Road asphalt anti-stripping agent as well as preparation method and application thereof
By using composite powder, fatty alcohol polyoxyethylene ether phosphate, soda lignin and modified nanosilica components in road asphalt anti-flaking agent, the problem of insufficient adhesion between tailings aggregate and asphalt is solved, which significantly It improves the water stability and high temperature stability of asphalt mixture, and meets the performance indicators of road surface use.
Patent Information
- Application Number
- CN202310652361.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-06-05
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2043-06-05
AI Technical Summary
In the prior art, insufficient adhesion between tailings aggregate and asphalt causes loose water damage problems such as lump surfaces, pit grooves, and slurry. The commonly used anti-flaking agent has poor thermal stability, making it difficult to effectively improve asphalt mixing. Water stability of the material.
Using a road asphalt anti-flaking agent, including composite powders, fatty alcohol polyoxyethylene ether phosphate, soda lignin, organosilane and modified nanosilia, to improve asphalt and aggregates through hydrogen bonding adsorption and crosslinking. The adhesion of the modified nanosilicon dioxide is closely combined with the aggregate and asphalt interface to enhance the anti-flaking performance.
It significantly improves the water stability, high temperature stability and low temperature crack resistance of tailings asphalt mixture, meets the performance indicator requirements for road surface use, extends the aging performance of asphalt, and promotes the comprehensive utilization of tailings solid waste.
Smart Images

Figure BDA0004265571660000081 
Figure BDA0004265571660000091
Abstract
Description
Technical Field
[0001] The invention relates to the field of road asphalt additives, and in particular to a road asphalt anti-stripping agent and a preparation method and application thereof. Background Art
[0002] The accumulation of large amounts of tailings can easily cause geological disasters, environmental pollution and waste of land resources. In recent years, the comprehensive utilization of tailings has become more and more common, but has not yet been applied on a large scale. Using tailings as an aggregate substitute in high-grade asphalt concrete pavement materials can not only improve the comprehensive utilization value of iron tailings, but also greatly reduce the cost of asphalt pavement construction.
[0003] Compared with conventional aggregates, the physical and mechanical properties of tailings aggregates meet the requirements of aggregate specifications. However, iron tailings are high-silicon stones with poor adhesion to asphalt, which can easily lead to loose, rough, pothole-like, pumping and other water damage on the road surface. The key to water damage is the insufficient adhesion between asphalt and aggregate, which causes the asphalt film to fall off the aggregate surface. Therefore, in order to use tailings aggregates and prevent the occurrence of water damage, it is crucial to improve the adhesion between asphalt and aggregate. The simplest and most effective way is to add an anti-stripping agent. However, at present, there is no anti-stripping agent specifically for tailings aggregates, and the commonly used anti-stripping agents are mostly amine compounds, which act directly on asphalt, have poor thermal stability, and easily lead to performance failure.
[0004] CN102174264A discloses a method for preparing a road asphalt anti-stripping agent and a preparation method thereof. The anti-stripping agent comprises the following components: 50-65 parts of polyethylene glycol; 10-30 parts of alkoxy aliphatic polyamines; 5-15 parts of alkylamines; 5-15 parts of polyamines; 1-2 parts of alcohol ether compounds; and 13-29 parts of diethanolamine. However, aliphatic amine anti-stripping agents have poor thermal stability and are mainly based on physical adsorption, which limits the use of amine anti-stripping agents.
[0005] CN108623207A discloses an asphalt anti-stripping agent containing phosphate salt and a method for using the same. The anti-stripping agent is composed of sodium dodecyl phosphate and octadecyl trimethyl ammonium chloride. When used, the anti-stripping agent needs to be evenly mixed with hot asphalt, but the aggregate is not modified. When the amount added is small, uneven dispersion is likely to result in limited anti-stripping effect.
