Method for recycling clear liquid
By controlling the alkali content and ammonia content of the reactor bottom liquid during the preparation of the lithium battery positive electrode material precursor, and recycling and utilization of the clean liquid, the problem of waste of water resources and environmental pressure in the preparation of the lithium battery positive electrode material precursor is solved. The effect of saving water resources and reducing emissions has been achieved.
Patent Information
- Application Number
- CN202411578236.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-11-07
- Publication Date
- 2024-12-06
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The ammonia-containing aqueous solution produced during the preparation of the precursor of the lithium battery positive electrode material is discharged in large quantities, resulting in waste of water resources and increased environmental protection pressure, making it difficult for the existing technology to effectively recycle and utilize.
During the preparation of the positive electrode material precursor, the alkali content and ammonia content of the reactor base liquid are controlled, and the ammonia content is gradually increased, and the concentrated discharge liquid is refluxed to the next reactor as the starting base liquid after the reaction is completed, reducing The amount of pure water, ammonia and alkali liquid is used to realize the recycling of the extract liquid.
On the premise of ensuring the quality of the precursor, the amount of water treatment and external emissions are reduced, the waste of water resources and environmental protection pressure are reduced, and the energy and environmental protection benefits are high.
Smart Images

Figure CN119080086A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of manufacturing positive electrode materials for lithium ion batteries, and in particular to a method for recycling clear liquid. Background Art
[0002] With the rapid development of new energy vehicles, energy storage devices, smart homes and other markets, especially the rapid popularization of new energy electric vehicles, battery materials, as the most important component of key parameters of battery performance, have received extensive attention. Lithium battery positive electrode materials are one of the most important battery materials, and their market size and development trends have also attracted much attention. The output of precursors for preparing lithium battery positive electrode materials has also increased significantly to meet market demand.
[0003] During the preparation process of the precursor of the positive electrode material, a large amount of aqueous solution containing ammonia and alkaline water will be produced, which will usually be transferred to the factory water treatment process for centralized treatment and discharged after passing the water treatment process. As the output of the precursor increases, the amount of such aqueous solution that needs to be treated is also increasing day by day, resulting in huge waste of water resources and environmental pressure. Summary of the invention
[0004] In order to overcome the shortcomings of the prior art, the present invention combines the precursor process and production equipment, and under the premise of ensuring the quality of the positive electrode material precursor, recycles the clear liquid generated in the intermittent precursor production method, saves the pure water, ammonia alkali and other raw materials required to start the reaction, reduces the amount of clear liquid discharged to the outside, and reduces the amount of steam consumed in ammonia evaporation, reduces the amount of water treatment in the later stage, reduces the waste of water resources and environmental pressure, and has higher energy and environmental benefits.
[0005] In order to achieve the above-mentioned purpose, the present invention provides the following technical solutions: a method for recycling the clear liquid, when the positive electrode material precursor is prepared, the reactor 1 is prepared with a bottom pot and started, and after the nucleation is completed, the alkali content of the bottom liquid is controlled to be stable, and the ammonia content is gradually increased to control the normal growth of the precursor; after the reaction is started, after the reaction liquid in the reactor 1 flows out, the material is concentrated, and the concentrated material is returned to the reactor 1 to continue the reaction, and the concentrated clear liquid is discharged to a storage tank for storage. When the reactor 2 needs to be started, the stored clear liquid is pumped into the reactor 2 as a reaction bottom liquid through a power pump, and the start-up reaction is carried out according to the start-up method of the reactor 1; by utilizing the reaction liquid in the preparation process, the use of pure water, ammonia liquid, and alkali liquid for starting the reactor is reduced; at the same time, the discharge of ammonia-alkali wastewater in the workshop is reduced.
