Muck-based geopolymer as well as preparation method and application thereof

By combining slag and slag with water glass and water, using alkali trigger and retarder water reducer, a slag base polymer with high compressive strength was prepared, which solved the existing slag preparation without burning bricks. The problems of insufficient intensity and high energy consumption have achieved efficient and environmentally friendly waste resource utilization.

CN119080444APending Publication Date: 2024-12-06SHENZHEN UNIV
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411187561.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-28
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

The 28-d compressive strength of the existing slag preparation bricks is not high enough, and the calcination process consumes high energy, which emits greenhouse gases and toxic gases.

Method used

Using a combination of solid waste (slag and slag) with water glass and water, the release of silicon-aluminum monomers is promoted through alkali exciters, forming a hydrated calcium aluminosilicate and sodium aluminosilicate gel, combined with a retarder and water reducing agent, pour or pressure forming to prepare slag base polymer to improve compressive strength.

Benefits of technology

The 28d compressive strength of the slag base polymer has been achieved above 17.67MPa, energy saving and emission reduction, CO2 emissions and energy consumption are reduced, process flow is simplified, and solid waste utilization is improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119080444A_ABST
    Figure CN119080444A_ABST
Patent Text Reader

Abstract

The invention provides a muck-based geopolymer as well as a preparation method and application thereof, and relates to the technical field of resource utilization of building materials. The muck-based geopolymer provided by the invention is prepared from the following raw materials: waste slag, water glass and water, and water; the waste slag charge comprises engineering muck and slag, and the mass content of the engineering muck in the waste slag charge is smaller than or equal to 70%; the mass of Na2O in the water glass accounts for 1.5-7% of the mass of the waste slag; the total mass of the water in the preparation raw materials accounts for 30-45% of the mass of the waste slag. The unfired, energy-saving, environment-friendly and high-strength muck-based geopolymer is prepared by taking engineering muck and slag as gel materials and utilizing an alkali excitation technology and reasonably controlling the proportion. A large number of different types of solid wastes are consumed, and meanwhile a large number of natural resources are saved. The muck-based geopolymer has the characteristics of high strength, low consumption of the alkali activator, low carbon, emission reduction and the like.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of resource utilization of building materials, and in particular to a slag base polymer and a preparation method and application thereof. Background Art

[0003] Geopolymers are inorganic materials produced by alkali activation of aluminosilicates, and solid waste (such as fly ash and blast furnace slag) can be used as aluminosilicate raw materials in large quantities. Therefore, the use of geopolymers instead of traditional binders (such as cement and lime) has significant environmental advantages, especially in terms of production energy consumption and greenhouse gas emissions. It has been found that the use of geopolymer concrete as a substitute for traditional Portland cement concrete can reduce carbon content by up to 80%. In terms of mechanical properties and durability, geopolymers can achieve comparable or superior performance to traditional binders or concretes while reducing the environmental footprint. The trend of strengthening sustainable practices in the construction industry has promoted research in this field.

[0004] The technology of utilizing slag mainly involves calcining slag and mixing it with an alkali activator and other additives to obtain a slag-based polymer. For example, Chinese patents CN113121157A, CN111454011A, and CN109776031A disclose methods of preparing slag-based polymers by calcining slag, which consumes a lot of energy and emits a large amount of room temperature gas.

[0005] Jiang Chaohua et al. (Jiang Chaohua, Pan Yuepeng, Leng Jie, et al. Experimental study on preparation of unburned bricks from sandy waste soil [J]. Bulletin of the Chinese Ceramic Society. 2015, 34(11): 3116-21.) used engineering sandy waste soil as the main raw material and prepared unburned bricks by vibration molding. They studied the effects of different mix ratios of inorganic binders such as cement, fly ash, gypsum and lime on the performance of unburned bricks from sandy waste soil. The optimal mix ratio of unburned bricks from sandy waste soil was: 72% sandy waste soil, 16% cement, 8% fly ash, 2% gypsum, 2% lime and 0.5% water reducer. The optimal mix ratio had a 28d compressive strength of 15.8 MPa. This existing technology uses unburned technology to save energy and does not produce greenhouse gases, SO2 and other toxic gases to pollute the air. However, the 28d compressive strength of the unburned bricks prepared from the above-mentioned sandy waste soil is only 15.8 MPa at most, which is not high enough. Summary of the invention

[0006] In view of this, the object of the present invention is to provide a slag-based polymer and a preparation method and application thereof. The slag-based polymer provided by the present invention has a 28d compressive strength of more than 17.67 MPa and has high compressive strength.

[0007] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:

[0008] The invention provides a slag-based polymer, wherein the raw materials for preparing the polymer are solid waste, water glass and water; the solid waste comprises slag and slag, the mass content of slag in the solid waste is ≤70%; the mass of Na2O in the water glass accounts for 1.5-7% of the mass of the solid waste; and the total mass of water in the raw materials for preparing the polymer accounts for 35-45% of the mass of the solid waste.

[0009] Preferably, the particle size of the slag is ≥80 mesh.

[0010] Preferably, the particle size of the slag is 50 to 1000 nm.

[0011] Preferably, the modulus of the water glass is 1.5 to 3.5.

[0012] Preferably, the raw materials for preparation further include admixtures; the admixtures are retarders and water reducers;

[0013] The mass of the admixture accounts for 0.4-1% of the mass of the solid waste.

