High-performance composite lightweight aggregate and preparation method thereof
Through two-step sintering method and glaze slurry treatment, the component ratio and sintering conditions of waste such as fly ash, iron tailings, etc. were optimized to prepare high-performance composite light aggregates, which solved the difficulty of process and insufficient performance in the existing technology. The problem is that high-performance and environmentally friendly light aggregate preparation is achieved, and the performance and environmental friendliness of structural concrete are improved.
Patent Information
- Application Number
- CN202411191729.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-28
- Publication Date
- 2024-12-06
AI Technical Summary
Among the existing light aggregate preparation methods, the sintering method has a high strength but a difficult process. The sintering method has a simple process but a low strength, making it difficult to take into account both high performance and low process difficulty, and at the same time, there is a lack of environmentally friendly solutions.
Using two-step sintering method, using fly ash, iron tailings and other industrial waste as raw materials, combined with glaze slurry, high-performance composite light aggregates are prepared through specific sintering systems and glaze preparation methods, including stirring into balls and grinding. Fine treatment, glazing and sintering steps to optimize component ratios and sintering conditions.
Light aggregates with high strength, small surface pore volume and low water absorption were obtained. They had excellent comprehensive performance, environmentally friendly characteristics, and improved the potential performance of structural concrete, which had certain promotion value.
Smart Images

Figure CN119080417A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of building materials and relates to a high-performance composite lightweight aggregate and a preparation method thereof. Background Art
[0002] With the continuous development of my country's social productivity, the construction industry has experienced rapid growth, but the requirements for construction technology have also become increasingly stringent. Currently, the high performance and green nature of structural concrete are key developments in the construction industry. This requires not only good workability, high strength, excellent service performance, and environmental friendliness, but also, for specific structural projects, reduced deadweight and improved overall performance. Furthermore, it must also achieve the goal of transforming waste into valuable resources, effectively utilizing industrial waste and achieving high quality.
[0003] Lightweight aggregate, with its lightweight and porous properties, has diverse applications in various fields. For example, it has been used to varying degrees in landscape architecture, the chemical industry, and construction, but construction represents the largest application area and the largest volume of consumption. Within the construction sector, water conservancy projects have gradually become a research focus, primarily focusing on river ecological management and improving the durability of marine engineering projects. In river ecosystems and marine environments, the porous nature of lightweight aggregate is primarily utilized to remove harmful ions from water or prevent their transport into the concrete. Raw materials used in its preparation primarily come from industrial solid waste, such as fly ash, slag, red mud, and silt, as well as minerals such as shale, metakaolin, and tailings. Performance indicators primarily focus on strength, apparent density, water absorption, and specific strength. Initial research focused primarily on waste recycling, but as the demand for lightweight aggregate performance has become increasingly stringent, researchers have shifted their focus to performance improvements, particularly in terms of specific strength, which in turn requires more demanding processes.
[0004] Currently, there are many methods for preparing lightweight aggregate, mainly including sintering and sinter-free methods. Each method has its own advantages. Sintering produces lightweight aggregate with higher strength, but the process is more difficult to achieve high-performance products. Sinter-free methods, on the other hand, are simple to produce but have relatively lower strength. Summary of the Invention
[0005] To reduce process complexity, produce lightweight aggregate with superior performance indicators, and maintain environmental protection, this invention provides a high-performance composite lightweight aggregate and its preparation method. Using industrial waste materials such as fly ash and iron ore tailings as raw materials, the high-performance lightweight aggregate is prepared using a two-step sintering process.
[0006] The present invention adopts the following technical solutions to achieve its purpose:
[0007] High-performance composite lightweight aggregate includes a lightweight aggregate matrix and a glaze slurry. The raw materials of the lightweight aggregate matrix include fly ash, iron tailings, and silicon carbide, wherein the mass ratio of fly ash, iron tailings, and silicon carbide is (1-2): (1-2): 0.15; the raw materials of the glaze slurry, calculated by mass percentage, include 10% mica powder, 20%-25% shale tailings, 0-20% iron tailings, 0-10% Class I fly ash, 40%-55% quartz powder, 0-5% sodium bicarbonate, and 0-5% zinc oxide.
