Alpha-type aluminum oxide and preparation method thereof, high-molecular polymer diaphragm and lithium battery

By grinding, calcining, slurrying and washing the aluminum hydroxide, the content of Na2O in the α-type alumina is reduced, the problem of high Na2O content in the lithium battery separator is solved, the purity and performance of the aluminum oxide are improved, and the The mechanical and safety performance requirements of lithium batteries.

CN119080038APending Publication Date: 2024-12-06CHALCO SHANDONG NEW MATERIALS CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411240682.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-05
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

The prior art is difficult to effectively reduce the Na2O content in α-type alumina, affecting the performance of lithium battery separators.

Method used

By grinding aluminum hydroxide to obtain a fine powder of a set particle size, a first calcination post-slurry is performed and CO2 gas is introduced for first desodium desodium, and then mixed with a mineralizer for second calcination, and a second calcination is achieved by washing. Desodium and gradually reduce the Na2O content.

Benefits of technology

The Na2O content in α-type alumina was successfully reduced to less than 0.02 wt%, and the purity and specific surface area of ​​alumina were improved, meeting the mechanical and safety performance requirements of lithium battery separators.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119080038A_ABST
    Figure CN119080038A_ABST
Patent Text Reader

Abstract

The invention relates to alpha-type aluminum oxide and a preparation method thereof, a high-molecular polymer diaphragm and a lithium battery, and the method comprises the following steps: grinding aluminum hydroxide to obtain aluminum hydroxide micro powder with set granularity; carrying out first calcination on the aluminum hydroxide micro powder to obtain gamma aluminum oxide; slurrying gamma aluminum oxide to obtain gamma aluminum oxide slurry; introducing CO2 gas into the gamma aluminum oxide slurry to realize first sodium removal of gamma aluminum oxide; mixing the gamma aluminum oxide subjected to the first sodium removal with a mineralizing agent, and then carrying out second calcination to obtain first alpha type aluminum oxide; and washing the alpha-type aluminum oxide to realize secondary sodium removal of the first alpha-type aluminum oxide to obtain the target alpha-type aluminum oxide. Through primary calcination, CO2 primary sodium removal, secondary calcination and water washing secondary sodium removal, sodium oxide in a target finished product is reduced to 0.02% or below, the main content of aluminum oxide reaches 99.9% or above, the median particle size of the finished product is 0.4-0.6 mu m, and the finished product is in a sphere-like shape.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of preparation of non-metallurgical aluminum oxide, and in particular to an α-type aluminum oxide and a preparation method thereof, a high molecular polymer diaphragm, and a lithium battery. Background Art

[0002] With the development of the country's new energy industry, the technical level of lithium batteries is gradually improving, and its application fields are becoming more and more extensive, but the safety performance of lithium batteries has always been widely concerned. In the physical structure of lithium batteries, the most important factors affecting their safety are the mechanical properties and thermal stability of the polymer separator. Therefore, a lot of research has been done on the modification of the separator, using high-melting-point polymer materials or coating inorganic materials and other technical solutions. In the inorganic material coating technology, Al2O3 has attracted much attention due to its good electrolyte wettability and stability, as well as high cost performance.

[0003] The higher the purity of calcined α-alumina used in the field of lithium battery separator coating, the better. The main impurities of industrial calcined α-alumina are Na2O, SiO2, Fe2O3, CaO, MgO, etc. In addition to these impurities with relatively high content, there are also some trace elements. Among them, the Na2O content is the most concerned chemical indicator in the application of finished products, which directly affects the performance of the products. Therefore, a method to reduce the Na2O content in α-alumina is urgently needed. Summary of the invention

[0004] The present application provides an α-alumina and a preparation method thereof, a polymer diaphragm, and a lithium battery to solve the following technical problem: how to reduce the Na2O content in the α-alumina.