[0014] Preferably, the retarder includes BNE-7602;

[0015] The water reducing agent includes one or more of ceramic water reducing agent mother liquor, BNE-7702, anti-mud water reducing agent, Sika Stabilizer-412MBF, SK 181, ASA300, 530P, 556P, 540P and 325C.

[0016] The present invention provides a method for preparing a slag-based polymer according to the technical solution, comprising the following steps: mixing the raw materials for preparation, performing molding and curing to obtain the slag-based polymer; the molding comprises casting molding or pressure molding.

[0017] Preferably, when the preparation of raw materials also includes an admixture, the mixing includes: mixing a retarder with part of the water to obtain a retarder solution; mixing a water reducer with the remaining water to obtain a water reducer solution; stirring the solid waste at a low speed of 30 to 60 r / min for 1 to 2 min, then adding the retarder solution and water glass, stirring at a low speed of 30 to 60 r / min for 1 to 2 min, then standing for 2 to 5 min, adding the water reducer solution, and stirring at a high speed of 100 to 150 r / min for 1 to 3 min.

[0018] Preferably, the pressure of the pressure forming is 1 to 5 tons.

[0019] The present invention also provides the use of the slag-based polymer described in the above technical solution or the slag-based polymer prepared by the preparation method described in the above technical solution as a building material.

[0020] The present invention provides a slag-based polymer, the preparation raw materials are solid waste, water glass and water; the solid waste includes slag and slag, the mass content of slag in the solid waste is ≤70%; the mass of Na2O in the water glass accounts for 1.5-7% of the mass of solid waste; the total mass of water in the preparation raw materials accounts for 30-45% of the mass of solid waste. In the present invention, water is mainly used as a reaction medium in the preparation process of the slag-based geopolymer, and participates in the dissolution and gel formation process of solid waste. Under the action of the alkaline activator water glass, the slag quickly releases silicon aluminum monomers and calcium ions, which are conducive to the formation of hydrated calcium aluminosilicate gel, one of the main products of the geopolymer, and then solidifies to form a polymer with a three-dimensional network structure, providing effective guarantee for the strength of the geopolymer. Under the action of the alkaline activator water glass, the slag releases part of the active silicon aluminum monomers, and the calcium ions dissolved from the slag are conducive to the further excitation of the slag, especially the kaolin component in the slag, which is conducive to the formation of hydrated sodium aluminosilicate gel, one of the main products of the geopolymer. In addition, geopolymers with high slag content have poor volume stability and are prone to microcracks that affect strength; while slag particles react slowly in the early stage and can effectively fill pores, which can alleviate the volume mismatch problem caused by the rapid early reaction of slag and help improve the compressive strength of geopolymers. Moreover, the slag-based polymer provided by the present invention does not require calcining of slag, making the preparation process of slag-based polymers more energy-saving and emission-reducing, the operation process is simple, and the problem of waste slag utilization can be solved more efficiently. Slag and slag are both solid wastes. While fully utilizing solid wastes, they also save other national resources, which is beneficial to environmental protection and green development. As shown in the test results of the embodiment, when the mass content of slag in the solid waste is ≤70%, the 28d compressive strength of the slag-based polymer is 17.67~103.17MPa, and the compressive strength of the slag-based polymer is high.

[0021] Furthermore, the present invention uses a combination of a retarder and a water reducer. The retarder is first used to increase the adsorption of ions / dimers on the surface of solid waste particles. After the surface of the solid waste particles is fully adsorbed, the functional groups on the surface of the water reducer are used to adsorb the charged raw materials and the solid waste particles in the reaction, thereby releasing water molecules, thereby improving the workability of the geopolymer slurry under the condition of high slag content. On the basis of ensuring fluidity, the amount of water is reduced, thereby optimizing the pore structure of the hardened test block and improving the compressive strength of the slag base polymer.

[0022] The present invention provides a method for preparing the slag-based polymer described in the above technical solution, comprising the following steps: mixing the raw materials for preparation, performing molding and curing to obtain the slag-based polymer; the molding includes casting molding or pressure molding. The preparation method provided by the present invention does not need to calcine the slag, and the preparation process of the slag-based polymer is more energy-saving and emission-reducing, the operation process is simple, and the problem of the utilization of waste slag can be solved more efficiently. Compared with the traditional cement production process that requires the calcination of limestone, consumes a lot of energy and releases a lot of carbon dioxide, the present invention only produces a small amount of carbon dioxide in the production process of water glass. The preparation method provided by the present invention has low energy consumption, simple operation, high utilization rate of solid waste (slag and slag), and the production cost is suitable for industrial production. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1 The dried, ground and sieved slag used in Example 1;

[0024] Figure 2 This is the SEM image of the slag in Example 1;

[0025] Figure 3 This is the SEM image of the slag in Example 1;

[0026] Figure 4 TEM image of the slag in Example 1;

[0027] Figure 5 TEM image of the slag in Example 1;

[0028] Figure 6 This is the SEM image of the slag base polymer at 3d age in Example 1;

[0029] Figure 7 This is the SEM image of the slag base polymer at 7 days of age in Example 1;

[0030] Figure 8 This is the SEM image of the slag base polymer at 28 days of age in Example 1;

[0031] Fig. 9 The pressure forming die and 30-ton electric powder tablet press (Hengchuang YPD-30S) used in the examples;

[0032] Fig.10 The XRD patterns of the slag base polymer at different ages (3d, 7d and 28d) in Example 1;

