producing silicon oxide aerogel using mineral solid waste raw materials with carbon dioxide as a regulator comprises the following steps:

[0056] (1) Activation leaching of silica from mineral solid waste: At a temperature of 800°C and a pressure of 0.1 MPa, red mud with a mass ratio of 1:1 reacts with a potassium carbonate solution with a mass fraction of 10%, thereby activating and decomposing the silica therein to obtain a liquid product containing silica and a gas product containing carbon dioxide; at a temperature of 80°C and a pressure of 0.5 MPa, the liquid product is immersed in clean water to dissolve the decomposed silica sol to obtain a solution containing silica sol.

[0057] (2) Adjusting pH with carbon dioxide: introducing carbon dioxide into the solution containing silica sol obtained in step (1) at a temperature of 70° C. and a pressure of 0.6 MPa to adjust the pH of the solution to 8, thereby forming a mixture of silica gel and strong alkaline carbonate solution.

[0058] (3) One-step replacement of strong base carbonate: adding hexamethylsiloxane and acetonitrile in a mass ratio of 15:1 to the mixture obtained in step (2) at a temperature of 160° C. and a pressure of 0.8 MPa to replace the strong base carbonate solution in the gel, and finally drying at a temperature of 120° C. to obtain silica aerogel.

[0059] Silica aerogel yield 51%, specific surface area 808m 2 / g.

[0060] Example 7

[0061] A method for producing silicon oxide aerogel using mineral solid waste raw materials with carbon dioxide as a regulator comprises the following steps:

[0062] (1) Activation leaching of silica from mineral solid waste: At a temperature of 600°C and a pressure of 0.1 MPa, manganese slag in a mass ratio of 2:1 reacts with a potassium hydroxide solution, where the mass fraction of the potassium hydroxide solution is 100%, to activate and decompose the silica therein, thereby obtaining a liquid product containing silica and a gas product containing carbon dioxide; at a temperature of 120°C and a pressure of 0.3 MPa, the liquid product is immersed in clean water to dissolve the decomposed silica sol, thereby obtaining a solution containing silica sol.

[0063] (2) Adjusting pH with carbon dioxide: introducing carbon dioxide into the solution containing silica sol obtained in step (1) at a temperature of 60° C. and a pressure of 0.4 MPa to adjust the pH of the solution to 5, thereby forming a mixture of silica gel and strong alkaline carbonate solution.

[0064] (3) One-step replacement of strong base carbonate: adding methylsiloxane and acetonitrile in a mass ratio of 20:1 to the mixture obtained in step (2) at a temperature of 120° C. and a pressure of 0.2 MPa to replace the strong base carbonate solution in the gel, and finally drying at a temperature of 120° C. to obtain silica aerogel.

[0065] Silica aerogel yield 60%, specific surface area 848m 2 / g.

[0066] Example 8

[0067] A method for producing silicon oxide aerogel using mineral solid waste raw materials with carbon dioxide as a regulator comprises the following steps:

[0068] (1) Activation leaching of silica from mineral solid waste: At a temperature of 500°C and a pressure of 0.1 MPa, a lead-zinc slag with a mass ratio of 1:1 reacts with a potassium hydroxide solution with a mass fraction of 10%, thereby activating and decomposing the silica therein to obtain a liquid product containing silica and a gas product containing carbon dioxide; at a temperature of 150°C and a pressure of 0.6 MPa, the liquid product is immersed in clean water to dissolve the decomposed silica sol to obtain a solution containing silica sol.

[0069] (2) Adjusting pH with carbon dioxide: introducing carbon dioxide into the solution containing silica sol obtained in step (1) at a temperature of 30° C. and a pressure of 0.2 MPa to adjust the pH of the solution to 8, thereby forming a mixture of silica gel and strong alkaline carbonate solution.

[0070] (3) One-step replacement of strong base carbonate: adding hexamethylsiloxane and ethanol in a mass ratio of 10:1 to the mixture obtained in step (2) at a temperature of 120° C. and a pressure of 0.2 MPa to replace the strong base carbonate solution in the gel, and finally drying at a temperature of 120° C. to obtain silica aerogel.

[0071] Silica aerogel yield 49%, specific surface area 762m 2 / g.