[0005] In a first aspect, the present application provides a method for preparing α-alumina, the method comprising:

[0006] Grinding aluminum hydroxide to obtain aluminum hydroxide micropowder with a set particle size;

[0007] The aluminum hydroxide powder is first calcined to obtain gamma alumina;

[0008] Slurrying the gamma alumina to obtain a gamma alumina slurry;

[0009] Introducing CO2 gas into the gamma alumina slurry to achieve a first de-sodiumization of the gamma alumina;

[0010] The gamma alumina after the first sodium removal is mixed with a mineralizer, and then subjected to a second calcination to obtain a first alpha alumina;

[0011] The α-type alumina is washed to achieve a second de-sodiumization of the first α-type alumina to obtain the target α-type alumina.

[0012] Optionally, the set particle size is 3-5 μm.

[0013] Optionally, the endpoint pH value of the gamma alumina slurry after the CO2 gas is introduced is less than 7.

[0014] Optionally, the process parameters of the first calcination include: a temperature of 600° C. to 900° C. and a time of 30 min to 60 min; and / or,

[0015] The process parameters of the second calcination include: temperature of 1200° C. to 1300° C. and time of 2 h to 4 h.

[0016] Optionally, the chemical composition of the aluminum hydroxide includes: Na2O, and the content of Na2O is ≤0.2wt%.

[0017] Optionally, the mineralizer includes at least one of the following: boric acid, magnesium oxide, and calcium oxide.

[0018] Optionally, the specific surface area of ​​the γ-alumina is 100 m 2 / g or above.

[0019] In a second aspect, the present application provides an α-type alumina prepared by the method described in any embodiment of the first aspect, wherein the α-type alumina meets the following indicators: D50 is 0.4 μm to 0.6 μm, the content of Na2O is ≤0.02 wt%, and the specific surface area is 3 m 2 / g~5m 2 / g.

[0020] In a second aspect, the present application provides a high molecular polymer membrane, the raw material components of the high molecular polymer membrane include the α-type aluminum oxide described in any one embodiment of the second aspect.

[0021] In a fourth aspect, the present application provides a lithium battery, comprising the high molecular polymer separator described in any one embodiment of the third aspect.

[0022] The above technical solution provided by the embodiment of the present application has the following advantages compared with the prior art:

[0023] The preparation method of the α-type alumina provided in an embodiment of the present application comprises: grinding aluminum hydroxide to obtain aluminum hydroxide powder with a set particle size; performing a first calcination on the aluminum hydroxide powder to obtain γ-alumina; slurrying the γ-alumina to obtain a γ-alumina slurry; introducing CO2 gas into the γ-alumina slurry to achieve a first de-sodiumization of the γ-alumina; mixing the γ-alumina after the first de-sodiumization with a mineralizer, and then performing a second calcination to obtain a first α-type alumina; washing the α-type alumina to achieve a second de-sodiumization of the first α-type alumina to obtain the target α-type alumina. Aluminum hydroxide is ground into aluminum hydroxide powder with a set particle size, so that the aluminum hydroxide powder will not form over-grinding agglomerates, thereby avoiding the occurrence of water loss and splashing of low-temperature aluminum hydroxide during the subsequent calcination process; the aluminum hydroxide powder is subjected to the first calcination to obtain γ alumina with a large specific surface area, so that the sodium oxide in the γ alumina is fully exposed to the surface, thereby facilitating the subsequent sodium removal; the acidic gas CO2 is passed through the γ alumina slurry, and the sodium oxide on the surface of the γ alumina reacts chemically with CO2 to form sodium carbonate soluble in water, so as to achieve the first sodium removal of the γ alumina; the mineralizer can regulate the original crystals of the target α alumina and make it spherical. The γ alumina after the first sodium removal is mixed with the mineralizer and then subjected to the second calcination, which can convert the γ alumina into stable α alumina. While the grains grow fully, the sodium oxide is further exposed to the surface of the α alumina. The soluble sodium oxide attached to the surface of the α alumina is removed by washing, so that the sodium oxide impurity content in the second calcined α alumina is further reduced, thereby achieving the second sodium removal of the α alumina. In summary, the method of reducing the Na2O content in α-alumina. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] The accompanying drawings, which are incorporated in and constitute a part of this specification, illustrate embodiments consistent with the present application and, together with the description, serve to explain the principles of the present application.