[0033] Fig.11 This is the scanning electron microscope-energy dispersive spectrometer result diagram of the slag base polymer at 28 days of age in Example 1;

[0034] Fig.12The slag (left picture) and slag (right picture) in Example 1 29 Si NMR spectrum;

[0035] Fig.13 is the 3d and 28d age of the slag-based polymer in Example 1 29 Si NMR spectrum;

[0036] Fig.14 The slag (left picture) and slag (right picture) in Example 1 27 Al NMR spectrum;

[0037] Fig.15 is the 3d and 28d age of the slag-based polymer in Example 1 27 Al NMR spectrum;

[0038] Fig.16 is the slag in Example 1 29 Si NMR and 27 Peak fitting results of Al NMR spectrum;

[0039] Fig.17 is the slag in Example 1 29 Si NMR and 27 Peak fitting results of Al NMR spectrum;

[0040] Fig.18 is the 3d age of the slag-based polymer in Example 1 29 Si NMR and 27 Peak fitting results of Al NMR spectrum;

[0041] Fig.19 is the 7d-old age of the slag-based polymer in Example 1 29 Si NMR and 27 Peak fitting results of Al NMR spectrum;

[0042] Fig. 20 is the 28d age of the slag-based polymer in Example 1 29 Si NMR and 27 Peak fitting results of Al NMR spectrum;

[0043] Fig.21 The compressive strength test results of the slag base polymers with different water-to-solid ratios prepared in Examples 1 to 5;

[0044] Fig. 22 The compressive strength test results of the slag-based polymers prepared in Comparative Example 2 and Examples 6 to 9 with different slag blending ratios are shown;

[0045] Fig.23The compressive strength test results of the slag-based polymers with different alkali contents prepared in Examples 10 to 14;

[0046] Fig.24 The compressive strength test results of the slag-based polymers with different alkali contents prepared in Examples 15 to 17;

[0047] Fig.25 The compressive strength test results of the slag-based polymers with and without admixtures prepared in Examples 19 to 20;

[0048] Fig.26 A comparison chart of the fluidity of the geopolymer slurry prepared in Example 18 (without adding a retarder and a water reducer) and Example 21 (adding a retarder and a water reducer at the same time);

[0049] Fig. 27 These are images of the slag-based polymer prepared using sodium hydroxide as the alkaline activator in Comparative Example 1 (upper image) and the polymer directly crushed after being compressed (lower image). DETAILED DESCRIPTION

[0050] The invention provides a slag-based polymer, the preparation raw materials of which are solid waste, water glass and water (referred to as added water).

[0051] Unless otherwise specified, the materials and equipment used in the present invention are all commercially available products in the art.

[0052] In the present invention, the solid waste includes muck and slag.

[0053] In the present invention, the main chemical components of the slag preferably include 53.55-59.60wt% SiO2 and 31.25-36.20wt% Al2O3, wherein the content of active SiO2 is preferably 18.30-22.30wt%; the particle size of the slag is preferably ≥80 mesh. In a specific embodiment of the present invention, the slag comes from the work site of underground engineering excavation, and most of the sand particles are removed after screening, and then dried, crushed, finely ground and sieved through an 80-mesh sieve to ensure the consistency and representativeness of the slag. The slag has a certain activity under the action of an alkali activator, so that it can play the role of filler and gel material after adding an alkali activator and slag.

[0054] In the present invention, the mass content of slag in the solid waste (i.e. the amount of slag added) is ≤70%, more preferably 0.5-70%, further preferably 1-60%, specifically 5%, 10%, 15%, 20%, 25%, 30%, 35%, 40%, 45%, 50%, 55%, 60%, 65%, 68% or 70%.

[0055] In the present invention, the particle size of the slag is preferably 50 to 1000 nm, more preferably 100 to 800 nm, and further preferably 300 to 500 nm; the main chemical components of the slag preferably include 38.40 to 40.84 wt% of CaO, 29.69 to 31.61 wt% of SiO2, and 15.91 to 17.86 wt% of Al2O3; the strength grade of the slag is preferably S95; the density of the slag is preferably 2.5 g / cm 3 ; The slag preferably includes blast furnace slag. The quality of the slag used in the present invention meets the requirements of GB / T18046-2008. Slag is a by-product of the blast furnace ironmaking process. The ground granular blast furnace slag is more similar to the chemical composition of ordinary cement than other mineral admixtures. The higher and finer glass and particle content enhances the reactivity of the mixture, thereby accelerating the polymerization process, and can effectively improve the mechanical properties of slag-based polymers and reduce the setting time of geopolymers; the amount of slag added plays a very critical role in the compressive strength of the sample. As the slag content increases, the strength of the sample will gradually increase. When used for building materials, the strength is required to be above 10MPa. The present invention explores the proportion of the minimum slag added to achieve the strength requirements, so as to achieve the purpose of absorbing a large amount of slag.

[0056] The present invention uses slag and slag as the main raw materials, utilizes alkali activation technology and reasonably controls the proportion to prepare a slag-based polymer that is free of burning, energy-saving and environmentally friendly. On the one hand, it consumes a large number of different types of solid waste, and on the other hand, it also saves a large number of natural resources. The slag-based polymer provided by the present invention has the characteristics of high strength, small amount of alkali activator, low carbon emission reduction, etc. When slag is added by 50%, compared with cement, CO2 emissions are reduced by 60.42%, energy consumption is reduced by 52.85%, and preparation costs are reduced by 77.05%.

