Large-dosage phosphogypsum cementing material, curing agent and curing method

By combining large amounts of phosphogypsum, slag and fly ash, low-cost and high-performance gelling materials are prepared, which solves the problems of low utilization rate of phosphogypsum and environmental pollution, and achieves the effect of efficient curing of sludge/soft soil. The compressive strength increases and reduces engineering costs.

CN119080411APending Publication Date: 2024-12-06CENT SOUTH UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411184737.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-27
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

In the prior art, the comprehensive utilization rate of phosphogypsum is low, resulting in environmental pollution and solid waste accumulation problems. The low-dose phosphogypsum gelling material is costly and has insufficient mechanical properties.

Method used

The gelling materials and curing agents are prepared by large-scale phosphogypsum combined with slag and fly ash. The pre-treatment of phosphogypsum by washing and adjusting the proportion of phosphogypsum, slag, fly ash and ripe lime to form low-cost and high-performance gelling Material, used for curing of subgrade materials and sludge/soft soil.

Benefits of technology

The resource utilization of phosphogypsum has been realized, solid waste accumulation and environmental pollution have been reduced, and low-cost and high-performance gelling materials have been provided, which can effectively cure silt or soft soil with high moisture content, compressive strength reaches more than 10MPa, and seepage The filtrate meets the sewage discharge standards.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119080411A_ABST
    Figure CN119080411A_ABST
Patent Text Reader

Abstract

The invention relates to a high-dosage phosphogypsum cementing material, a curing agent and a curing method. The ardealite cementing material is prepared from 45 to 70 parts of ardealite, 16.5 to 35 parts of slag, 3 to 25 parts of fly ash and 0.5 to 2 parts of slaked lime. The curing agent comprises an ardealite cementing material and cement, and the mass ratio of the ardealite cementing material to the cement is 7: 3-3: 7. According to the invention, the cementing material which is low in cost, safe, environment-friendly and excellent in performance is prepared on the basis of high-doping-amount phosphogypsum and industrial solid waste, and when the doping amount of phosphogypsum reaches 60%, the compressive strength of the obtained cementing material can reach 10 MPa or above. And when being used as a curing agent of sludge or soft soil, the curing agent can achieve a better curing effect compared with cement.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of industrial solid waste recycling, and in particular to a high-dosage phosphogypsum cementitious material, a curing agent and a curing method. Background Art

[0002] At present, the discharge of various types of industrial solid waste is growing, especially in the mining, metallurgy, power and other industries. Phosphogypsum, as a common industrial solid waste, generally appears as a by-product in the production process of phosphoric acid. For every ton of phosphoric acid produced, about 5 tons of phosphogypsum are discharged, and the global production of phosphogypsum is estimated to be about 100 million to 280 million tons per year. The current growth of phosphogypsum is estimated to be 200 million tons per year, and the idealized statistical mass utilization rate is 10-15%. At present, the disposal of phosphogypsum is still mainly stockpiling, and the comprehensive utilization rate is low. At the same time, since phosphogypsum contains a large amount of sulfate and other components, its seepage will also cause serious environmental pollution. In order to solve the problem of phosphogypsum accumulation, some scholars have proposed to prepare it as a cementitious material, which is conducive to stacking and can reduce the seepage of harmful components, and further use it as an environmental governance material, such as roadbed materials or silt, soft soil curing agent components, to achieve the effect of resource utilization. However, although phosphogypsum can provide a large amount of sulfate and promote the formation of calcium sulfonite, the proportion of silicon and aluminum elements in it is relatively low. In order to ensure that there is enough silicon oxide and aluminum oxide to participate in the hydration reaction, it is considered to add slag and fly ash with volcanic ash properties into the reaction system. Considering the mechanical properties of phosphogypsum itself, most scholars will use low-dosage phosphogypsum to prepare cementitious materials. When used as a curing agent, a high proportion of cement is added to improve the curing effect, but the addition of cement will lead to a higher cost of this type of cementitious material. Summary of the invention

[0003] One of the purposes of the present invention is to find a new direction for the resource utilization of phosphogypsum, using a large amount of phosphogypsum as a raw material to prepare a cementitious material and a curing agent, and having good mechanical properties.