[0025] In order to more clearly illustrate the embodiments of the present application or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, for ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative labor.

[0026] Figure 1 A schematic diagram of a process for preparing α-alumina provided in an embodiment of the present application;

[0027] Figure 2 A scanning electron microscope image of an α-alumina provided in an embodiment of the present application;

[0028] Figure 3This is a particle size distribution diagram of α-type aluminum oxide provided in an embodiment of the present application. DETAILED DESCRIPTION

[0029] In order to make the purpose, technical solution and advantages of the embodiments of the present application clearer, the technical solution in the embodiments of the present application will be clearly and completely described below in conjunction with the drawings in the embodiments of the present application. Obviously, the described embodiments are part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of this application.

[0030] Various embodiments of the present application may be presented in the form of a range; it should be understood that the description in the form of a range is only for convenience and brevity, and should not be understood as a rigid limitation on the scope of the present application; therefore, the range description should be considered to have specifically disclosed all possible sub-ranges and single numerical values ​​within the range. For example, the range description from 1 to 6 should be considered to have specifically disclosed sub-ranges, such as from 1 to 3, from 1 to 4, from 1 to 5, from 2 to 4, from 2 to 6, from 3 to 6, etc., as well as single numbers within the range, such as 1, 2, 3, 4, 5 and 6, which apply regardless of the range. In addition, whenever a numerical range is indicated herein, it is meant to include any cited number (fractional or integer) within the indicated range.

[0031] In the present application, in the absence of any contrary description, the directional words used, such as "upper" and "lower", are specifically the directions of the drawings in the accompanying drawings. In addition, in the description of the present specification, the terms "including", "comprising", etc. refer to "including but not limited to". In this article, relational terms such as "first" and "second" are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply that there is any such actual relationship or order between these entities or operations. In this article, "and / or" describes the association relationship of the associated objects, indicating that there may be three relationships, for example, A and / or B, which can represent: A exists alone, A and B exist at the same time, and B exists alone. Wherein A, B can be singular or plural. In this article, "at least one" refers to one or more, and "plural" refers to two or more. "At least one", "at least one of the following" or similar expressions refer to any combination of these items, including any combination of singular or plural items. For example, "at least one of a, b, or c", or "at least one of a, b and c", can both mean: a, b, c, ab (i.e. a and b), ac, bc or abc, where a, b, c can be single or plural, respectively.

[0032] Unless otherwise specified, various raw materials, reagents, instruments and equipment used in this application can be purchased from the market or prepared by existing methods.

[0033] In a first aspect, the present application provides a method for preparing α-alumina. Figure 1 A method for implementing the present application

[0034] kind

[0035] Schematic diagram of the process for preparing α-alumina; see Figure 1 , the method comprising:

[0036] S1, grinding aluminum hydroxide to obtain aluminum hydroxide powder with a set particle size;

[0037] In some embodiments, the chemical composition of the aluminum hydroxide includes: Na2O, the content of Na2O is

[0038] ≤0.2wt%.

[0039] In the embodiment of the present application, the content of Na2O in the chemical composition of aluminum hydroxide can be ≤0.2wt%, which can better reduce the content of sodium oxide in the post-treatment process of sodium removal. Exemplarily, the content of Na2O can be 0.2wt%, 0.18wt%, 0.15wt%, 0.13wt%, etc. The aluminum hydroxide can be prepared by a carbon fractionation process, and the particles are agglomerates and are easy to grind. Please refer to the chemical composition and particle size of aluminum hydroxide shown in Table 1.