[0006] Furthermore, the specific steps are as follows: (1) Prepare a ternary or binary mixed salt solution of nickel, cobalt and manganese as required, with a concentration of 0.5-2.3 mol / L; prepare a 2-8 mol / L alkaline solution; prepare a 2.0-6.0 mol / L ammonia solution; (2) In reactor 1, prepare a bottom liquid with a pH of 11.5-13.5 and an ammonia content of 1-25 g / L, which accounts for 40%-90% of the reactor volume, and introduce protective gas. At a speed of 400-800 r / min and a temperature of 40-70°C, pump the mixed liquid, alkali solution, and ammonia solution into reactor 1 through a metering pump to carry out a crystallization reaction. Stop the line after the precursor reaction is completed; (3) During the crystallization reaction process, the reactor slurry flows to the middle tank through the overflow pipe, and the material is pumped into the concentrator for concentration by a power pump. The concentrated material is returned to the reactor to continue the reaction, and the separated clear liquid is pumped into the storage tank for standby use, and is used as the bottom liquid of the next reactor 2 to start the line; (4) When the reactor 2 needs to be started, the collected and stored clear liquid is pumped into the reactor 2, and ammonia and alkali are added at a rate of 0.1-1.0 times the ammonia and alkali flow rate. The nucleation time is 1-5 times that of the normal process. After that, the reaction is carried out according to the same process method as the reactor 1, and the reaction clear liquid is collected in the storage tank and retained for standby; (5) After the crystallization reaction is completed, washing; (6) After dehydration and drying, the product is circulated according to the drying process, and the magnetic packaging is removed by screening to obtain a ternary or binary hydroxide precursor.
[0007] Furthermore, the crystallization reaction process is an intermittent production reaction process with concentration and solidification.
[0008] Furthermore, the clear liquid from the concentration and solidification process is colorless, transparent and clear, and there is no nickel loss during the reaction process.
[0009] Furthermore, the bottom pot of the reactor 2 is prepared by adding ammonia liquid at a flow rate of 0.1-1 times the inherent flow rate, and adding alkali liquid at a flow rate of 0.1-1 times the inherent flow rate.
[0010] Furthermore, the reaction process is stabilized by controlling the high alkali content, and the material size is controlled by controlling the ammonia content.
[0011] Furthermore, the washing in step (5) is carried out according to the alkaline water concentration, temperature and deionization temperature of the conventional process, which can reduce the amount of alkaline washing and the amount of deionized water washing while maintaining stable indicators. Beneficial Effects
[0012] The present invention provides a method for recycling clear liquid. In the intermittent preparation method of positive electrode material precursor, by adjusting the precursor nucleation control method, the clear liquid of the reaction process is directly recovered and formulated into the starting bottom liquid of the next reactor. The index performance of the prepared precursor is the same as that of the conventional method. At the same time, the discharge of the reaction clear liquid and the amount of environmental water treatment are reduced, and the use of pure water is saved, which has good economic and environmental benefits. BRIEF DESCRIPTION OF THE DRAWINGS
[0013] Figure 1 It is a schematic diagram of the process of the present invention; Figure 2 It is a comparison between the SEM of the product prepared in Example 1 of the present invention (the picture on the right) and the SEM of the product prepared by the conventional method (the picture on the left).