[0008] Preferably, the fly ash is Class I fly ash with a density of 2.31 g / cm 3 , specific surface area 334m 2 / kg.
[0009] The preparation method of high-performance composite lightweight aggregate comprises the following steps:
[0010] S1. Preparation of lightweight aggregate matrix: Fly ash, iron ore tailings, and silicon carbide were weighed in a mass ratio of (1-2):(1-2):0.15. The weighed materials were placed in a pelletizing tray and the instrument was started. During the stirring process, an appropriate amount of water (0.4 times the mass of the powder) was gradually added to form pellets and sintered. The sintering schedule was as follows: a heating rate of 10°C / min, a holding period of 10 min at 900°C, and a holding period of 5 min at 1300°C.
[0011] S2. Glaze slurry preparation: by mass percentage, weigh 10% mica powder, 20% to 25% shale tailings, 0 to 20% iron tailings, 0 to 10% Class I fly ash, 40% to 55% quartz powder, 0 to 5% sodium bicarbonate and 0 to 5% zinc oxide, the weighed raw materials were placed in a ball mill for grinding, the ball milling time was 6 hours, the ball mill speed was 320r / min; the ground raw material was sieved through a 250 mesh square, the bottom fine material was taken, the metal impurities in the fine material were removed, the fine powder was added to the same mass of tap water, and stirred evenly for 120s and set aside;
[0012] S3. Glazing: After the glaze slurry is prepared, the lightweight aggregate substrate is evenly coated with glaze (immersed in the glaze slurry for 10 seconds and then removed). The glaze layer is 0.3-0.5 mm thick and left to stand for 24 hours.
[0013] S4. Sintering: After glazing the surface of the lightweight aggregate, pre-sinter it to 200°C at a heating rate of 5°C / min, roast it to 900°C and hold it for 10 minutes, calcine it to 1200°C and hold it for 5 minutes, and finally cool it naturally to room temperature to obtain a high-performance composite lightweight aggregate.
[0014] The beneficial effects of the present invention are:
[0015] This invention uses industrial waste materials such as fly ash and iron ore tailings as primary raw materials. Through component optimization and a two-step sintering process, the resulting lightweight aggregate boasts high strength, relatively low surface pore volume, low water absorption, and excellent overall performance. This lightweight aggregate not only potentially enhances the performance of modern structural concrete but also transforms waste into valuable resources, achieving environmentally friendly benefits and significant potential for widespread adoption.
[0016] The preparation method of the present invention sets the heating rate at 5°C / min, pre-sintering to 200°C, heating to 900°C and holding for 10 minutes, then heating to 1200°C and holding for 5 minutes, followed by natural cooling to room temperature. The resulting lightweight aggregate has excellent properties. Its particle strength increased by approximately 7.00%, its water absorption decreased by approximately 36.07%, its apparent density decreased by approximately 14.65%, and its specific strength increased by approximately 25.37%. BRIEF DESCRIPTION OF THE DRAWINGS
[0017] Figure 1 This is the SEM morphology of fly ash.
[0018] Figure 2 This is the XRD phase diagram of fly ash.
[0019] Figure 3 It is a characteristic diagram of lightweight aggregate matrix strength, apparent density and water absorption.
[0020] Figure 4 It is the water absorption and specific strength characteristics of the lightweight aggregate matrix.
[0021] Figure 5 It is a defect diagram of glazed and then sintered lightweight aggregate.
[0022] Figure 6 It is a diagram of the glazed and sintered lightweight aggregate of the present invention.
[0023] Figure 7 This is a comparison chart of the performance changes of lightweight aggregate before and after glazing according to the proportion.
[0024] Figure 8 This is a performance comparison chart of lightweight aggregate before and after glazing according to the second ratio.
[0025] Figure 9 This is a performance comparison chart of lightweight aggregate before and after glazing.
[0026] Figure 10 This is the XRD characteristic diagram of lightweight aggregate.