[0006] In summary, developing an asphalt anti-stripping agent with good thermal stability and significantly improved adhesion to comprehensively utilize iron ore solid waste has important social and economic significance. Summary of the invention
[0007] In view of the shortcomings of the prior art, the purpose of the present invention is to provide a road asphalt anti-stripping agent and its preparation method and application. The road asphalt anti-stripping agent of the present invention can improve the adhesion between tailings aggregate and asphalt and improve the water stability of tailings asphalt mixture.
[0008] The first aspect of the present invention provides a road asphalt anti-stripping agent, which comprises the following components in parts by weight:
[0009] Composite powder: 100 parts;
[0010] Fatty alcohol polyoxyethylene ether phosphate: 3 to 15 parts, preferably 5 to 10 parts;
[0011] Soda lignin: 40-80 parts, preferably 60-75 parts;
[0012] Organosilane: 2 to 8 parts, preferably 2 to 5 parts;
[0013] Modified nano-silicon dioxide: 15 to 50 parts, preferably 20 to 40 parts.
[0014] The composite powder is a mixture of at least two of CaCO3 powder, Ca(OH)2 powder and NaOH powder, preferably a mixture of three of CaCO3 powder, Ca(OH)2 powder and NaOH powder. The average particle size of the composite powder is 20 to 50 μm.
[0015] Among them, the composite powder is preferably a mixture of CaCO3 powder, Ca(OH)2 powder and NaOH powder. Based on the total mass of the composite powder, CaCO3 powder accounts for 30% to 50% of the total mass, Ca(OH)2 powder accounts for 30% to 40% of the total mass, and NaOH powder accounts for 10% to 40% of the total mass.
[0016] The fatty alcohol polyoxyethylene ether phosphate AEO-P has a general formula of RO(CH2CH2O)nPO3H2, where n is an integer of 3 to 9. The fatty alcohol ROH used in synthesizing the fatty alcohol polyoxyethylene ether phosphate is a normal fatty alcohol and / or an isomeric fatty alcohol selected from C8-18 alcohols, such as one or more of isooctyl alcohol, lauryl alcohol, isomeric decanol, and cetyl alcohol.
[0017] The properties of the soda lignin include: density of 0.3-0.5 g / cm 3 , average particle size of 25 to 40 μm, purity of not less than 70 wt%, ash content of not more than 8 wt%, water content of not more than 10 wt%, and degradation temperature of 200 to 500 °C.
[0018] The soda lignin can be extracted by a conventional soda pulp process, wherein the soda pulp is pulped by sodium hydroxide.
[0019] The organosilane is a mixture of aminosilane and long-chain organosilane, wherein the aminosilane accounts for 30% to 50% of the total mass of the organosilane, and the long-chain organosilane accounts for 50% to 70% of the total mass of the organosilane.
[0020] The aminosilane is one or more of N-(2-N-benzylaminoethyl)-3-aminopropyltrimethoxysilane, N-[[[2-(trimethoxysilyl)ethyl]phenyl]methyl]-1,2-ethylenediamine, N-(6-aminohexyl)aminomethyltriethoxysilane, 3-(4-ureaamino)propyltriethoxysilane, and N-(2-aminoethyl)-11-aminoundecyltrimethoxysilane.
[0021] The long-chain organic silane is one or more of dodecyltrimethoxysilane, dodecyltriethoxysilane, dodecylmethyldimethoxysilane, hexadecyltrimethoxysilane and octadecyltrimethoxysilane.
[0022] The modified nano silicon dioxide comprises the following components by weight:
[0023] Nano silicon dioxide: 100 parts;
[0024] 3-glycidyloxypropylmethyldiethoxysilane (GPTMS): 3 to 8 parts, preferably 3 to 6 parts;
[0025] Polyethyleneimine (PEI): 3 to 10 parts, preferably 5 to 8 parts.
[0026] The nano silicon dioxide and 3-glycidyloxypropylmethyldiethoxysilane are both commercially available products.