[0014] Figure 3 It is a comparison between the SEM of the product prepared in Example 3 of the present invention (the picture on the right) and the SEM of the product prepared by the conventional method (the picture on the right). DETAILED DESCRIPTION
[0015] The present invention will be further described below in conjunction with embodiments. Example 1
[0016] (1) Nickel sulfate, cobalt sulfate and manganese sulfate were weighed according to a molar ratio of 65:15:20, and then dissolved in deionized water to prepare a mixed solution A with a concentration of 2.1 mol / L, and the test flow rate was 5.5 L / min. A sodium hydroxide solution with a concentration of 8 mol / L was prepared as solution B, and the test flow rate was 3.0 L / min. An ammonia solution with a concentration of 4 mol / L was prepared as solution C, and the test flow rate was 0.25 L / min; (2) Prepare 70% of the bottom liquid with a pH of 13.20 and an ammonia content of 4.5g / L in reactor 1. The bottom liquid temperature is controlled at 60°C, nitrogen protective gas is introduced, and the stirring speed is turned on at 700r / min. Solutions A, B, and C are added to the reactor simultaneously through metering pumps, with flow rates of 5.5L / min, 3.0L / min, and 0.25L / min, respectively. According to the product process, the pH is controlled at 12.40±0.05, the ammonia content is 4.2±0.5g / L, and the temperature in the reactor is 60±1°C; after the overflow of the material, it is concentrated by a concentrator, and the material is refluxed to the reactor to continue the reaction, and the clear liquid is collected and stored in a storage tank. After the reaction is completed for 60 hours, the normal downstream process flows; (3) The collected mother liquor was pumped into reactor 2, and the ammonia and alkali content in the clear liquid was tested. Ammonia and alkali liquid were added according to the deviation between the specific content and the requirement, so that the solution pH reached 13.20 and the ammonia content was 4.5 g / L. The alkali liquid was added at a flow rate of 1.0 L / min and the ammonia liquid was added at a flow rate of 0.25 L / min.
[0017] (4) The temperature of the reactor is controlled at 60°C, nitrogen protective gas is introduced, and the stirring speed is turned on at 700r / min. Solutions A, B, and C are added to the reactor simultaneously through metering pumps, with flow rates of 5.5L / min, 3.0L / min, and 0.25L / min, respectively. According to the product process, the pH is controlled at 12.40±0.05, the ammonia content is 4.2±0.5g / L, and the temperature in the reactor is 60±1°C; after the overflow of the material, it is concentrated by a concentrator, and the material is refluxed to the reactor to continue the reaction, and the clear liquid is collected and stored in a storage tank. After the reaction is completed for 60 hours, the subsequent process flows normally; Step (1) and step (2) in Example 1 are combined to form a conventional method. Figure 2 The SEM of the product prepared in Example 1 of the present invention (the right picture) is compared with the SEM of the product prepared by the conventional method (the left picture). As can be seen from the figure, the morphology and index of the product produced by the present invention are the same as those of the conventional product, but the mother liquor produced in the production process can be greatly reduced, the waste water discharged from the workshop can be reduced, and pure water and ammonia alkali raw materials can be saved, and the pressure of water treatment in the environmental protection zone can be reduced, which has high economic and environmental benefits. Example 2
[0018] (1) Nickel sulfate, cobalt sulfate and manganese sulfate were weighed in a molar ratio of 55:20:25, and then dissolved in deionized water to prepare a mixed solution A with a concentration of 2.1 mol / L, and the test flow rate was 7.0 L / min. A sodium hydroxide solution with a concentration of 8 mol / L was prepared as solution B, and the test flow rate was 3.80 L / min. An ammonia solution with a concentration of 4 mol / L was prepared as solution C, and the test flow rate was 0.10 L / min; (2) Prepare 70% of the bottom liquid with a pH of 12.50 and an ammonia content of 1.8 g / L in reactor 1. The bottom liquid temperature is controlled at 50°C, nitrogen protective gas is introduced, and the stirring speed is turned on at 750 r / min. Solutions A, B, and C are added to the reactor simultaneously through metering pumps, with flow rates of 7.0 L / min, 3.8 L / min, and 0.1 L / min, respectively. According to the product process, the pH is controlled at 12.05±0.05, the ammonia content is 3.0±0.5 g / L, and the temperature in the reactor is 50±1°C; after the overflow of the material, it is concentrated by a concentrator, and the material is refluxed to the reactor to continue the reaction, and the clear liquid is collected and stored in a storage tank. After the reaction is completed for 115 hours, the normal downstream process flows; (3) The collected mother liquor was pumped into reactor 2, and the ammonia and alkali content in the clear liquid was tested. Ammonia and alkali liquid were added according to the deviation between the specific content and the requirement, so that the solution pH reached 12.50 and the ammonia content was 1.8 g / L. The alkali liquid was added at a flow rate of 3.8 L / min and the ammonia liquid was added at a flow rate of 0.1 L / min.