[0004] The solution adopted by the present invention to solve the above technical problems is:

[0005] A high-dosage phosphogypsum cementitious material, comprising, by weight:

[0006] 45-70 parts of phosphogypsum

[0007] Slag 16.5~35 parts

[0008] 3-25 parts fly ash

[0009] 0.5 to 2 parts of slaked lime.

[0010] Furthermore, the high-dosage phosphogypsum cementitious material is composed of the following components in parts by weight:

[0011] 50-66 parts of phosphogypsum

[0012] 28 parts of slag

[0013] 5-20 parts fly ash

[0014] 1.25 to 2 parts of slaked lime.

[0015] Furthermore, the high-dosage phosphogypsum cementitious material is composed of the following components in parts by weight:

[0016] 50.57 parts of phosphogypsum

[0017] 28 parts of slag

[0018] 20 parts fly ash

[0019] 1.43 parts of slaked lime.

[0020] Furthermore, the high-dosage phosphogypsum cementitious material is composed of the following components in parts by weight:

[0021] 65.75 parts of phosphogypsum

[0022] 28 parts of slag

[0023] 5 parts fly ash

[0024] 1.25 parts of slaked lime.

[0025] Furthermore, the high-dosage phosphogypsum cementitious material is composed of the following components in parts by weight:

[0026] 57.5 parts of phosphogypsum

[0027] 28 parts of slag

[0028] 12.5 parts fly ash

[0029] 2 parts slaked lime.

[0030] Furthermore, the high-dosage phosphogypsum cementitious material is composed of the following components in parts by weight:

[0031] 59 parts of phosphogypsum

[0032] 28 parts of slag

[0033] 12.5 parts fly ash

[0034] 0.5 parts of slaked lime.

[0035] Furthermore, the calcium content of the fly ash does not exceed 10%.

[0036] Furthermore, the phosphogypsum is pretreated, and the pretreatment is mainly used to remove a large amount of impurities in fresh phosphogypsum, and the pretreatment method can be selected as water washing. Furthermore, taking pH as an example, the pretreated phosphogypsum should meet pH ≥ 3.

[0037] The second object of the present invention is to provide a large-dosage phosphogypsum-based curing agent, the curing agent comprises the above-mentioned phosphogypsum cementitious material and cement, wherein the mass ratio of the phosphogypsum cementitious material to the cement is 7:3 to 3:7. Optionally, the mass ratio of the phosphogypsum cementitious material to the cement is 7:3, 6:4, 5:5, 4:6, 3:7.

[0038] The third object of the present invention is to provide a method for solidifying silt / soft soil, which uses the above-mentioned phosphogypsum-based curing agent and mixes it into the silt / soft soil to be solidified to consolidate it.

[0039] Further, the dosage of the phosphogypsum-based curing agent is 15% or more of the dry weight of the sludge / soft soil to be solidified, and further preferably the dosage is 15% to 50% of the dry weight of the sludge / soft soil to be solidified. Optionally, the dosage of the phosphogypsum-based curing agent is 15%, 18%, 20%, 25%, 30%, 35%, 40%, 45%, 50% of the dry weight of the sludge / soft soil to be solidified.

[0040] Furthermore, the water content of the sludge / soft soil to be solidified is not more than 3 times the liquid limit of the sludge / soft soil (the critical water content / amount that changes a substance from a solid state to a liquid state), and is preferably 2 to 3 times the liquid limit of the sludge / soft soil. For example, when the mass of water contained in the sludge / soft soil to be solidified reaches 50% of the dry weight of the sludge / soft soil, the sludge becomes liquid, that is, when the sludge liquid limit is 50%, the sludge water content that can be solidified by the phosphogypsum-based curing agent described in the present application can reach up to 150%.