[0027] Figure 11 This is the SEM morphology of lightweight aggregate.
[0028] Figure 12 This is the SEM-EDS line analysis test result of the proportioned, glazed and then fired lightweight aggregate.
[0029] Figure 13 This is the SEM-EDS line analysis test result of the second-proportion glazing and re-fired lightweight aggregate.
[0030] Figure 14 This is the SEM-EDS line analysis test result of the three-glaze re-fired lightweight aggregate DETAILED DESCRIPTION
[0031] The present invention is described in detail below with reference to the accompanying drawings and specific embodiments. It should be understood that the embodiments described are only a portion of the embodiments of the present invention, not all of them. All other embodiments derived by persons of ordinary skill in the art based on the embodiments of the present invention without inventive effort should fall within the scope of protection of the present invention. 1. Specific embodiments
[0033] Example 1
[0034] The raw materials of the lightweight aggregate matrix include fly ash, iron tailings, and silicon carbide, wherein the mass ratio of fly ash, iron tailings, and silicon carbide is 2:1:0.15.
[0035] Weigh the materials one by one, place them in the ball-forming tray, and start the instrument. During the stirring process, gradually add an appropriate amount of water (0.4 times the weight of the powder) to form balls. When the surface of the lightweight aggregate is slightly shiny, stop the rotation. The raw lightweight aggregate is sintered according to the established sintering system: a heating rate of 10°C / min, a holding time of 900°C for 10 minutes, and a holding time of 1300°C for 5 minutes.
[0036] Example 2
[0037] The raw materials of the lightweight aggregate matrix include fly ash, iron tailings, and silicon carbide, wherein the mass ratio of fly ash, iron tailings, and silicon carbide is 1:1:0.15.
[0038] Weigh the materials one by one, place them in the ball-forming tray, and start the instrument. During the stirring process, gradually add an appropriate amount of water (0.4 times the weight of the powder) to form balls. When the surface of the lightweight aggregate is slightly shiny, stop the rotation. The raw lightweight aggregate is sintered according to the established sintering system: a heating rate of 10°C / min, a holding time of 900°C for 10 minutes, and a holding time of 1300°C for 5 minutes.
[0039] Example 3
[0040] The raw materials of the lightweight aggregate matrix include fly ash, iron tailings, and silicon carbide, wherein the mass ratio of fly ash, iron tailings, and silicon carbide is 1:2:0.15.
[0041] Weigh the materials one by one, place them in the ball-forming tray, and start the instrument. During the stirring process, gradually add an appropriate amount of water (0.4 times the weight of the powder) to form balls. When the surface of the lightweight aggregate is slightly shiny, stop the rotation. The raw lightweight aggregate is sintered according to the established sintering system: a heating rate of 10°C / min, a holding time of 900°C for 10 minutes, and a holding time of 1300°C for 5 minutes.
[0042] Example 4
[0043] The glaze slurry raw materials, calculated by mass percentage, include 10% mica powder, 25% shale tailings, 0 iron tailings, 10% Class I fly ash, 55% quartz powder, 0 sodium bicarbonate and 0 zinc oxide.
[0044] According to the above-mentioned established ratio, the raw materials were accurately weighed; the weighed raw materials were placed in a ball mill for grinding for 6 hours at a ball mill speed of 320r / min; the ground raw materials were passed through a 250-mesh square sieve to take the bottom fine material; and a magnetic rod was used to absorb the metal impurities in the fine material, mainly iron; the obtained fine powder was added to an equal mass of tap water, stirred evenly for 120s, and set aside for use.
[0045] Example 5
[0046] The glaze slurry raw materials, calculated by mass percentage, include 10% mica powder, 20% shale tailings, 20% iron tailings, 0% Class I fly ash, 45% quartz powder, 5% sodium bicarbonate and 0% zinc oxide.