[0057] In the present invention, the mass of Na2O in the water glass accounts for 1.5-7% of the mass of solid waste (recorded as alkali content), preferably 2-6.5%, more preferably 2.5-6%, further preferably 3-5%, and most preferably 3-4%. In the present invention, the modulus of the water glass (sodium silicate aqueous solution) is preferably 1.5-3.5, more preferably 2-3, further preferably 2-2.5; the density of the water glass is preferably 1.44 g / cm 3. In the preparation process of the slag-based polymer of the present invention, the changes in the SiO2 and Na2O contents in the water glass have a significant effect on the alkali excitation effect of the slag-based polymer. The silicate in the water glass and the aluminosilicate generated by the excited slag are adsorbed on the surface of the mineral particles, fill the ends of the crystals, and undergo polycondensation reactions in an alkaline environment to form a block-like dense structure, thereby improving the strength and durability of the geopolymer. The alkali activator can promote the dissolution of silicon and aluminum elements in the aluminosilicate raw materials and gradually polymerize to form the main products of the geopolymer, such as hydrated calcium aluminosilicate and hydrated sodium aluminosilicate.

[0058] In the present invention, the total mass of water (water in water glass and added water) in the raw materials for preparing the slag-based polymer accounts for 30-45% of the mass of solid waste (i.e., the water-to-solid ratio is 0.3-0.45), preferably 35-42%, more preferably 38-40%, and specifically preferably 30%, 31%, 32%, 33%, 34%, 35%, 36%, 37%, 38%, 39%, 40%, 41%, 42%, 43%, 44% or 45%. Water is mainly used as a reaction medium in the preparation process of geopolymer, and participates in the dissolution and gel formation process of geopolymer raw materials. However, water is completely discharged after the reaction is completed, and the geopolymer finally forms a three-dimensional network structure without water or with little water. The water-to-solid ratio in the raw materials for preparing the slag-based polymer provided by the present invention can be as low as 0.3. Due to the reduction in the amount of added water, the pores formed in the material after the water evaporates are relatively small, which is beneficial to improving the compressive strength of the material.

[0059] In the present invention, the raw materials for preparing the landfill base polymer preferably also include an admixture, and the mass of the admixture preferably accounts for 0.4-1% of the mass of solid waste, more preferably 0.5-0.8%, and further preferably 0.6-0.7%. In the present invention, the admixture preferably includes a retarder and a water reducer; the mass of the retarder preferably accounts for 0.1-0.4% of the mass of solid waste, more preferably 0.15-0.35%, and further preferably 0.2-0.3%; the mass of the water reducer preferably accounts for 0.3-0.6% of the mass of solid waste, more preferably 0.4-0.6%, and further preferably 0.5-0.6%. In the present invention, the retarder preferably includes BNE-7602 (Beijing Bono New Materials Technology Co., Ltd.). In the present invention, the water reducer preferably includes one or more of ceramic water reducer mother liquor, BNE-7702, anti-mud water reducer, Sika Stabilizer-412MBF, SK181, ASA300, 530P, 556P, 540P and 325C; the mass concentration of the ceramic water reducer mother liquor is preferably 30-50%, more preferably 35-45%, and further preferably 40%. The slow setting used in the present invention is to make the surface of solid waste particles adsorb more ions, so that the water reducer can better play its role. The present invention uses a combination of a retarder and a water reducer. The retarder is first used to increase the adsorption of ions / dimers on the surface of solid waste particles. After the surface of the solid waste particles is fully adsorbed, the functional groups on the surface of the water reducer are used to adsorb charged raw materials and solid waste particles in reaction, thereby releasing water molecules, thereby improving the workability of the geopolymer slurry under the condition of high slag content. Under the premise of ensuring the fluidity of the geopolymer slurry, the amount of water is reduced, thereby optimizing the pore structure of the hardened test block and improving the compressive strength of the slag base polymer.

[0060] Under the action of the alkaline activator water glass, the slag quickly releases silicon-aluminum monomers and calcium ions, which contribute to the formation of calcium silicate gel, one of the main products of the geopolymer, and then solidifies to form a polymer with a three-dimensional network structure, providing effective protection for the strength of the geopolymer. Under the action of the alkaline activator water glass, the slag releases some active silicon-aluminum monomers, and at the same time, the calcium ions dissolved from the slag are conducive to the further excitation of the slag, especially the kaolin component in the slag, which contributes to the formation of sodium silicate gel, one of the main products of the geopolymer. In addition, the volume stability of geopolymers with high slag content is poor, and microcracks are easily generated to affect the strength; while the slag particles react slowly in the early stage, can effectively fill the pores, can alleviate the volume mismatch problem caused by the rapid reaction of the slag in the early stage, and help to improve the compressive strength of the geopolymer. The slag that has not been activated by alkali has low activity itself. In an alkaline environment, the present invention can achieve that even if only a small amount (30%) of slag and a large amount (70%) of slag are added, the 28d compressive strength of the slag base polymer can reach 17.67MPa.

[0061] The present invention provides a method for preparing a slag-based polymer according to the technical solution, comprising the following steps: mixing the raw materials for preparation, performing molding and curing to obtain the slag-based polymer; the molding comprises casting molding or pressure molding.

[0062] In the present invention, the soil is preferably dried, crushed, finely ground and sieved in sequence before use. The present invention has no special limitation on the drying, crushing and finely grinding, and the drying, crushing and finely grinding operations well known to those skilled in the art can be used. In the present invention, the sieving is preferably a standard sample sieve of 80 mesh.