[0027] The molecular weight of the polyethyleneimine is 1000-70000, preferably one or more of 1000, 20000 and 70000.
[0028] The second aspect of the present invention provides a method for preparing the above-mentioned road asphalt anti-stripping agent, comprising:
[0029] (1) uniformly mixing fatty alcohol polyoxyethylene ether phosphate and organosilane to prepare a prefabricated mixed solution;
[0030] (2) preparing modified nano-silicon dioxide;
[0031] (3) mixing the composite powder, soda lignin, and modified nano-silica uniformly to obtain a prefabricated mixed powder;
[0032] (4) The prefabricated mixed liquid obtained in step (1) is evenly sprayed on the prefabricated mixed powder obtained in step (3), and dried to obtain an asphalt anti-stripping agent.
[0033] In step (1), the fatty alcohol polyoxyethylene ether phosphate can be prepared by the following method: under nitrogen protection, first add 3 parts by weight of fatty alcohol polyoxyethylene ether AEO, preferably add 1 part by weight of P2O5 in batches while stirring, heat up and continue stirring, add and hydrolyze to obtain fatty alcohol polyoxyethylene ether phosphate. Wherein, the heating temperature is 80-90°C, the stirring time after heating is 3-6h, the hydrolysis temperature is consistent with the reaction temperature, the hydrolysis time is 1.5-3h, and the amount of water added is 3%-7% of the total product.
[0034] In step (1), the mixing temperature of the fatty alcohol polyoxyethylene ether phosphate and the organosilane is 45-65°C.
[0035] In step (2), the method for preparing modified nano-silicon dioxide is as follows:
[0036] Nano-silica and 3-glycidyloxypropylmethyldiethoxysilane (GPTMS) are mixed in anhydrous ethanol, reacted under a first heating reflux condition, polyethyleneimine (PEI) is added after the reaction is completed, reacted under a second heating reflux condition, filtered, washed and dried after cooling to obtain modified nano-silica.
[0037] The first heating reflux reaction temperature is 90° C. to 130° C., preferably 100° C. to 115° C., and the reaction time is 12 to 18 hours.
[0038] The reaction temperature of the second heating reflux is 90° C. to 120° C., preferably 95° C. to 110° C., and the reaction time is 20 to 24 hours.
[0039] The first reflux temperature is preferably 3-10° C. higher than the second reflux temperature.
[0040] The filtering and washing can be performed in a conventional manner in the art.
[0041] The drying temperature is 80° C. to 120° C., and the drying time is 0.5 to 5 hours, preferably 3 to 5 hours.
[0042] In step (4), the drying temperature is 95 to 110° C., and the drying time is 2 to 5 hours.
[0043] The third aspect of the present invention discloses an application of the above-mentioned road asphalt anti-stripping agent in asphalt mixture.
[0044] The asphalt mixture is tailings aggregate asphalt mixture.
[0045] The application includes: adding the road asphalt anti-stripping agent into the mineral powder of tailings aggregate asphalt mixture, wherein the amount of the road asphalt anti-stripping agent added accounts for 30wt% to 50wt% of the mineral powder mass, the coarse aggregate and the fine aggregate in the tailings aggregate asphalt mixture are both iron ore waste rock, and the mineral powder is iron tailings powder after magnetic separation.
[0046] Compared with the prior art, the present invention has the following characteristics:
[0047] (1) The asphalt anti-stripping agent of the present invention shows appropriate alkalinity and acts as part of the mineral powder, which can improve the acidic environment of the aggregate surface, and has a large specific surface area, and can more fully adsorb asphalt. The fatty alcohol polyoxyethylene ether phosphate has different functional groups at both ends, one end undergoes hydrogen bonding adsorption with the hydroxyl group on the aggregate surface, and the other end is entangled and cross-linked with the asphalt polymer, so that the overall adhesion of the asphalt mixture is enhanced, and the different functional groups at both ends of the fatty alcohol polyoxyethylene ether phosphate can cooperate with the aminosilane and long-chain organosilane in the organosilane to improve the connection ability with the acidic stone and the matrix asphalt, and enhance the adhesion of the asphalt to the aggregate.