[0040] Table 1 Chemical composition (wt%) and particle size of aluminum hydroxide

[0041] <![CDATA[Fe2O3%]]> <![CDATA[Na2O%]]> <![CDATA[SiO2%]]> <![CDATA[Na2O(s)%]]> D50,μm Moisture% ≤0.010 ≤0.2 ≤0.035 ≤0.01 90-110 ≤8-10

[0042] In some embodiments, the set particle size is 3-5 μm.

[0043] In the embodiment of the present application, aluminum hydroxide is ground into aluminum hydroxide micropowder with a set particle size, so that the aluminum hydroxide micropowder will not have over-grinding agglomerates, thereby avoiding the occurrence of low-temperature aluminum hydroxide dehydration and splashing during the subsequent calcination process. The white aluminum hydroxide is ground to 3μm to 5μm using a vertical mill, and the particle size distribution is concentrated. Exemplarily, the above-mentioned set particle size can be 3μm, 4μm, 5μm, etc.

[0044] S2, calcining the aluminum hydroxide powder for the first time to obtain gamma alumina;

[0045] In some embodiments, the process parameters of the first calcination include: a temperature of 600° C. to 900° C., and a time of 30 min to 60 min.

[0046] In the embodiment of the present application, the temperature of the first calcination can be 600°C to 900°C, and the time of the first calcination can be 30min to 60min, so as to adjust the specific surface area of ​​the aluminum hydroxide powder when it turns to the γ phase. For example, the temperature of the first calcination can be 600°C, 700°C, 800°C, 900°C, etc., and the time of the first calcination can be 30min, 40min, 50min, 60min, etc.

[0047] In some embodiments, the specific surface area of ​​the γ-alumina is 100 m 2 / g or above.

[0048] In the embodiment of the present application, the specific surface area of ​​γ-alumina can be 100 m 2 / g or more, the specific surface area of ​​γ alumina is increased to the maximum extent, which is conducive to the subsequent first sodium removal. For example, the specific surface area of ​​the γ alumina can be 100m 2 / g, 110m 2 / g, 120m 2 / g, 130m 2 / g, 140m 2 / g, 150m 2 / g, etc.

[0049] S3, slurrying the gamma alumina to obtain a gamma alumina slurry;

[0050] S4, introducing CO2 gas into the γ-alumina slurry to achieve a first de-sodiumization of the γ-alumina;

[0051] In some embodiments, the endpoint pH value of the gamma alumina slurry after the CO2 gas is introduced is less than 7.

[0052] In the embodiment of the present application, aluminum hydroxide powder can be dissolved in an acid solution, and CO2 gas is introduced into the γ-alumina slurry to form an acidic γ-alumina slurry, which will not introduce new impurities, and the sodium oxide in the aluminum hydroxide powder is difficult to remove. The aluminum hydroxide powder can be converted into γ-alumina with a large specific area by the first calcination, and the sodium oxide is fully exposed on the particle surface of the γ-alumina, thereby achieving the first sodium removal of the γ-alumina. When the end point pH of the γ-alumina slurry after the introduction of CO2 gas is less than 7, it means that the sodium oxide on the surface of the γ-alumina has reacted completely with the carbon dioxide to form sodium carbonate soluble in water, and the first sodium removal can be achieved. Exemplarily, the end point pH value of the γ-alumina slurry after the introduction of CO2 gas can be 6.5, 6, 5.5, etc. In addition, the solid content of the γ-alumina slurry can be 200g / l to 300g / l. After the end point pH of the γ-alumina slurry after the introduction of CO2 gas is less than 7, the sodium oxide content in the alumina can be reduced to less than 0.05% after washing and drying.

[0053] S5, mixing the γ-alumina after the first sodium removal with a mineralizer, and then performing a second calcination to obtain a first α-alumina;

[0054] S6. Washing the α-type alumina to achieve a second de-sodiumization of the first α-type alumina to obtain target α-type alumina.