[0047] According to the above-mentioned established ratio, the raw materials were accurately weighed; the weighed raw materials were placed in a ball mill for grinding for 6 hours at a ball mill speed of 320r / min; the ground raw materials were passed through a 250-mesh square sieve to take the bottom fine material; and a magnetic rod was used to absorb the metal impurities in the fine material, mainly iron; the obtained fine powder was added to an equal mass of tap water, stirred evenly for 120s, and set aside for use.
[0048] Example 6
[0049] The raw materials of the glaze slurry include, by mass percentage, 10% mica powder, 20% shale tailings, 20% iron tailings, 0% Class I fly ash, 40% quartz powder, 5% sodium bicarbonate and 5% zinc oxide.
[0050] According to the above-mentioned established ratio, the raw materials were accurately weighed; the weighed raw materials were placed in a ball mill for grinding for 6 hours at a ball mill speed of 320r / min; the ground raw materials were passed through a 250-mesh square sieve to take the bottom fine material; and a magnetic rod was used to absorb the metal impurities in the fine material, mainly iron; the obtained fine powder was added to an equal mass of tap water, stirred evenly for 120s, and set aside for use.
[0051] Example 7
[0052] The lightweight aggregate substrate is evenly covered with glaze by dipping it in glaze slurry for 10 seconds and then taking it out. The thickness of the glaze layer is 0.3 to 0.5 mm. The substrate is left to stand naturally for 24 hours to obtain the glazed lightweight aggregate.
[0053] Example 8
[0054] After glazing the collective surface of the lightweight aggregate, it was pre-fired to 200°C at a heating rate of 5°C / min, roasted to 900°C and kept warm for 10 minutes, calcined to 1200°C and kept warm for 5 minutes, and finally naturally cooled to room temperature to obtain high-performance composite lightweight aggregate.
[0055] 2. Performance Study
[0056] 1. Study the properties of the matrix in composite lightweight aggregate, mainly including the strength, apparent density, water absorption, specific strength and P specific strength characteristics of the lightweight aggregate matrix, see Figure 3 .
[0057] from Figure 3 As can be seen from the data, the strength and apparent density of lightweight aggregate exhibit different characteristics as the fly ash to iron tailings ratio changes. In terms of strength, increasing fly ash content leads to a sharp drop in strength. When the fly ash ratio is 1:1, the strength is relatively small, decreasing by approximately 41.2% compared to the 2:1 ratio. At a 1:2 ratio, the strength recovers slightly. Apparent density also shows a downward trend, but the decrease is relatively balanced across the different fly ash ratios. Furthermore, water absorption increases with increasing fly ash content, a result consistent with apparent density. The strength characteristics of a material are closely related to its apparent density. Similarly, variations in the elemental content of lightweight aggregate due to changes in the fly ash ratio lead to differences in physical properties, such as viscosity, in the resulting products and during calcination. This results in variations in strength and apparent density among different lightweight aggregates.
[0058] 2. Characteristics of water absorption and strength
[0059] Based on the above research, the specific strength and P specific strength characteristics of lightweight aggregate with different mixing ratios were studied. The results are as follows: Figure 4 shown.
[0060] from Figure 4It can be seen that with the change of the mixing ratio of fly ash and iron tailings, their specific strength and P specific strength show a large difference. First of all, the specific strength here is an indicator of the compressive strength of lightweight aggregate and its apparent density. The figure shows that when the mixing ratio of the two is 2:1, the specific strength of the lightweight aggregate is relatively large. As a result, its strength characteristics show that under this working condition, the strength of the lightweight aggregate is large, while the decrease in its apparent density is not significant. The use of specific strength to analyze the comprehensive performance of materials is better than that of a single strength. However, for materials such as lightweight aggregate, they should have low permeability in improving the durability of structural concrete. Therefore, the use of P specific strength (specific strength divided by its water absorption rate) to ensure the comprehensive performance of lightweight aggregate is better to a certain extent. As Figure 4 As shown in Figure (b), it is clear that the fly ash and iron tailings ratio of 2:1 still has a higher P specific strength, followed by the ratio of 1:2. The P specific strength is lowest when the ratio is 1:1, indicating that the lightweight aggregate has low strength and poor surface condition.