[0048] (2) The modified nano-silica in the present invention can not only be closely adsorbed and bonded with the aggregate, but the modified introduced branched active groups can also react with the hydroxyl group, carboxyl group, unsaturated bond, etc. in the asphalt, so as to closely bond the interface between the asphalt and the aggregate, thereby improving the anti-stripping performance of the asphalt mixture; the soda lignin in the present invention can not only adjust the environmental pH together with the composite powder, but also improve the anti-aging ability of the asphalt, prevent the adhesion of the asphalt from decreasing after aging, and has good compatibility with asphalt, greatly improving the high-temperature stability of the asphalt mixture with little impact on the low-temperature performance.
[0049] (3) The tailings asphalt mixture obtained by using the asphalt anti-stripping agent of the present invention not only significantly enhances the water stability, but also improves the high temperature stability and low temperature crack resistance, comprehensively improves the road performance of the mixture, and all road performances meet the road pavement usage index requirements in the "Technical Specifications for Highway Asphalt Pavement Construction" (JTG F40-2004), promotes the comprehensive utilization of tailings solid waste, and also provides a good foundation for the subsequent application of tailings asphalt mixture. DETAILED DESCRIPTION
[0050] The technical solution of the present invention is further described below by way of examples, but these examples cannot limit the protection scope of the present invention, and the wt % involved is the mass fraction.
[0051] The experimental methods in the following examples, unless otherwise specified, are all conventional methods in the art. The experimental materials used in the following examples, unless otherwise specified, were purchased from conventional biochemical reagent stores.
[0052] The preparation method of the fatty alcohol polyoxyethylene ether phosphate used in the embodiments and comparative examples is as follows: under nitrogen protection, first add 3 parts of fatty alcohol polyoxyethylene ether AEO (the fatty alcohol used to synthesize fatty alcohol polyoxyethylene ether is isooctyl alcohol, and n is 6), add 1 part of P2O5 in batches while stirring, increase the temperature and continue stirring, and obtain fatty alcohol polyoxyethylene ether phosphate after hydrolysis, wherein the P2O5 batch addition time is 2h, the heating temperature is 80°C, the stirring time is 4h, the hydrolysis temperature is consistent with the reaction temperature, the hydrolysis time is 2h, and the amount of water added for hydrolysis is 4% of the total mass of all materials.
[0053] Example 1
[0054] (1) 6 parts of fatty alcohol polyoxyethylene ether phosphate and 3 parts of organosilane (a mixture of N-(2-N-benzylaminoethyl)-3-aminopropyltrimethoxysilane and dodecyltrimethoxysilane, wherein dodecyltrimethoxysilane accounts for 60 wt %) are mixed and stirred at 50° C. to obtain a prefabricated mixed solution.
[0055] (2) 100 parts of nano-silica and 5 parts of 3-glycidyloxypropylmethyldiethoxysilane (GPTMS) were mixed in anhydrous ethanol, heated under reflux at 110°C for 12 hours, and after the reaction, 6 parts of polyethyleneimine (PEI) with a molecular weight of 20,000 were added, and heated under reflux at 105°C for 24 hours. After the reaction, the mixture was filtered, washed, and dried at 100°C for 5 hours to obtain modified nano-silica for use.
[0056] (3) 100 parts of composite powder (including 50 parts of CaCO3 powder, 30 parts of Ca(OH)2 powder, and 20 parts of NaOH powder, respectively) and 60 parts of soda lignin (density 0.45 g / cm 3 , average particle size 35.6 μm, purity 80 wt%, ash content 7 wt%, water content 8.2 wt%, degradation temperature 260° C.), 20 parts of modified nano silicon dioxide are mixed evenly to obtain a prefabricated mixed powder.