[0041] Further, the water content of the silt / soft soil to be solidified (i.e., the ratio of the mass of water contained in the silt / soft soil to the dry weight of the silt / soft soil) does not exceed 85%. Preferably, the water content of the silt / soft soil to be solidified is 60% to 85%. Optionally, the water content of the silt / soft soil to be solidified is 60%, 65%, 70%, 75%, 80%, 85%.

[0042] The present invention is based on a large amount of phosphogypsum and industrial solid waste to prepare a new type of road solid waste-based cementitious material with low cost, safety, environmental protection and excellent performance. On the one hand, it can make full use of solid wastes such as phosphogypsum, fly ash, slag, etc. as raw materials, reduce the land occupation and storage of solid waste, and reduce the environmental harm caused by solid waste accumulation. On the other hand, the prepared low-cost, high-performance new type of road solid waste-based cementitious material can replace traditional cement, etc., to reduce engineering costs. When the dosage of phosphogypsum reaches 60%, the compressive strength of the obtained cementitious material itself can reach more than 10MPa. The curing agent described in the present application is particularly suitable for sludge or soft soil with high water content. When used to solidify sludge or soft soil with a water content of 2 to 3 times the liquid limit, it can achieve better curing effect than cement. BRIEF DESCRIPTION OF THE DRAWINGS

[0043] Figure 1 It is the mixed reaction mechanism of phosphogypsum, fly ash, slag, calcium hydroxide and water. DETAILED DESCRIPTION

[0044] For a better understanding of the present invention, the following examples are provided to further illustrate the present invention, but the present invention is not limited to the following examples.

[0045] Ingredients:

[0046] The phosphogypsum used in the present invention is taken from Xifeng mining area in Guiyang City, Guizhou Province, and is pre-treated by a water washing method.

[0047] The fly ash used in the present invention is taken from Longjiang Fly Ash Development and Utilization Co., Ltd. in Hejin City, Shanxi Province, and the variety model is Grade I.

[0048] The slag used in the present invention is purchased from Baifeng Mineral Products Processing Plant in Shijiazhuang City, Hebei Province, and the grade is S95 slag.

[0049] The calcium hydroxide used in the present invention is purchased from Shanghai MacLean Biochemical Technology Co., Ltd. and has analytical purity.

[0050] The cement used in the present invention is purchased from Anhui Xuanyu Conch Cement Co., Ltd., and the type is ordinary silicate PO 42.5 cement.

[0051] The sludge used in the present invention comes from the dredged sludge in the Xiangjiang River Basin in Yuelu District, Changsha City, Hunan Province, and has a liquid limit of 30.1%.

[0052] Examples 1 to 16

[0053] Phosphogypsum, slag, fly ash and slaked lime were weighed and added into a beaker according to the proportions shown in Table 1, and stirred and mixed using a stirrer with the speed set at 100 rpm and the stirring time at 2 min to ensure that the dry powders were fully mixed.

[0054] Add water to the dry powder mixture at a liquid-to-solid mass ratio of 0.5:1, set the mixer speed to 300 rpm, stir for 2 minutes, and after stopping, use a glass rod to drive the ash on the wall of the cup into the slurry, and continue stirring for 2 minutes.

[0055] After mixing, pour it into a 40mm*40mm*160mm mold, use the knife method and manual shaking, and stop shaking when there are no bubbles.

[0056] The mold is covered with plastic wrap and then put into a sealed bag. After 3 days, the mold is demoulded, and the mold is covered with plastic wrap again. The mold is placed in a curing box at 20°C and 95% humidity for curing.

[0057] When the curing age reached 7d, 14d and 28d respectively, the compressive strength UCS was tested using a uniaxial compression instrument. The test method adopted GB / T17671 cement mortar strength test method (ISO method). Multiple parallel samples were tested and the average value was taken. The results are shown in Table 1 below.