[0061] 3. Characteristics of high-performance composite lightweight aggregate products
[0062] After the glaze slurry is prepared, the lightweight aggregate is evenly covered with glaze on the surface by dipping it in glaze, and then placed naturally for 24 hours before sintering. The lightweight aggregate after surface glazing is based on the benchmark sintering system, and the heating rate and the maximum calcination temperature are adjusted for different ratios. During the adjustment process, with Example 1 as the lightweight aggregate matrix and Example 4 as the glazed glaze slurry, the heating rate is above 8°C, the maximum calcination temperature is above 1250°C, and the insulation time is above 5 minutes, dry glaze, cracks, glaze protrusions and other phenomena appear. The characteristics of the fired lightweight aggregate are as follows: Figure 5 Combined with the actual firing conditions, when the heating rate is reduced to 5℃ / min, the calcination temperature is reduced to 1200℃, and the rest are calcined according to the benchmark sintering system, the sintering effect of the lightweight aggregate is better. The fired lightweight aggregates are as follows Figure 6 As shown ( Figure 6 Ratio 1 is Example 1 + Example 4, Ratio 2 is Example 1 + Example 5, and Ratio 3 is Example 1 + Example 6).
[0063] pass Figure 5 and Figure 6 It can be seen that the raw material composition and sintering schedule have a significant impact on the sintering quality of glazed and refired lightweight aggregate. Due to the presence of a certain amount of micropores on the surface of the base lightweight aggregate, when sintering using different sintering schedules, the amount of glaze adhering to the lightweight aggregate is too small, which can easily lead to dry glaze. If the heating rate is too fast, the difference in expansion between the raw materials can easily cause stress differences, resulting in cracking of the glaze layer. If the raw materials have poor meltability and the sintering time is too short, glaze protrusion is likely to occur. If the sintering time is too long, the porous structure of the lightweight aggregate can easily lead to glaze seepage.
[0064] Based on the above experiments and analysis, after the surface of the lightweight aggregate is glazed, it is pre-fired to 200℃ at a heating rate of 5℃ / min, roasted to 900℃ and kept warm for 10min, calcined to 1200℃ and kept warm for 5min, and finally naturally cooled to room temperature. The surface properties of the fired lightweight aggregate are better (such as Figure 6 ).
[0065] 4. Basic characteristics of high-performance composite lightweight aggregate
[0066] (1) Ratio 1 (Example 1+Example 4)
[0067] First, glaze slurry was prepared with ratio 1, and glaze was applied on the surface of lightweight aggregate using the "dipping glaze" method; the glaze was calcined to 1200℃ at a heating rate of 5℃ / min, and then re-sintered, and compared with the lightweight aggregate before glazing and the unglazed and re-fired lightweight aggregate.
[0068] A comprehensive analysis of the water absorption, apparent density, particle strength and specific strength of lightweight aggregate before and after glazing was conducted to compare the effects of glazing on the performance of lightweight aggregate. The performance of lightweight aggregate sintered after glazing was compared with that of lightweight aggregate before glazing and lightweight aggregate sintered without glazing. The specific numerical change rates are as follows: Figure 7 shown.
[0069] pass Figure 7 It can be seen that, compared with the unglazed lightweight aggregate, the water absorption rate of the glazed and refired lightweight aggregate decreased by about 43.17%, the apparent density decreased by about 3.77%, the particle strength decreased by about 2.81%, and the specific strength increased by about 1.00%. Compared with the unglazed and refired lightweight aggregate, the water absorption rate decreased by about 24.36%, the apparent density decreased by about 0.22%, the particle strength decreased by about 16.68%, and the specific strength decreased by about 16.49%. This shows that when lightweight aggregate is glazed and refired, its water absorption rate, apparent density, and particle strength decrease, while its specific strength increases. Compared with the unglazed and refired lightweight aggregate, the water absorption rate, particle strength, and apparent density-to-strength ratio all decrease. Based on the above analysis, the reasons are that after the unglazed lightweight aggregate is re-fired, the unmelted substances in the lightweight aggregate may remelt again, thereby increasing the strength; after glazing and re-firing, the fly ash and other materials in the glaze slurry raw materials have poor meltability, resulting in poor compatibility between the glaze-forming layer and the lightweight aggregate surface, which in turn leads to a decrease in the strength of the lightweight aggregate.