[0057] (4) The prefabricated mixed liquid was evenly sprayed on the prefabricated mixed powder, and dried at 105° C. for 4 h to obtain the road asphalt anti-stripping agent A1.
[0058] Example 2
[0059] (1) 6 parts of fatty alcohol polyoxyethylene ether phosphate and 4 parts of organosilane (a mixture of N-(2-N-benzylaminoethyl)-3-aminopropyltrimethoxysilane and dodecyltrimethoxysilane, wherein dodecyltrimethoxysilane accounts for 60 wt %) are mixed and stirred at 50° C. to obtain a prefabricated mixed solution.
[0060] (2) 100 parts of nano-silica and 5 parts of GPTMS were mixed in anhydrous ethanol, heated under reflux at 106°C for 12 hours, and after the reaction, 6 parts of PEI with a molecular weight of 20,000 were added, and heated under reflux at 100°C for 24 hours. After the reaction, the mixture was filtered, washed, and dried at 100°C for 5 hours to obtain modified nano-silica for use.
[0061] (3) 100 parts of composite powder (including 50 parts of CaCO3 powder, 40 parts of Ca(OH)2 powder, and 10 parts of NaOH powder, respectively) and 65 parts of soda lignin (density 0.45 g / cm 3 , average particle size 35.6 μm, purity 80 wt%, ash content 7 wt%, water content 8.2 wt%, degradation temperature 280° C.), 25 parts of modified nano silicon dioxide are mixed evenly to obtain a prefabricated mixed powder.
[0062] (4) The prefabricated mixed liquid was evenly sprayed on the prefabricated mixed powder, and dried at 102° C. for 5 h to obtain the road asphalt anti-stripping agent A2.
[0063] Example 3
[0064] (1) 8 parts of fatty alcohol polyoxyethylene ether phosphate and 3 parts of organosilane (a mixture of N-(2-N-benzylaminoethyl)-3-aminopropyltrimethoxysilane and hexadecyltrimethoxysilane, wherein the hexadecyltrimethoxysilane accounts for 70 wt %) are mixed and stirred at 50° C. to obtain a prefabricated mixed solution.
[0065] (2) 100 parts of nano-silica and 6 parts of GPTMS were mixed in anhydrous ethanol, heated under reflux at 110°C for 12 hours, and after the reaction, 7 parts of PEI with a molecular weight of 20,000 were added, and heated under reflux at 106°C for 24 hours. After the reaction, the mixture was filtered, washed, and dried at 100°C for 5 hours to obtain modified nano-silica for use.
[0066] (3) 100 parts of composite powder (including 50 parts of CaCO3 powder, 40 parts of Ca(OH)2 powder, and 10 parts of NaOH powder, respectively) and 60 parts of soda lignin (density 0.45 g / cm 3 , average particle size 35.6 μm, purity 80 wt%, ash content 7 wt%, water content 8.2 wt%, degradation temperature 260° C.), 20 parts of modified nano silicon dioxide are mixed evenly to obtain a prefabricated mixed powder.
[0067] (4) The prefabricated mixed liquid was evenly sprayed on the prefabricated mixed powder, and dried at 105° C. for 4 h to obtain the road asphalt anti-stripping agent A3.
[0068] Example 4
[0069] (1) 8 parts of fatty alcohol polyoxyethylene ether phosphate and 3 parts of organosilane (a mixture of N-(2-N-benzylaminoethyl)-3-aminopropyltrimethoxysilane and hexadecyltrimethoxysilane, wherein the hexadecyltrimethoxysilane accounts for 70 wt %) are mixed and stirred at 55° C. to obtain a prefabricated mixed solution.
[0070] (2) 100 parts of nano-silica and 6 parts of GPTMS were mixed in anhydrous ethanol, and the mixture was heated under reflux at 108°C for 12 hours. After the reaction, 3 parts of PEI with a molecular weight of 20,000 and 4 parts of PEI with a molecular weight of 70,000 were added, and the mixture was heated under reflux at 100°C for 24 hours. After the reaction, the mixture was filtered, washed, and dried at 100°C for 5 hours to obtain modified nano-silica for use.