[0063] In the present invention, when the preparation raw materials are solid waste, water glass and water, the mixing preferably includes: stirring the slag and slag at a low speed of 30 to 60 r / min (more preferably 45 to 50 r / min) for 1 to 2 min (more preferably 1 to 1.5 min), then adding water glass and water, and stirring at a high speed of 100 to 150 r / min (more preferably 120 to 130 r / min) for 1 to 3 min (more preferably 1.5 to 2 min) to obtain a geopolymer slurry.

[0064] In the present invention, when the raw materials for preparation further include a retarder and a water reducer, the mixing preferably includes: mixing the retarder with part of the water to obtain a retarder solution; mixing the water reducer with the remaining water (excluding the water in the water glass) to obtain a water reducer solution; stirring the solid waste at a low speed of 30 to 60 r / min (more preferably 45 to 50 r / min) for 1 to 2 min (more preferably 1 to 1.5 min), then adding the retarder solution and water glass, stirring at a low speed of 30 to 60 r / min (more preferably 45 to 50 r / min) for 1 to 2 min (more preferably 1 to 1.5 min), then standing for 2 to 5 min (more preferably 3 to 4 min), adding the water reducer solution, and stirring at a high speed of 100 to 150 r / min (more preferably 120 to 130 r / min) for 1 to 3 min (more preferably 1.5 to 2 min) to obtain a geopolymer slurry. In the present invention, the mass of the partial water is preferably 1 / 3 to 1, more preferably 2 / 3, of the total mass of the added water; the mass of the remaining water is preferably 1 / 5 to 2 / 5, more preferably 1 / 3, of the total mass of the added water.

[0065] In the present invention, the casting molding preferably includes: injecting the mixed geopolymer slurry into a mold, vibrating, sealing with plastic wrap, and demolding after static molding to obtain a slag-based polymer gel. In the present invention, the mold is preferably cleaned before use, tape is pasted on the contact surface, and a release agent is applied to the mold wall to facilitate demolding of the slag-based polymer gel. In the present invention, the mold is preferably placed on a vibrating table first, and then the geopolymer slurry is preferably injected into the mold in layers; the injection is vibrated at the same time, and then vibrated until the surface of the sample in the mold is flat and smooth. The present invention is sealed with plastic wrap to prevent the surface of the slag-based polymer gel from drying and shrinking due to water evaporation, resulting in cracks. In the present invention, the temperature of the static molding is preferably 25±2°C, the relative humidity is preferably 92-98%, more preferably 94-95%, and the time is preferably 23-25h, more preferably 24h.

[0066] In the present invention, the pressure of the pressure molding is preferably 1 to 5 tons, more preferably 2 to 3 tons; the pressure molding preferably includes: placing the mixed geopolymer slurry in a steel mold, covering it with a lid, using a press to perform pressure molding and then demolding to obtain a slag-based polymer gel. In the present invention, a release agent is brushed on all inner walls of the steel mold before use to facilitate demolding. The present invention controls the compression ratio by controlling the pressure of the pressure molding, thereby ensuring the consistency of the slag-based polymer gel; when the compression molding method is adopted, the water-solid ratio can be reduced to 0.3, and due to the reduction in the amount of added water, the pores formed in the material after the water evaporates are relatively small; the pressing process enhances the structural compactness of the material, which is beneficial to improve the compressive strength of the material.

[0067] In the present invention, the curing temperature is preferably 25±2° C., the relative humidity is preferably 92-98%, more preferably 94-95%, and the curing time is preferably 1-28 days, more preferably 2 days, 6 days or 27 days.

[0068] The present invention also provides the use of the slag-based polymer described in the above technical solution or the slag-based polymer prepared by the preparation method described in the above technical solution as a building material.

[0069] In order to further illustrate the present invention, a landfill base polymer provided by the present invention and its preparation method and application are described in detail below in conjunction with embodiments, but they should not be construed as limiting the scope of protection of the present invention.

[0070] In the following examples and comparative examples, the slag cakes were obtained from the work site of underground engineering excavation. The slag cakes were dried at 60°C, ground with a grinding machine, and then passed through a standard 80-mesh sieve. Figure 1 As shown, the slag under the sieve is used, and the main chemical components of the slag are 56.65wt% SiO2 and 33.15wt% Al2O3. The slag is selected from Guangdong Shaoguan Iron and Steel Company, with a strength grade of S95 and a density of 2.5g / cm 3 , the quality meets the requirements of GB / T18046-2008, the particle size is 50-1000nm, and the main chemical components include 39.84wt% CaO, 30.61wt% SiO2 and 16.91wt% Al2O3. The amount of slag added (the proportion of slag added) = the mass of slag / (the mass of slag + the mass of slag) × 100%; the water-solid ratio = (the mass of water in water glass + the mass of added water) / (the mass of slag + the mass of slag); the amount of alkali = the mass of Na2O in water glass / (the mass of slag + the mass of slag) × 100%; the amount of water reducer = the mass of water reducer / (the mass of slag + the mass of slag) × 100%; the amount of retarder = the mass of retarder / (the mass of slag + the mass of slag) × 100%. The pressure forming mold and the 30-ton electric powder tablet press (Hengchuang YPD-30S) are shown in Fig. 9 . Figure 2-3 and Figure 6 to Figure 8 The text information on the medium magnification is very small, but it does not affect the expression of the technical effect.