[0070] (2) Ratio 2 (Example 1+Example 5)
[0071] Using the second ratio, a comprehensive analysis was conducted on the water absorption rate, apparent density, particle strength and specific strength of the lightweight aggregate before and after glazing, and the effects of glazing on the performance of the lightweight aggregate were compared. The performance of the lightweight aggregate after glazing and then fired was compared with that before glazing and that of the lightweight aggregate after unglazing and then fired. The specific numerical change rates are as follows: Figure 8 shown.
[0072] pass Figure 8 It can be seen that the water absorption rate of the glazed and refired lightweight aggregate decreased by about 37.43%, the apparent density decreased by about 2.06%, the particle strength decreased by about 1.07%, and the specific strength increased by about 1.01% compared with the unglazed and refired lightweight aggregate. Compared with the unglazed and refired lightweight aggregate, the water absorption rate decreased by about 16.73%, the apparent density increased by about 1.55%, the particle strength decreased by about 15.19%, and the specific strength decreased by about 16.48%. Figure 3 The analysis shows that after improving the sintering performance of the glaze slurry raw materials, the water absorption rate, apparent density and particle strength of the lightweight aggregate still decrease, and the specific strength still increases; compared with the unglazed and re-fired lightweight aggregate, the water absorption rate, particle strength and specific strength decrease, and the apparent density increases; compared with the use of ratio 1, the water absorption rate, apparent density and particle strength of the lightweight aggregate increase, while the specific strength remains basically unchanged. Based on the above analysis, the reason is considered to be: after the lightweight aggregate is glazed and re-fired, the aggregate surface undergoes a complex melting reaction with the glaze slurry raw materials, resulting in defects such as glaze protrusion and shrinkage ( Figure 6 As can be seen in (d), the strength and other properties of lightweight aggregate decrease.
[0073] (3) Ratio 3 (Example 1+Example 6)
[0074] A comprehensive analysis of the water absorption, apparent density, particle strength and specific strength of lightweight aggregate before and after glazing was conducted to compare the effects of glazing on the performance of lightweight aggregate. The performance of lightweight aggregate sintered after glazing was compared with that of lightweight aggregate before glazing and lightweight aggregate sintered without glazing. The specific numerical change rates are as follows: Figure 9 shown.
[0075] pass Figure 9 It can be seen that the water absorption rate of the glazed and refired lightweight aggregate decreased by about 36.07%, the apparent density decreased by about 14.65%, the particle strength increased by about 7.00%, and the specific strength increased by about 25.37% compared with the unglazed and refired lightweight aggregate; compared with the unglazed and refired lightweight aggregate, the water absorption rate decreased by about 14.91%, the apparent density increased by about 11.50%, the particle strength decreased by about 8.27%, and the specific strength increased by about 3.66%. Figure 7-9The analysis in shows that after the introduction of zinc oxide, the water absorption rate and apparent density of the lightweight aggregate decrease, and the particle strength and specific strength increase; compared with the unglazed and refired lightweight aggregate, the water absorption rate, apparent density and particle strength decrease, and the specific strength increases; compared with the use of ratio 2, the water absorption rate, particle strength and specific strength of the lightweight aggregate all increase, while the apparent density decreases.
[0076] 5. Micro-analysis
[0077] The above studies have studied the macroscopic properties of once-sintered and glazed and then-sintered lightweight aggregates. In order to further clarify their mechanism of action, this part, based on the above studies, further studies and analyses are conducted from the aspects of microscopic phase and morphological characteristics, respectively. Figure 10 、 Figure 11 and Figure 12 shown.