[0072] The description of the above embodiments is only used to help understand the technical solution and core ideas of the present invention. It should be pointed out that for technicians in this technical field, several improvements and modifications can be made to the present invention without departing from the principles of the present invention. These improvements and modifications also fall within the scope of protection of the claims of the present invention.

Claims

1. A method for producing silicon oxide aerogel using mineral solid waste raw materials with carbon dioxide as a regulator, characterized in that: The steps include: (1) Activation and leaching of silicon oxide from mineral solid waste: At a temperature of 200°C to 1500°C and a pressure of 0.1 to 10 MPa, silicon-containing mineral solid waste reacts with a strong alkali and weak acid salt solution or a strong alkali solution to activate and deconstruct silicon oxide in the mineral solid waste to obtain a liquid product containing silicon oxide and a gas product containing carbon dioxide; At a temperature of 25°C to 500°C and a pressure of 0.1 to 10 MPa, the liquid product is immersed in water to dissolve the deconstructed silicon oxide to obtain a solution containing silicon oxide sol; (2) adjusting the pH with carbon dioxide: introducing the carbon dioxide obtained in step (1) into the solution containing the silica sol obtained in step (1) at a temperature of 20° C. to 180° C. and a pressure of 0.1 to 10 MPa to adjust the pH of the solution containing the silica sol to 1 to 12, thereby forming a mixture of silica gel and a strong alkaline carbonate solution; (3) One-step replacement of strong base carbonate: adding a water-insoluble solvent A and a water-soluble solvent B soluble in solvent A to the mixture of step (2) at a temperature of 20°C to 200°C and a pressure of 0.1 to 10 MPa to replace the strong base carbonate solution in the silica gel, and drying the silica gel to obtain silica aerogel.

2. The method according to claim 1, characterized in that: The mass ratio of the silicon-containing mineral solid waste to the strong base weak acid salt solution or the strong base solution in step (1) is 1 to 5:1, and the mass fraction of the strong base weak acid salt solution or the strong base solution is 5% to 100%.

3. The method according to claim 2, characterized in that The conditions for activating and deconstructing silicon oxide in mineral solid waste in step (1) are: temperature 450°C to 1200°C and pressure 0.1 to 1.0 MPa; the conditions for forming silicon oxide sol are: temperature 80°C to 150°C and pressure 0.1 to 0.6 MPa.

4. The method according to claim 1 or 2, characterized in that: The silicon-containing mineral solid waste described in step (1) includes coal-based solid waste and waste tailings, wherein the coal-based solid waste is selected from at least one of fly ash, coal slime, coal gangue and gasification slag, and the waste tailings is selected from at least one of iron ore slag, steelmaking and ironmaking slag, manganese slag, tungsten slag, aluminum red mud and composite associated slag.

5. The method according to claim 1 or 2, characterized in that: The strong base and weak acid salt described in step (1) is an alkali metal carbonate or an alkaline earth metal carbonate, and the strong base is a strong alkali metal or an alkaline earth metal strong base.

6. The method according to claim 5, characterized in that The strong base and weak acid salt described in step (1) is sodium carbonate or potassium carbonate, and the strong base is sodium hydroxide or potassium hydroxide.

7. The method according to claim 1, characterized in that The pH adjustment conditions in step (2) are: temperature 20°C to 80°C, pressure 0.1 to 0.6 MPa, and the pH of the silica sol is adjusted to 5 to 8.

8. The method according to claim 1, characterized in that The reaction conditions of step (3) are: temperature 80°C to 160°C, pressure 0.2 to 3 MPa.

9. The method according to claim 1, characterized in that: The solvent A in step (3) is n-hexane, n-heptane or hexamethyldisiloxane, the solvent B is acetonitrile, ethanol or methanol, and the mass ratio of solvent A to solvent B is 2 to 20:

1.

10. The method according to claim 1 or 9, characterized in that: The drying conditions in step (3) are: temperature -20°C to 500°C.

Citation Information

Patent Citations

  • Production technique for extracting gallium from coal ash and coal gangue

    CN101255504A

  • Method for preparing silica aerogel from desilicication liquid of fly ash

    CN106986346A

  • Preparation method of simple aerogel daylighting glass

    CN111021629A

  • Method for concentrating mineral solid waste low-concentration occurrence rare and precious elements and co-producing high-grade aluminum-silicon raw materials

    CN114314597A

  • Method for preparing aluminum oxide and silicon dioxide from high-alumina fly ash

    CN114735732A