[0058] The test block with a curing age of 7 days was taken for environmental impact test. The specific experimental method adopted the standard HJ 557-2010 "Solid Waste Leaching Toxicity Leaching Method Horizontal Oscillation Method". A sample with a dry weight of 100g was taken, and the required leachate was determined according to the liquid-solid ratio of 10:1 with pure water extract. The oscillation frequency was 110 times / minute, and the room temperature was oscillated for 8 hours and allowed to stand for 16 hours. Finally, the leachate to be tested was obtained with a 0.45μm filter membrane. The sulfate concentration, phosphate ion concentration, fluoride ion concentration and pH value in the sample leachate were measured, and the results are shown in Table 1 below.

[0059] Figure 1 The reaction mechanism is a mixture of phosphogypsum, fly ash, slag, calcium hydroxide and water. The initial reaction of slag and fly ash can produce calcium aluminate hydrate (CAH), which then reacts with phosphogypsum to produce calcium sulfonate (AFt) with better gelling properties to replace CAH and improve the gelling properties of the cementitious material. The reaction process of generating AFt is shown in the following formula (1):

[0060] 3Ca(OH)2+Al2O3+3CaSO4·2H2O+23H2O→3CaO·Al2O3·3CaSO4·32H2O (1)

[0061] The fly ash used in the present invention has a calcium content of less than 10%, and is a low-calcium fly ash. It has low gelling properties. However, when reacting with calcium hydroxide, the active SiO2 and Al2O3 contained in the fly ash can undergo a volcanic ash reaction to generate CSH and CAH with gelling properties.

[0062] The specific CSH reaction process is shown in the following formula (2):

[0063] SiO2+mCa(OH)2+nH2O→mCaO·SiO2·(m+n)CaO·SiO2·(m+n)H2O (2)

[0064] The reaction process of generating CAH is shown in the following formula (3):

[0065] mCa(OH)2+mAl2O3+nH2O→mCaO·Al2O3·(m+n)H2O (3)

[0066] Slag contains a certain amount of cement clinker mineral dicalcium silicate (C2S), etc. Therefore, slag has a certain reactivity and can be mixed with water to undergo hydrolysis reaction to generate CSH and calcium hydroxide crystals. The reaction process is shown in the following formula (4). At the same time, the slag contains alumina components, which can undergo hydration reaction to generate CAH in an alkaline environment. The reaction formula is shown in the above (3).

[0067] 2CaO·SiO2+mH2O=xCaO·SiO2·(m+x-2)H2O+(2-x)Ca(OH)2 (4)

[0068] As can be seen from Table 1, the sulfate concentration of the leachate of the test blocks obtained in each embodiment is higher than 1000 mg / L, which is related to the fact that the main component of phosphogypsum is CaSO4·H2O. The sulfate concentration of the leachate of the test blocks obtained in Examples 2 and 4 is lower than 1500 mg / L, and the compressive strength of these two groups is the highest. This shows that in the reaction systems of these two groups, a large amount of sulfate participates in the volcanic ash reaction, generating a large amount of calcium sulfonate, which increases the strength. In addition, the 28d compressive strength of the test blocks obtained in Examples 6 and 8 exceeds 10 MPa. The soluble phosphate concentration, fluoride ion concentration, and pH of the leachate of these four groups meet the GB 8978-1996 comprehensive sewage discharge standard, that is, the soluble phosphate concentration of the leachate is lower than 0.5 mg / L, the fluoride ion concentration is lower than 10 mg / L, and the pH is between 6 and 9. The reason is that in an alkaline environment, sufficient calcium ions provided by phosphogypsum react with fluoride ions and phosphate ions to generate Ca-F and Ca-P precipitates. At the same time, the cementitious material itself also fixes a large amount of fluoride and inorganic phosphate.