[0078] 5.1 Phase analysis (XRD)
[0079] Figure 10 (a) is the XRD diffraction characteristic peak of the raw material mixture, sintering before glazing (raw material primary sintering) and re-sintering before glazing (raw material secondary sintering). Figure 10 As can be seen in (a), the main phases of the raw materials are silicon dioxide crystals (26.639°, type 101) and calcium-containing silicon organic crystals (8.315°~9.245°). For the samples sintered before glazing, due to the effect of high-temperature sintering, the concentration of silicon dioxide and other crystalline phases decreased sharply, especially the calcium-containing silicon organic crystals, whose characteristic peaks almost disappeared; as the samples were re-sintered, the intensity of the characteristic peaks of the silicon dioxide crystal phase continued to decrease. Figure 10 (b) shows the XRD peaks inside and outside the lightweight aggregates at different mixes. As can be seen from the figure, the XRD peaks inside and outside the three mixes have similar characteristics, namely, the concentration of the crystalline phase on the outside is lower than that on the inside. This is mainly due to the more enamelized material on the outside, and the enamel material is mostly amorphous, which is beneficial for improving the surface properties of lightweight aggregates.
[0080] 5.2 Morphology analysis (SEM)
[0081] On this basis, we further analyzed the microstructure of lightweight aggregate. The results are as follows: Figure 11 shown.
[0082] from Figure 11 It can be seen that the internal structure of the three proportions of lightweight aggregates are all porous, which is the basis of lightweight aggregates. From the perspective of sintering and re-sintering ( Figure 11 (h) and Figure 11 (i)), its internal structure has not changed significantly, and its amorphous degree has been further improved (e.g. Figure 10(a)). From the external conditions, the glaze materials of the three ratios show that the surface pore volume of ratio 1 is larger, followed by ratio 2, and the smallest is ratio 3. This is one of the main reasons for the difference in P specific strength of lightweight aggregate.
[0083] 5.3 Elemental analysis (EDS)
[0084] At the same time, the lightweight aggregate after glazing and sintering was subjected to SEM-EDS line analysis test, and the results are as follows Figure 12 shown.
[0085] pass Figure 12 It can be seen that the silicon and aluminum content in the lightweight aggregate changes significantly from the inside to the outside. The closer to the outer surface, the higher the silicon and oxygen content, while the aluminum content decreases. From these results, it can be inferred that the glass micro-glaze content on the aggregate surface increases after glazing.
[0086] pass Figure 13 It can be seen that when the glaze slurry is prepared according to ratio 2 and the glaze is applied to the lightweight aggregate surface and then sintered, the main elements of the internal skeleton of the aggregate remain almost unchanged compared with ratio 1, but the content of small amounts of elements such as calcium, magnesium, sodium, potassium and iron in the surface area increases slightly.
[0087] pass Figure 13 It can be seen that when the glaze slurry is prepared with the ratio 2 and the glaze is applied on the surface of the lightweight aggregate and calcined again, the outer surface of the aggregate is mainly composed of silicon, aluminum and oxygen elements. Compared with the ratio 1, a small amount of elements such as magnesium in the outer surface area has increased. The sintering performance of the raw materials for preparing the glaze slurry is improved. Figure 11 It can also be seen that the firing quality of the glaze layer improves, and the changes in the types and contents of elements cause changes in its performance.
[0088] Summary:
[0089] (1) The sintering system has a significant effect on the compatibility of the body (lightweight aggregate) and glaze. The performance of the glazed and then fired light aggregate also changes with different sintering systems. When the three self-developed ratios are used, after glazing the surface of the light aggregate, the temperature is increased at a rate of 5°C / min, pre-fired to 200°C, roasted to 900°C and kept warm for 10 minutes, calcined to 1200°C and kept warm for 5 minutes, and finally naturally cooled to room temperature, the performance of the fired light aggregate is relatively good.
[0090] (2) Compared with the light aggregate before glazing, the water absorption rate, apparent density and particle strength of the glazed and refired light aggregate decreased, while the specific strength increased when the ratio 1 and ratio 2 were used; when the ratio 3 was used, the water absorption rate and apparent density of the light aggregate decreased, while the particle strength and specific strength increased.