[0071] (3) 100 parts of composite powder (including 50 parts of CaCO3 powder, 40 parts of Ca(OH)2 powder, and 10 parts of NaOH powder, respectively) and 60 parts of soda lignin (density 0.45 g / cm 3 , average particle size 35.6 μm, purity 80 wt%, ash content 7 wt%, water content 8.2 wt%, degradation temperature 250° C.), 20 parts of modified nano silicon dioxide are mixed evenly to obtain a prefabricated mixed powder.
[0072] (4) The prefabricated mixed liquid was evenly sprayed on the prefabricated mixed powder, and dried at 110° C. for 4 h to obtain a road asphalt anti-stripping agent A4.
[0073] Example 5
[0074] (1) 6 parts of fatty alcohol polyoxyethylene ether phosphate and 3 parts of organosilane (a mixture of N-(2-N-benzylaminoethyl)-3-aminopropyltrimethoxysilane and hexadecyltrimethoxysilane, wherein the hexadecyltrimethoxysilane accounts for 60 wt %) are mixed and stirred at 50° C. to obtain a prefabricated mixed solution.
[0075] (2) 100 parts of nano-silica and 6 parts of GPTMS were mixed in anhydrous ethanol, and the mixture was heated under reflux at 110°C for 12 hours. After the reaction, 3 parts of PEI with a molecular weight of 20,000, 2 parts of PEI with a molecular weight of 1,000, and 2 parts of PEI with a molecular weight of 70,000 were added, and the mixture was heated under reflux at 105°C for 24 hours. After the reaction, the mixture was filtered, washed, and dried at 100°C for 5 hours to obtain modified nano-silica for use.
[0076] (3) 100 parts of composite powder (including 45 parts of CaCO3 powder, 40 parts of Ca(OH)2 powder, and 15 parts of NaOH powder, respectively) and 60 parts of soda lignin (density 0.45 g / cm 3 , average particle size 35.6 μm, purity 80 wt%, ash content 7 wt%, water content 8.2 wt%, degradation temperature 260° C.), 20 parts of modified nano silicon dioxide are mixed evenly to obtain a prefabricated mixed powder.
[0077] (4) The prefabricated mixed liquid was evenly sprayed on the prefabricated mixed powder, and dried at 105° C. for 4 h to obtain the road asphalt anti-stripping agent A5.
[0078] Comparative Example 1
[0079] The same as Example 1, except that no soda lignin was added during the preparation process, to obtain an anti-stripping agent B1.
[0080] Comparative Example 2
[0081] The same as Example 1, except that nano-silica is directly used instead of modified nano-silica in the preparation process to obtain anti-stripping agent B2.
[0082] Comparative Example 3
[0083] The same as Example 1, except that the preparation method of the modified nano-silica in the preparation process is as follows: 6 parts of the bionic material methacrylamide dopamine and 100 parts of nano-silica ethanol dispersion are mixed and stirred evenly for 5 minutes to obtain a mixture. After the reaction is completed, the mixture is filtered, washed, and dried at 100°C for 5 hours to obtain a modified nano-silica composite modifier for use, and finally an exfoliating agent B3 is obtained.
[0084] Comparative Example 4
[0085] The same as Example 1, except that the mixture of organic silane (N-(2-N-benzylaminoethyl)-3-aminopropyltrimethoxysilane and dodecyltrimethoxysilane) was not added during the preparation process, to obtain an anti-stripping agent B4.
[0086] Comparative Example 5
[0087] The same as Example 1, except that no fatty alcohol polyoxyethylene ether phosphate was added during the preparation process, to obtain an anti-stripping agent B5.
[0088] Comparative Example 6
[0089] The same as Example 1, except that vinyl triethoxysilane is used instead of fatty alcohol polyoxyethylene ether phosphate in the preparation process to obtain anti-stripping agent B6.