[0055] In some embodiments, the process parameters of the second calcination include: a temperature of 1200° C. to 1300° C. and a time of 2 h to 4 h.

[0056] In the embodiment of the present application, the grain growth of the γ alumina after the first sodium removal during the second calcination process is reduced by solid phase mass transfer, and it tends to grow in a spherical shape under the action of the mineralizer, and the particle size distribution is uniform and spherical. The γ alumina after the first sodium removal is mixed with the mineralizer and then calcined for the second time, so that the γ alumina can be converted into a stable α-type alumina, and the grains are fully grown (grain size 0.4μm to 0.6μm), while the sodium oxide is further exposed to the surface of the α-type alumina, and the second sodium removal of the α-type alumina is achieved by the second washing. Therefore, after the second calcination, the soluble sodium oxide attached to the surface of the α-type alumina is removed by washing, so that the sodium oxide impurity content in the second calcined α-type alumina is further reduced, thereby achieving the second sodium removal of the α-type alumina. Exemplarily, the temperature of the above-mentioned second calcination can be 1200℃, 1220℃, 1240℃, 1260℃, 1280℃, 1300℃, etc., and the time of the second calcination can be 2h, 3h, 4h, etc. In addition, the above S6 also includes: filtering and drying, using a drum mill for ultrafine grinding to prepare an α-type alumina finished product.

[0057] In some embodiments, the mineralizer includes at least one of the following: boric acid, magnesium oxide, and calcium oxide.

[0058] In the embodiment of the present application, the mineralizer can regulate the original crystals of the target α-type aluminum oxide and make them spherical. The mineralizer can be one or more of boric acid, magnesium oxide, and calcium oxide.

[0059] In a second aspect, the present application provides an α-type alumina prepared by the method described in any embodiment of the first aspect, wherein the α-type alumina meets the following indicators: D50 is 0.4 μm to 0.6 μm, the content of Na2O is ≤0.02 wt%, and the specific surface area is 3 m 2 / g~5m 2 / g.

[0060] The α-type alumina is realized based on the preparation method of the α-type alumina mentioned above. The specific steps of the preparation method of the α-type alumina can refer to the above-mentioned embodiment. Since the α-type alumina adopts part or all of the technical solutions of the above-mentioned embodiment, it at least has all the beneficial effects brought by the technical solutions of the above-mentioned embodiment, which will not be described one by one here.

[0061] In a second aspect, the present application provides a high molecular polymer membrane, the raw material components of the high molecular polymer membrane include the α-type aluminum oxide described in any one embodiment of the second aspect.

[0062] The high molecular polymer diaphragm is realized based on the above-mentioned α-type alumina. The specific indicators of the α-type alumina can refer to the above-mentioned embodiments. Since the high molecular polymer diaphragm adopts part or all of the technical solutions of the above-mentioned embodiments, it has at least all the beneficial effects brought by the technical solutions of the above-mentioned embodiments, which will not be described one by one here.

[0063] In a fourth aspect, the present application provides a lithium battery, comprising the high molecular polymer separator described in any one embodiment of the third aspect.

[0064] In the embodiment of the present application, the lithium-ion battery is composed of positive and negative electrode materials, an electrolyte, a diaphragm and a battery casing. As one of the important components of the battery, the diaphragm can block the contact between the positive and negative electrodes to prevent short circuits, while allowing lithium ions to conduct between the electrodes. The performance of the diaphragm determines the safety of the battery, and a diaphragm with excellent performance plays an important role in improving the comprehensive performance of the battery. The polyethylene or polypropylene diaphragm prepared by coating the α-type alumina material provided in the embodiment of the present application has the advantages of high mechanical strength, stable pore structure and low cost, and can effectively improve the mechanical properties and safety performance of the battery.