[0071] Example 1

[0072] (1) Preparation of geopolymer slurry: Add slag and slag into a slurry mixer, stir at a low speed of 45 r / min for 1 min, add water glass and water, stir at a high speed of 120 r / min for 2 min, and obtain geopolymer slurry. The proportion of each raw material of the geopolymer slurry to the total mass of slag and slag is shown in Table 1.

[0073] (2) Casting and curing: The geopolymer slurry is layered and injected into a 40mm×40mm×40mm cube triple mold and a 40mm×40mm×160mm rectangular triple mold placed on a vibrating table. The slurry is vibrated while being injected until the surface of the sample in the mold is flat and smooth. The sample is sealed with plastic wrap and stored. The sample is placed in a constant temperature and humidity curing box and allowed to stand for 24 hours for molding and demolding to obtain a slag-based polymer gel. The slag-based polymer gel is cured in the above-mentioned constant temperature and humidity box for 2d, 6d and 27d to obtain slag-based polymers of different ages (3d, 7d and 28d). Before using the cube triple mold and the rectangular triple mold, tape is pasted on the contact surface, and a release agent is applied to the mold wall to facilitate demolding. The constant temperature and humidity are 25±2℃, and the relative humidity is 95%.

[0074] Figure 2 This is the SEM image of the slag in Example 1. Figure 3 From the SEM image of the slag in Example 1, it can be seen that the surface morphology of the slag particles is relatively rough, mainly stacked flaky structures, and there are irregular microscopic gaps and protrusions between the particles. At the same time, it can be observed that the slag has a large number of agglomerates, and there are particles surrounding it. A large number of agglomerates are arranged in a non-directional manner. The agglomerates are mainly generated in the form of edge-face and face-face, with relatively loose contact, and the outer particles also have no obvious directional distribution pattern. The surface morphology of the slag raw material is flat, and it is block-like particles, which is an amorphous glass body.

[0075] Figure 4 This is the TEM image of the slag in Example 1. Figure 5 This is the TEM image of the slag in Example 1. It can be seen that there are a large number of flocculent and rod-like structures in the slag, and some samples are interspersed with high-density needle-like substances. At the same time, the diffraction pattern of the slag shows a diffusely scattered halo, showing the characteristics of an amorphous electron diffraction pattern, in which the diffraction ring radius is similar, while the slag raw material is a flaky structure.

[0076] Figure 6 This is the SEM image of the 3d-age polymer of the slag base in Example 1. Figure 7 This is the SEM image of the slag base polymer at 7 days of age in Example 1. Figure 8 This is the SEM image of the slag base polymer at 28 days of age in Example 1. Figure 6 to Figure 8 It can be seen that the microstructure of the slag base polymer in Example 1 shows a certain degree of roughness, but the bonding between its particles is tighter than that of the unactivated slag. The gelation of the geopolymer is not just to simply contact the slag sheet units with each other, but to make them tightly combined through cementation, and the generated gel covers and connects the scattered sheet units of the slag.

[0077] Fig.10The XRD patterns of the slag-based polymer at different ages (3d, 7d and 28d) in Example 1 show that under the influence of the activator, the slag-based polymer in Example 1 exhibits a slight chemical reaction, resulting in the gradual weakening of the characteristic peak of kaolinite in the system, while the quartz component still dominates. Compared with the raw material, the characteristic peak observed at 2θ=12.32° of the slag-based polymer after alkali activation treatment appears to be broader, and this change indicates the formation of the unique diffraction peak of the amorphous geopolymer. The peak height at 2θ=6.10° of the 7-day-old sample increased significantly compared to that at 3 days, indicating that a large amount of new hydration products were generated at this stage. In addition, the intensity of the quartz peak at 2θ=26.63° decreased significantly, which may be attributed to the increase in the content of amorphous products, which reduced the volume proportion of quartz, resulting in a weakening of the quartz peak intensity.

[0078] Fig.11 The results of scanning electron microscope-energy dispersive spectrometer (SEM-EDS) of the slag-based polymer in Example 1 at 28 days of age are shown in Figure 1. SEM can obtain the microscopic morphology of the geopolymer, and combined with EDS, the quantitative results of the micro-area element content can be obtained. The quantitative results are presented in the form of a pie chart. The SEM-EDS results show that the Ca / Si ratio of the slag-based polymer in Example 1 is very high, which indicates that more calcium is dissolved from the slag and participates in the reaction. It can be seen that the hydration product of the slag-based polymer is mainly a dense CASH gel, and the content of the Fe element at each point at 28 days has dropped significantly, and Fe may be consumed in the reaction.

[0079] Fig.12 The slag (left) and slag (right) in Example 1 29 From the Si NMR spectrum, we can see that a sharp resonance peak is observed at -91ppm for the slag raw material; the main characteristic peak of the NMR spectrum of slag is a diffuse broad peak, appearing in the -60 to -80ppm region. The broad peak usually indicates that the silicon atom environment in the sample is more diverse or uneven, indicating that the silicon phase in the slag is an active silicon-oxygen tetrahedral structure.