[0069]

[0070] Examples 17 to 26

[0071] The dry powder composition and proportion of the cementitious material obtained in Example 4, i.e., 50.57% phosphogypsum, 28% slag, 20% fly ash, and 1.43% slaked lime, were mixed and stirred for 2 minutes with a mixer, and cement in a corresponding proportion was added and stirred again for 2 minutes to obtain a curing agent dry powder mixture. The mixed curing agent was mixed with the corresponding proportion of sludge for 3 minutes according to the curing agent dosage of 15% to 25% (i.e., the curing agent dosage accounted for the dry weight of the sludge / soft soil to be cured) to obtain a curing system.

[0072] The curing system mixture is poured into a 50mm*100mm cylindrical mold, and the knife method is used in combination with manual shaking. When there are no bubbles, stop shaking.

[0073] The mold is covered with plastic wrap and then put into a sealed bag. After 3 days, the mold is demoulded, and the mold is covered with plastic wrap again. The mold is placed in a curing box at 20°C and 95% humidity for curing.

[0074] When the curing age reaches 7d, 14d, 28d, and 60d, the compressive strength UCS is tested using a uniaxial compression instrument. The test method adopts the standard regulations for unconfined compressive strength test in JTG 3430-2020 "Highway Geotechnical Test Code", tests multiple parallel samples, and takes the average value. The results are shown in Table 2 below.

[0075] Table 2 Curing agent component ratio and curing effect

[0076]

[0077] Note: The moisture content of silt represents the ratio of the mass of water in silt to the mass of dry sludge.

[0078] As shown in Table 2, under the same low dosage conditions, as the addition ratio of cementitious material relative to cement increases, the curing effect of the curing agent of the present application shows a trend of first decreasing and then rapidly increasing. In the range of 3:7 to 7:3 of cement to cementitious material ratio, the curing effect of the curing agent obtained in the present application on sludge is better than that of pure cement. The curing effect of sludge increases with the increase of curing agent dosage. It can be foreseen that with the further increase of curing agent dosage, the curing effect of sludge will also be further improved.

[0079] The above is only a preferred embodiment of the present invention, which certainly cannot be used to limit the scope of rights of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and changes can be made without departing from the principle of the present invention, and these improvements and changes are also regarded as the protection scope of the present invention.

Claims

1. A high-dosage phosphogypsum cementitious material, characterized in that: The parts by weight include: 45-70 parts of phosphogypsum Slag 16.5~35 parts 3-25 parts fly ash 0.5 to 2 parts of slaked lime.

2. The high-dosage phosphogypsum cementitious material according to claim 1, characterized in that: The parts by weight include: 50-66 parts of phosphogypsum 28 parts of slag 5-20 parts fly ash 1.25 to 2 parts of slaked lime.

3. The high-dosage phosphogypsum cementitious material according to claim 1, characterized in that: The phosphogypsum is pretreated by water washing.

4. A high-dosage phosphogypsum-based curing agent, characterized in that: The curing agent comprises the phosphogypsum cementitious material according to any one of claims 1 to 3 and cement, wherein the mass ratio of the phosphogypsum cementitious material to the cement is 7:3 to 3:

7.

5. The high-dosage phosphogypsum-based curing agent according to claim 4, characterized in that: The mass ratio of phosphogypsum cementitious material to cement is 6:4 to 4:

6.

6. A method for solidifying silt / soft soil, characterized in that: The phosphogypsum-based curing agent according to claim 4 or 5 is added to the sludge / soft soil to be solidified.

7. The method according to claim 6, characterized in that The dosage of the phosphogypsum-based curing agent is 15% or more of the dry weight of the sludge / soft soil to be cured.

8. The method according to claim 6, characterized in that The dosage of the phosphogypsum-based curing agent is 15% to 50% of the dry weight of the sludge / soft soil to be cured.

9. The method according to claim 6, characterized in that The moisture content of the silt / soft soil to be solidified is not more than 3 times the liquid limit of the silt / soft soil.

10. The method according to claim 6, characterized in that The water content of the silt / soft soil to be solidified is 2 to 3 times the liquid limit of the silt / soft soil.