[0065] The lithium battery is realized based on the above-mentioned high molecular polymer membrane. The main raw material components of the high molecular polymer membrane can refer to the above-mentioned embodiments. Since the lithium battery adopts part or all of the technical solutions of the above-mentioned embodiments, it has at least all the beneficial effects brought by the technical solutions of the above-mentioned embodiments, which will not be described one by one here.

[0066] The present application will be further described below in conjunction with specific embodiments. It should be understood that these embodiments are intended only to illustrate the present application and are not intended to limit the scope of the present application. The experimental methods for which specific conditions are not specified in the following examples are usually measured according to national standards. If there is no corresponding national standard, then the conditions recommended by the manufacturer are followed.

[0067] Example 1

[0068] A method for preparing α-type alumina comprises: grinding white aluminum hydroxide with a Na2O content of 0.2 wt% by using a vertical mill to obtain aluminum hydroxide powder with a size of 3 μm to 5 μm; calcining the aluminum hydroxide powder for the first time at a temperature of 700°C for 40 minutes to obtain aluminum hydroxide with a specific surface area of ​​200 m 2 / g of gamma alumina; pulping the gamma alumina to obtain a gamma alumina slurry with a solid content of 250g / l; introducing CO2 gas into the gamma alumina slurry to a pH value of 6.5 to achieve a first de-sodiumization of the gamma alumina, followed by a first water washing and drying to reduce the sodium oxide content in the alumina to 0.04%; mixing the gamma alumina after the first de-sodiumization with a mineralizer, and then performing a second calcination at a temperature of 1200°C for 2h to obtain a first alpha alumina; pulping the first alpha alumina, performing a second water washing to achieve a second de-sodiumization of the first alpha alumina, followed by filtering and drying, and using a drum mill for ultrafine grinding to prepare an alpha alumina finished product.

[0069] Example 2

[0070] A method for preparing α-type alumina comprises: grinding white aluminum hydroxide with a Na2O content of 0.2 wt% by using a vertical mill to obtain aluminum hydroxide powder with a size of 3 μm to 5 μm; calcining the aluminum hydroxide powder for the first time at a temperature of 600°C for 60 minutes to obtain a specific surface area of ​​180 m 2 / g of gamma alumina; pulping the gamma alumina to obtain a gamma alumina slurry with a solid content of 250g / l; introducing CO2 gas into the gamma alumina slurry to a pH value of 6.5 to achieve the first de-sodiumization of the gamma alumina, followed by the first water washing and drying, and the sodium oxide content in the alumina is reduced to 0.043%; mixing the gamma alumina after the first de-sodiumization with a mineralizer, and then calcining for a second time at a temperature of 1300°C for 2h to obtain alpha alumina; pulping the alpha alumina, washing it for a second time to achieve the second de-sodiumization of the alpha alumina, filtering and drying, and using a drum mill for ultrafine grinding to prepare an alpha alumina finished product.

[0071] Example 3

[0072] A method for preparing α-alumina comprises: grinding white aluminum hydroxide with a Na2O content of 0.2 wt% by using a vertical mill to obtain aluminum hydroxide powder with a size of 3 μm to 5 μm; calcining the aluminum hydroxide powder for the first time at a temperature of 800°C for 60 minutes to obtain a specific surface area of ​​120 m 2 / g of gamma alumina; pulping the gamma alumina to obtain a gamma alumina slurry with a solid content of 250g / l; introducing CO2 gas into the gamma alumina slurry to a pH value of 6.5 to achieve the first de-sodiumization of the gamma alumina, followed by the first water washing and drying to reduce the sodium oxide content in the alumina to 0.045%; mixing the gamma alumina after the first de-sodiumization with a mineralizer, and then calcining for a second time at a temperature of 1300°C for 2h to obtain alpha alumina; pulping the alpha alumina, washing it for a second time to achieve the second de-sodiumization of the alpha alumina, filtering and drying it, and using a drum mill for ultrafine grinding to prepare an alpha alumina finished product.