[0080] Fig.13 is the 3d and 28d age of the slag-based polymer in Example 1 29Si NMR spectrum, it can be seen that in the reactants in Example 1, the peak height corresponding to the slag decreases rapidly, while a sharp peak still appears at -91ppm. This may be due to the low activity of the tetrahedral silicon (Q4) site in the slag soil and the fact that it did not participate in the reaction in the early stage. Overall, the slag participated in the reaction in large quantities at the age of 3 days, forming a CASH gel with a relatively uniform structure. However, in the sample at the age of 28 days, the height and area of ​​the peak at the chemical shift of -91ppm decreased during the reaction, which may be due to the dissolution of more silicon sources (such as kaolin and quartz) and the participation in the gel formation reaction. With the increase of curing time, the main band continued to move to a higher chemical shift, and the relative intensity of the peak in the -60ppm to -70ppm region decreased significantly. This shows that the breaking of most of the Si-O-Si and Al-O-Al bonds in the raw materials is conducive to the next step of polycondensation reaction to form more polymer products. From 7 days to 28 days, the curve only moved slightly, indicating that a stable Si coordination environment was formed.

[0081] Fig.14 The slag (left) and slag (right) in Example 1 27 From the AlNMR spectrum, we can see that the slag spectrum is a broad peak appearing in the 80-20ppm region. The position of this peak may indicate tetrahedrally coordinated aluminum (AlO4), but this peak is wider and has a different shape than the corresponding peak in the NMR spectrum of the slag raw material, indicating that this raw material may contain a certain degree of structural disorder or coordination diversity, indicating that the aluminum element participates in the formation of the aluminosilicate network in the form of AlO4, which is one of the unique structural characteristics of NASH gel.

[0082] Fig.15 is the 3d and 28d age of the slag-based polymer in Example 1 27 From the AlNMR spectrum, it can be seen that the sharpness of the broad peak corresponding to the slag raw material increases, but when comparing the spectra of 3 days and 28 days, they look very similar in chemical shift and peak shape, which indicates that the aluminum environment does not change much during the reaction, or the reaction has reached a certain equilibrium state in the early stage. The peak of AlO6 at 4ppm has always existed, and the peak intensity has slightly decreased. It can be judged that the hexacoordinated aluminum in Example 1 comes from the unreacted slag raw material.

[0083] Fig.16 is the slag in Example 1 29 Si NMR and 27 The peak fitting results of AlNMR spectrum, Fig.17 is the slag in Example 1 29 Si NMR and 27 The peak fitting results of Al NMR spectrum, Fig.18 is the 3d age of the slag-based polymer in Example 129 Si NMR and 27 The peak fitting results of AlNMR spectrum, Fig.19 is the 7d-old age of the slag-based polymer in Example 1 29 SiNMR and 27 The peak fitting results of Al NMR spectrum, Fig. 20 is the 28d age of the slag-based polymer in Example 1 29 Si NMR and 27 The peak fitting results of Al NMR spectrum. It can be seen that the peaks of slag are all single peaks, appearing in the range of -90ppm to -110ppm, and the single peaks still exist in the reactants, proving that there is always an unreacted part of the slag. The strongest peak of the slag raw material at -91.0 belongs to Q 3 (1Al), the peaks of -94.1ppm, -96.9ppm, -100.1ppm, and -107.1ppm in the slag raw material belong to Q 4 (3Al), Q 4 (2Al), Q 4 (1Al), Q 4 , which corresponds to the main components of quartz and kaolin in the slag, are mostly three-dimensional network structures and layered structures with low activity; due to a large number of highly polymerized Si groups, the slag raw material has a large peak between -60ppm and -90ppm, and the peaks of the slag raw material at -65.3ppm, -70.1ppm, -73.7ppm, -77.0ppm, -80.7ppm, and 84.7ppm belong to Q 0 , Q 1 (1Al), Q 1 , Q 2 (2Al), Q 2 (1Al), Q 2 After alkali activation, the intensity of this peak is significantly reduced. Although the main spectral bands of the slurry are in different positions, the peak structure and characteristic peak position of each reaction product between -100 and -73 ppm are very obvious, indicating that the Al substitution rate in the reaction product after activation is very high.

[0084] According to the obtained 27 In the Al NMR spectrum, the peaks in the range of 0 to 14 ppm correspond to hexacoordinated aluminum, the peaks in the range of 27 to 37 ppm correspond to pentacoordinated aluminum, and the peaks in the range of 45 to 70 ppm correspond to tetracoordinated aluminum. The peaks at -45.3 ppm, -54.7 ppm, -60.3 ppm, -64.9 ppm, -70.3 ppm and -80.7 ppm are respectively assigned to q 4 ,q 3 ,q 2 ,q 1 ,q0 (n represents the number of next-nearest silicon atoms connected to the core aluminum atom). 29 Si and 27 The AlNMR spectrum was deconvoluted and the obtained fitting spectrum was highly consistent with the original spectrum, and the difference in total area did not exceed 1%. Therefore, it can be determined that the data processed by this deconvolution process is highly reliable.