[0090] According to the method of use, the asphalt mixture anti-stripping agent of Examples 1 to 5 and Comparative Examples 1 to 6 was added to the mineral powder of the tailings aggregate asphalt mixture at a dosage of 40wt% (accounting for 40wt% of the mineral powder mass), and then the asphalt mixture was prepared. The coarse aggregate and fine aggregate in the iron tailings aggregate asphalt mixture are both iron ore waste rock, the mineral powder is tailings powder, the matrix asphalt is Qilu 70A asphalt, and the asphalt mixture grading type is AC-20. The road performance of the asphalt mixture was evaluated.
[0091] The road performance of asphalt mixture was tested in accordance with the (JTG E20-2011) "Test Procedure for Asphalt and Asphalt Mixture in Highway Engineering". The water stability was investigated by the water residual stability MS0 of the immersion Marshall test (T 0709-2011) and the freeze-thaw splitting strength ratio TSR of the freeze-thaw splitting test (T0729-2000). The high temperature stability was investigated by the dynamic stability of the rutting test (T0719-2011). The low temperature crack resistance was investigated by the flexural tensile strength and maximum flexural tensile strain of the low temperature bending test (T0715-2011). The results are shown in Table 1.
[0092] Table 1 Performance of asphalt mixtures prepared in Examples 1 to 5 and Comparative Examples 1 to 6
[0093]
[0094] Table 1
[0095]
[0096] It can be seen from the results in Table 1 that the tailings asphalt mixture prepared by the road asphalt anti-stripping agent prepared by the present invention has good water stability and high and low temperature performance, and various road performances meet the road pavement usage index requirements in (JTG F40-2004) "Technical Specifications for Highway Asphalt Pavement Construction".
Claims
1. A road asphalt anti-stripping agent, It is characterized in that By weight, it includes the following components: Composite powder: 100 parts; Fatty alcohol polyoxyethylene ether phosphate: 3 to 15 parts, preferably 5 to 10 parts; Soda lignin: 40-80 parts, preferably 60-75 parts; Organosilane: 2 to 8 parts, preferably 2 to 5 parts; Modified nano-silicon dioxide: 15 to 50 parts, preferably 20 to 40 parts.
2. The road asphalt anti-stripping agent according to claim 1, It is characterized in that The composite powder is CaCO 3 Powder, Ca(OH) 2 A mixture of at least two of powder and NaOH powder; the average particle size of the composite powder is 20 to 50 μm.
3. The road asphalt anti-stripping agent according to claim 1, It is characterized in that The composite powder is CaCO 3 Powder, Ca(OH) 2 powder and NaOH powder; based on the total mass of the composite powder, CaCO 3 Powder accounts for 30% to 50% of the total mass, Ca(OH) 2 The powder accounts for 30% to 40% of the total mass, and the NaOH powder accounts for 10% to 40% of the total mass.
4. The road asphalt anti-stripping agent according to claim 1, It is characterized in that The fatty alcohol polyoxyethylene ether phosphate has the general formula RO(CH 2 CH 2 O)nPO 3 H 2 , n is an integer from 3 to 9.
5. The road asphalt anti-stripping agent according to claim 1, It is characterized in that The properties of the soda lignin include: density of 0.3-0.5 g / cm 3 , average particle size of 25 to 40 μm, purity of not less than 70 wt%, ash content of not more than 8 wt%, water content of not more than 10 wt%, degradation temperature of 200 to 500 °C.
6. The road asphalt anti-stripping agent according to claim 1, It is characterized in that The organosilane is a mixture of aminosilane and long-chain organosilane, wherein the aminosilane accounts for 30% to 50% of the total mass of the organosilane, and the long-chain organosilane accounts for 50% to 70% of the total mass of the organosilane.