[0073] Example 4

[0074] A method for preparing α-type alumina comprises: grinding white aluminum hydroxide with a Na2O content of 0.2 wt% by using a vertical mill to obtain aluminum hydroxide powder with a size of 3 μm to 5 μm; calcining the aluminum hydroxide powder for the first time at a temperature of 900°C for 60 minutes to obtain a specific surface area of ​​80 m 2 / g of gamma alumina; pulping the gamma alumina to obtain a gamma alumina slurry with a solid content of 250g / l; introducing CO2 gas into the gamma alumina slurry to a pH value of 6.5 to achieve the first de-sodiumization of the gamma alumina, followed by the first water washing and drying, and the sodium oxide content in the alumina is reduced to 0.048%; mixing the gamma alumina after the first de-sodiumization with a mineralizer, and then calcining for a second time at a temperature of 1300°C for 2h to obtain alpha alumina; pulping the alpha alumina, washing it for a second time to achieve the second de-sodiumization of the alpha alumina, filtering and drying it, and using a drum mill for ultrafine grinding to prepare an alpha alumina finished product.

[0075] Comparative Example 1

[0076] A method for preparing α-alumina comprises: grinding white aluminum hydroxide with a Na2O content of 0.2 wt% by using a vertical mill to obtain aluminum hydroxide powder with a size of 3 μm to 5 μm; calcining the aluminum hydroxide powder for the first time at a temperature of 800°C for 60 minutes to obtain a specific surface area of ​​120 m 2 / g of gamma alumina; slurrying the gamma alumina to obtain a gamma alumina slurry with a solid content of 250g / l; introducing CO2 gas into the gamma alumina slurry to a pH value of 6.5 to achieve the first de-sodiumization of the gamma alumina, followed by the first water washing and drying to reduce the sodium oxide content in the alumina to 0.048%; mixing the gamma alumina after the first de-sodiumization with a mineralizer, and then calcining for a second time at a temperature of 1300°C for 2h, and ultrafine grinding using a drum mill to obtain alpha alumina.

[0077] Comparative Example 2

[0078] A preparation method of alpha alumina comprises: grinding white aluminum hydroxide with a Na2O content of 0.2 wt% by using a vertical mill to obtain aluminum hydroxide micropowder of 3 μm to 5 μm; mixing the aluminum hydroxide micropowder with a mineralizer and calcining the mixture at a temperature of 1300°C for 2 hours, and ultrafine grinding the mixture with a drum mill to obtain alpha alumina.

[0079] The α-alumina products obtained in Examples 1 to 4 and Comparative Examples 1 to 2 were tested for various indicators. Please see Table 2 for the results.

[0080] Table 2 Index of α-type alumina finished products

[0081] Serial number D50,μm <![CDATA[Na2O / wt%]]> <![CDATA[Specific surface area m 2 / g <!-- 6 -->]]> Example 1 0.436 0.017 4.2 Example 2 0.443 0.017 4.3 Example 3 0.452 0.018 4.2 Example 4 0.448 0.018 4.4 Comparative Example 1 0.458 0.042 4.5 Comparative Example 2 0.685 0.271 2.5

[0082] From Table 2, it can be seen that after two calcinations and two sodium removals, the sodium oxide content in the alumina product can be reduced to below 0.02%, and the original crystal D50 is between 0.4-0.6 μm. Figure 2This is a scanning electron microscope image of an α-type aluminum oxide provided in the embodiment of the present application; see Figure 2 It can be seen that the grains of the α-type alumina finished product provided in the embodiment of the present application are all spherical, and the grain size is uniform, without large-sized grains; Figure 3 This is a particle size distribution diagram of α-alumina provided in the embodiment of the present application; please refer to Figure 3 It can be seen that the median particle size D50 of the α-type alumina product provided in the embodiment of the present application is between 0.4 μm and 0.6 μm, and D99≤2 μm, which meets the particle size index requirements of lithium battery separator coating.