[0091] (3) Compared with the unglazed and refired lightweight aggregate, when the glazed and refired lightweight aggregate adopts the ratio 1, the water absorption rate, apparent density, particle strength and specific strength of the lightweight aggregate decrease; when the ratio 2 is adopted, the water absorption rate, particle strength and specific strength decrease, and the apparent density increases; when the ratio 3 is adopted, the water absorption rate, apparent density and particle strength decrease, and the specific strength increases.
[0092] (4) Compared with the three glaze slurry ratios, when the three pairs of lightweight aggregates were glazed and fired again, the water absorption rate decreased by about 36.07%, the apparent density decreased by about 14.65%, the particle strength increased by about 7.00%, and the specific strength increased by about 25.37%. Its apparent density was lower, the particle strength and specific strength were larger, the aggregate surface was denser, and the overall performance was better.
Claims
1. High performance composite lightweight aggregate, characterized in that: It includes a lightweight aggregate matrix and a glaze slurry. The raw materials of the lightweight aggregate matrix include fly ash, iron tailings, and silicon carbide, wherein the mass ratio of fly ash, iron tailings, and silicon carbide is (1-2): (1-2): 0.15; the raw materials of the glaze slurry, calculated by mass percentage, include 10% mica powder, 20%-25% shale tailings, 0-20% iron tailings, 0-10% Class I fly ash, 40%-55% quartz powder, 0-5% sodium bicarbonate, and 0-5% zinc oxide.
2. The high performance composite lightweight aggregate according to claim 1, characterized in that: The fly ash is Class I fly ash with a density of 2.31 g / cm 3 , specific surface area 334m 2 / kg.
3. A method for preparing high-performance composite lightweight aggregate, characterized in that: The following steps are involved: S1. Preparation of lightweight aggregate matrix: fly ash, iron tailings and silicon carbide are weighed in a mass ratio of (1-2): (1-2): 0.15, the weighed materials are placed in a ball-forming plate, and the instrument is started. Water is gradually added during the stirring process to form balls and sinter them; S2. Preparation of glaze slurry: According to the mass percentage, weigh 10% mica powder, 20% to 25% shale tailings, 0 to 20% iron tailings, 0 to 10% Class I fly ash, 40% to 55% quartz powder, 0 to 5% sodium bicarbonate and 0 to 5% zinc oxide, and put the weighed raw materials into a ball mill for grinding. The ball milling time is 6 hours and the ball mill speed is 320r / min; the ground raw materials are sieved through a 250-mesh square sieve, the bottom fine material is taken, the metal impurities in the fine material are removed, and the obtained fine powder is added to the same mass of tap water, and stirred evenly for 120s and set aside; S3. Glazing: After the glaze slurry is prepared, the lightweight aggregate substrate is evenly covered with glaze by dipping the glaze on the surface of the lightweight aggregate substrate and left to stand naturally for 24 hours; S4. Sintering: After glazing the collective surface of the lightweight aggregate, pre-sinter it to 200°C at a heating rate of 5°C / min, roast it to 900°C and keep it warm for 10 minutes, calcine it to 1200°C and keep it warm for 5 minutes, and finally cool it naturally to room temperature to obtain high-performance composite lightweight aggregate.
4. The method for preparing high-performance composite lightweight aggregate according to claim 3, characterized in that: In step S1, the sintering system is: heating rate 10°C / min, keeping at 900°C for 10min, and keeping at 1300°C for 5min.
5. The method for preparing high-performance composite lightweight aggregate according to claim 3, characterized in that: In step S1, the amount of water added is 0.4 times the total mass of fly ash, iron ore tailings and silicon carbide powder.
6. The method for preparing high-performance composite lightweight aggregate according to claim 3, characterized in that: In step S3, the glazing is performed by immersing the object in the glaze slurry for 10 seconds and then taking the object out.
7. The method for preparing high-performance composite lightweight aggregate according to claim 3, characterized in that: In step S3, the thickness of the glaze layer is 0.3-0.5 mm.