7. The road asphalt anti-stripping agent according to claim 6, It is characterized in that The aminosilane is one or more of N-(2-N-benzylaminoethyl)-3-aminopropyltrimethoxysilane, N-[[[2-(trimethoxysilyl)ethyl]phenyl]methyl]-1,2-ethylenediamine, N-(6-aminohexyl)aminomethyltriethoxysilane, 3-(4-ureaamino)propyltriethoxysilane, and N-(2-aminoethyl)-11-aminoundecyltrimethoxysilane; and / or the long-chain organosilane is one or more of dodecyltrimethoxysilane, dodecyltriethoxysilane, dodecylmethyldimethoxysilane, hexadecyltrimethoxysilane, and octadecyltrimethoxysilane.
8. The road asphalt anti-stripping agent according to claim 1, It is characterized in that The modified nano silicon dioxide comprises the following components by weight: Nano silicon dioxide: 100 parts; 3-glycidyloxypropylmethyldiethoxysilane: 3 to 8 parts, preferably 3 to 6 parts; Polyethyleneimine: 3 to 10 parts, preferably 5 to 8 parts.
9. A method for preparing the road asphalt anti-stripping agent according to any one of claims 1 to 8, It is characterized in that The preparation method comprises: (1) uniformly mixing fatty alcohol polyoxyethylene ether phosphate and organosilane to prepare a prefabricated mixed solution; (2) preparing modified nano-silicon dioxide; (3) mixing the composite powder, soda lignin, and modified nano-silica uniformly to obtain a prefabricated mixed powder; (4) The prefabricated mixed liquid obtained in step (1) is evenly sprayed on the prefabricated mixed powder obtained in step (3), and dried to obtain an asphalt anti-stripping agent.
10. The preparation method according to claim 9, It is characterized in that In step (1), the mixing temperature of the fatty alcohol polyoxyethylene ether phosphate and the organosilane is 45-65°C.
11. The preparation method according to claim 9, It is characterized in that In step (2), the method for preparing modified nano-silicon dioxide is as follows: The nano-silica and 3-glycidyloxypropylmethyldiethoxysilane are mixed in anhydrous ethanol, reacted under a first heating reflux condition, polyethyleneimine is added after the reaction is completed, reacted under a second heating reflux condition, filtered, washed and dried after cooling to obtain modified nano-silica.
12. The preparation method according to claim 11, It is characterized in that The reaction temperature of the first heating reflux is 90°C to 130°C, preferably 100°C to 115°C, and the time is 12 to 18 hours, and / or the reaction temperature of the second heating reflux is 90°C to 120°C, preferably 95°C to 110°C, and the time is 20 to 24 hours; preferably, the first reflux temperature is 3 to 10°C higher than the second reflux temperature.
13. The preparation method according to claim 9, It is characterized in that In step (4), the drying temperature is 95 to 110° C., and the drying time is 2 to 5 hours.
14. Use of the road asphalt anti-stripping agent according to any one of claims 1 to 8 or the road asphalt anti-stripping agent prepared according to any one of claims 9 to 13 in asphalt mixture.
15. The use according to claim 14, It is characterized in that The application includes: adding the road asphalt anti-stripping agent into the mineral powder of tailings aggregate asphalt mixture, wherein the amount of the road asphalt anti-stripping agent added accounts for 30wt% to 50wt% of the mineral powder mass, the coarse aggregate and the fine aggregate in the tailings aggregate asphalt mixture are both iron ore waste rock, and the mineral powder is iron tailings powder after magnetic separation.
Citation Information
Patent Citations
Cationic pitch warm mixing agent and preparation method thereof
CN104559248A
Biomimetic material-containing asphalt anti-stripping agent and asphalt preparation method based on same
CN113652000A
Micron-sized anti-stripping agent for acidic aggregate asphalt mixture and use method of micron-sized anti-stripping agent
CN114133154A
Closed-water thin-layer asphalt mixture as well as preparation method and use method thereof
CN115180874A