[0019] (4) The temperature of the reactor is controlled at 50°C, nitrogen protective gas is introduced, and the stirring speed is turned on at 750r / min. Solutions A, B, and C are added to the reactor simultaneously through metering pumps, with flow rates of 7.0L / min, 3.8L / min, and 0.1L / min, respectively. According to the product process, the pH is controlled at 12.05±0.05, the ammonia content is 3.0±0.5g / L, and the temperature in the reactor is 50±1°C; after the overflow of the material, it is concentrated by a concentrator, and the material is refluxed to the reactor to continue the reaction, and the clear liquid is collected and stored in a storage tank. After the reaction is completed for 115 hours, the subsequent process flows normally; Example 3
[0020] (1) Nickel sulfate, cobalt sulfate and manganese sulfate were weighed according to a molar ratio of 80:05:15, and then dissolved in deionized water to prepare a mixed solution A with a concentration of 2.1 mol / L, and the test flow rate was 10.0 L / min. A sodium hydroxide solution with a concentration of 8 mol / L was prepared as solution B, and the test flow rate was 5.6 L / min. An ammonia solution with a concentration of 4 mol / L was prepared as solution C, and the test flow rate was 0.8 L / min; (2) Prepare 70% of the bottom liquid with a pH of 13.20 and an ammonia content of 6.8g / L in reactor 1. The bottom liquid temperature is controlled at 45°C, nitrogen protective gas is introduced, and the stirring speed is turned on at 800r / min. Solutions A, B, and C are added to the reactor simultaneously through metering pumps, with flow rates of 10.0L / min, 5.6L / min, and 0.8L / min, respectively. The process is controlled at pH 12.8±0.05, ammonia content 6.8±0.5g / L, and the temperature in the reactor at 45±1°C according to the product process; after the material overflows, it is concentrated by a concentrator, and the material is refluxed to the reactor to continue the reaction, and the clear liquid is collected and stored in a storage tank. After the reaction is completed for 55 hours, the subsequent process flows normally; (3) The collected mother liquor was pumped into reactor 2, and the ammonia and alkali content in the clear liquid was tested. Ammonia and alkali liquid were added according to the deviation between the specific content and the requirement, so that the solution pH reached 13.20 and the ammonia content was 6.8 g / L. The alkali liquid was added at a flow rate of 2.8 L / min, and the ammonia liquid was added at a flow rate of 0.4 L / min.
[0021] (4) The temperature of the reactor is controlled at 45°C, nitrogen protective gas is introduced, and the stirring speed is turned on at 800r / min. Solutions A, B, and C are added to the reactor simultaneously through metering pumps, with flow rates of 10.0L / min, 5.6L / min, and 0.8L / min, respectively. According to the product process, the pH is controlled at 12.8±0.05, the ammonia content is 6.8±0.5g / L, and the temperature in the reactor is 45±1°C; after the overflow of the material, it is concentrated by a concentrator, and the material is refluxed to the reactor to continue the reaction, and the clear liquid is collected in a storage tank for storage. After the reaction is completed for 55 hours, it flows normally to the next process; Step (1) and step (2) in Example 3 are combined to form a conventional method. Figure 3 The SEM of the product prepared in Example 3 of the present invention (the right picture) is compared with the SEM of the product prepared by the conventional method (the right picture). As can be seen from the figure, the morphology and indexes of the product produced by the present invention are the same as those of the conventional product, but the mother liquor produced in the production process can be greatly reduced, the waste water discharged from the workshop can be reduced, and pure water and ammonia alkali raw materials can be saved, and the pressure of water treatment in the environmental protection zone can be reduced, which has high economic and environmental benefits.