[0083] One or more technical solutions in the embodiments of the present application also have at least the following technical effects or advantages:

[0084] (1) After the first roasting of aluminum hydroxide, CO2 gas is introduced for the first sodium removal, which does not introduce new impurities; after low-temperature calcination, the second washing and second sodium removal wash away the soluble sodium oxide attached to the surface, making the sodium oxide impurity content in the calcined α-alumina lower;

[0085] (2) Aluminum hydroxide micropowder with uniform particle size distribution is prepared by grinding aluminum hydroxide. During the calcination process, the solid phase mass transfer is reduced due to grain growth, and the particles tend to grow in a spherical shape under the action of a mineralizer, and the particle size distribution is uniform and spherical;

[0086] (3) Using white aluminum hydroxide as raw material, after the first calcination and CO2 de-sodiumization, the second calcination and water washing de-sodiumization, the sodium oxide in the α-alumina product is reduced to less than 0.02%, the main content of alumina reaches more than 99.9%, the median particle size of the finished product is 0.4μm to 0.6μm, and the morphology is spherical;

[0087] (4) The preparation method of α-alumina is simple and easy to operate, which has a great promoting effect on improving the quality of the finished product. The prepared finished product has a concentrated particle size distribution and a low impurity content, which can meet the application needs of the lithium battery diaphragm coating industry.

[0088] The above description is only a specific implementation of the present application, so that those skilled in the art can understand or implement the present application. Various modifications to these embodiments will be apparent to those skilled in the art, and the general principles defined herein can be implemented in other embodiments without departing from the spirit or scope of the present application. Therefore, the present application will not be limited to the embodiments shown herein, but will conform to the widest range consistent with the principles and novel features applied for herein.

Claims

1. A method for preparing α-alumina, characterized in that: The method comprises: Grinding aluminum hydroxide to obtain aluminum hydroxide micropowder with a set particle size; The aluminum hydroxide powder is first calcined to obtain gamma alumina; Slurrying the gamma alumina to obtain a gamma alumina slurry; Introducing CO2 gas into the gamma alumina slurry to achieve a first de-sodiumization of the gamma alumina; The gamma alumina after the first sodium removal is mixed with a mineralizer, and then subjected to a second calcination to obtain a first alpha alumina; The α-type alumina is washed to achieve a second de-sodiumization of the first α-type alumina to obtain the target α-type alumina.

2. The method according to claim 1, characterized in that: The set particle size is 3-5 μm.

3. The method according to claim 1, characterized in that: The endpoint pH value of the gamma alumina slurry after the CO2 gas is introduced is less than 7.

4. The method according to claim 1, characterized in that: The process parameters of the first calcination include: a temperature of 600° C. to 900° C. and a time of 30 min to 60 min; and / or, The process parameters of the second calcination include: temperature of 1200° C. to 1300° C. and time of 2 h to 4 h.

5. The method according to claim 1, characterized in that: The chemical composition of the aluminum hydroxide includes: Na2O, and the content of Na2O is ≤0.2wt%.

6. The method according to claim 1, characterized in that: The mineralizer includes at least one of the following: boric acid, magnesium oxide, and calcium oxide.

7. The method according to claim 1, characterized in that: The specific surface area of ​​the γ-alumina is 100 m 2 / g or above.

8. An α-alumina according to any one of claims 1 to 7, characterized in that: The α-alumina meets the following indicators: D50 is 0.4 μm to 0.6 μm, the content of Na2O is ≤ 0.02 wt%, and the specific surface area is 3 m 2 / g~5m 2 / g.

9. A high molecular polymer membrane, characterized in that: The raw material component of the high molecular polymer separator includes the α-alumina described in claim 8.

10. A lithium battery, characterized in that: The lithium battery comprises the high molecular polymer separator according to claim 9.

Citation Information

Cited By

  • Adsorption and removal of bacteria from oral cavities and from the skin of infected humans and animals