Claims
1. A method for recycling a clear liquid, characterized in that: During the preparation of the cathode material precursor, the reactor 1 is started by preparing the bottom pot. After the nucleation is completed, the alkali content of the bottom liquid is controlled to be stable, and the ammonia content is gradually increased to control the normal growth of the precursor. After the reaction is started, after the reaction liquid in the reactor 1 flows out, the material is concentrated, and the concentrated material is returned to the reactor 1 to continue the reaction. The concentrated clear liquid is discharged into the storage tank for storage. When the reactor 2 needs to be started, the stored clear liquid is pumped into the reactor 2 as the reaction bottom liquid through a power pump, and the start-up reaction is carried out according to the start-up method of the reactor 1. The reaction liquid in the preparation process is used to reduce the use of pure water, ammonia liquid and alkali liquid for the reactor startup; at the same time, the discharge of ammonia-alkali wastewater in the workshop is reduced.
2. A method for recycling clear liquid according to claim 1, characterized in that: The specific steps are as follows: (1) Prepare a ternary or binary mixed salt solution of nickel, cobalt and manganese as required, with a concentration of 0.5-2.3 mol / L; prepare a 2-8 mol / L alkaline solution; prepare a 2.0-6.0 mol / L ammonia solution; (2) In reactor 1, prepare a bottom liquid with a pH of 11.5-13.5 and an ammonia content of 1-25 g / L, which accounts for 40%-90% of the reactor volume, and introduce protective gas. At a speed of 400-800 r / min and a temperature of 40-70°C, pump the mixed liquid, alkali solution, and ammonia solution into reactor 1 through a metering pump to carry out a crystallization reaction. Stop the line after the precursor reaction is completed; (3) During the crystallization reaction process, the reactor slurry flows to the middle tank through the overflow pipe, and the material is pumped into the concentrator for concentration by a power pump. The concentrated material is returned to the reactor to continue the reaction, and the separated clear liquid is pumped into the storage tank for standby use, and is used as the bottom liquid of the next reactor 2 to start the line; (4) When the reactor 2 needs to be started, the collected and stored clear liquid is pumped into the reactor 2, and ammonia and alkali are added at a rate of 0.1-1.0 times the ammonia and alkali flow rate. The nucleation time is 1-5 times that of the normal process. After that, the reaction is carried out according to the same process method as the reactor 1, and the reaction clear liquid is collected in the storage tank and retained for standby; (5) After the crystallization reaction is completed, washing; (6) After dehydration and drying, the product is circulated according to the drying process, and the magnetic packaging is removed by screening to obtain a ternary or binary hydroxide precursor.
3. The method for recycling the clear liquid according to claim 2, characterized in that: The crystallization reaction process is an intermittent production reaction process with concentration and solidification.
4. The method for recycling the clear liquid according to claim 3, characterized in that: The clear liquid from the concentration and solidification process is colorless, transparent and clear, and there is no nickel loss during the reaction process.
5. The method for recycling the clear liquid according to claim 2, characterized in that: The method for preparing the bottom pot of the reactor 2 is to add ammonia liquid at a flow rate of 0.1-1 times the inherent flow rate, and to add alkali liquid at a flow rate of 0.1-1 times the inherent flow rate.
6. The method for recycling the clear liquid according to claim 2, characterized in that: The reaction process is stabilized by controlling the high alkali content, and the material size is controlled by controlling the ammonia content.
7. The method for recycling the clear liquid according to claim 2, characterized in that: The washing in step (5) is carried out according to the alkaline water concentration, temperature and deionization temperature of the conventional process, which can reduce the amount of alkaline washing and the amount of deionized water washing while maintaining stable indicators.
Citation Information
Patent Citations
Ternary positive electrode material precursor preparation method
CN108529688A
Preparation method for spherical nickel cobalt manganese hydroxide precursor with narrow particle size distribution
CN109860581A
Method for preparing semi-continuous ternary precursor
CN110600683A
Preparation method and application of precursor with good primary particle uniformity
CN111540898A
Ternary precursor and preparation method and application thereof
CN115745020A