[0085] At the 3-day stage, aluminum substituted a high proportion of silicon atoms, such as Q 3 (1Al) and Q 4 (3Al), whose content significantly exceeds that of Q 4 (2Al), Q 4 (1Al) and Q 4 This phenomenon indicates that under the promotion of the activator, the original structure began to disintegrate and release active silicon. At the same time, it was observed that Q 0 and Q 1 The characteristic peak of (1Al) decreases, indicating that in the early stage of the reaction, a large amount of silicon monomers in the slag are dissolved, which promotes the CASH gel with a low degree of polymerization. As the reaction time increases, the content of silicon atoms in the chain structure is relatively high, the main band continues to move to a higher chemical shift, and the relative intensity of the -60ppm to -70ppm region decreases. The amount of Si from monomers to oligomers decreases, and more polymerization products are generated. 2 The peak only exists in a small amount in the raw slag, but the peak area gradually increases with the reaction age, especially in the later stage of the reaction. It can be inferred that more CASH and NASH gels are formed in the system, and the chain length is gradually getting longer. The proportion of low-substituted silicon atoms in the system is always increasing. The reason is that Si-O-Si bonds are more stable than Si-O-Al bonds. Si-O-Si bonds are preferentially generated during the polycondensation reaction, and the product gradually changes from an aluminum-rich state to a silicon-rich state. This change is also conducive to the improvement of mechanical properties. From 7 days to 28 days, the curve only moves slightly, indicating that a stable Si coordination environment has been formed.

[0086] Compressive strength test of landfill base polymer: According to GB / T17671-1999 standard test, the size of landfill base polymer compressive strength is 40mm×40mm×40mm, the loading speed is 2.4kN / s, the testing machine used is Wuxi Zhongke building materials strength testing machine, and the landfill base polymer gel is in an environment with a curing temperature set at 25±2℃ and a relative humidity set at 95%; in order to ensure the accuracy of the results, the average value of three parallel tests is taken as the final data result. The compressive strength test results are shown in Tables 1 and Fig. 22 .

[0087] Comparative Example 1

[0088] The only difference from Example 1 is that the alkali activator is changed from water glass to solid sodium hydroxide, and the amounts of the raw materials used are shown in Table 1.

[0089] Comparative Example 2

[0090] The only difference from Example 1 is that no slag is added, and the amounts of each prepared raw material are shown in Table 1.

[0091] Embodiments 2 to 14

[0092] The slag base polymer was prepared according to the method of Example 1. The amount of each raw material used and the compressive strength test results are shown in Tables 1 and Figure 21 to Figure 23 ,in, Fig.21 The compressive strength test results of the slag base polymers with different water-to-solid ratios prepared in Examples 1 to 5; Fig. 22 The compressive strength test results of the slag-based polymers prepared in Comparative Example 2 and Examples 5 to 9 with different slag blending ratios are shown; Fig.23 These are the compressive strength test results of the slag-based polymers with different alkali contents prepared in Examples 10 to 14.

[0093] Embodiments 15 to 17

[0094] (1) Same as Example 1;

[0095] (2) Compression molding and curing: The geopolymer slurry is placed in steel molds of 45mm×40mm×40mm and 45mm×40mm×160mm, the cover of the steel mold is 5mm thick, and a press is used to apply 2 tons of pressure to form it. The mold is sealed with plastic wrap and placed in a constant temperature and humidity curing box for pressure molding for 24 hours. The mold is demolded to obtain a slag-based polymer gel. The slag-based polymer gel is cured in the above-mentioned constant temperature and humidity for 2d, 6d and 27d to obtain slag-based polymers of different ages (3d, 7d and 28d). Among them, a release agent is applied to all inner walls of the steel mold before use. The temperature of the constant temperature and humidity is 25±2℃, and the relative humidity is 95%.

[0096] The dosage of each raw material and the compressive strength test results are shown in Table 1 and Fig.24 .

[0097] Embodiment 18

[0098] The geopolymer slurry was prepared according to the method of Example 1, the only difference from Example 1 being that the amounts of the various preparation raw materials were shown in Table 1.

[0099] Examples 19 to 21

[0100] (1) Mix the retarder with 2 / 3 water (excluding the water in the water glass) to obtain a retarder solution. Mix the water reducer with 1 / 3 water (excluding the water in the water glass) to obtain a water reducer solution. Add slag and slag to the slurry mixer, first stir at a low speed of 45 r / min for 1 min, add the retarder solution and water glass, stir at a low speed of 45 r / min for 1 min, let it stand for 3 min, add the water reducer solution, stir at a high speed of 120 r / min for 2 min, and obtain a geopolymer slurry. The proportions of the raw materials of the geopolymer slurry are shown in Table 1.

[0101] (2) Same as Example 1.

[0102] The dosage of each raw material and the compressive strength test results are shown in Table 1 and Fig.25 .

[0103] Comparative Examples 3 to 7

[0104] (1) Mix the water reducer with all the water (excluding the water in the water glass) to obtain a water reducer solution. Add the slag and slag to the slurry mixer, stir at a low speed of 45 r / min for 1 min, add the water glass, stir at a low speed of 45 r / min for 1 min, let it stand for 3 min, add the water reducer solution, stir at a high speed of 120 r / min for 2 min, and obtain the geopolymer slurry. The proportion of the raw materials of the geopolymer slurry is shown in Table 1.

[0105] (2) Same as Example 1.

[0106] The amounts of raw materials used in Examples 1 to 21 and Comparative Examples 1 to 7 and the compressive strength test results are shown in Table 1.

[0107] Table 1 Preparation of raw material dosage and compressive strength test results

[0108]

[0109]

[0110] Note: “—” means not tested.

[0111] As shown in Table 1, when the water-solid ratio is 0.35, the strength of the slag-based polymer reaches its peak, with a 3d compressive strength of 21.73MPa and a 28d compressive strength of 50.4MPa. When the water-solid ratio varies in the range of 0.35 to 0.45, the strength performance of the slag-based polymer decreases linearly with the increase of the water-solid ratio. When the water-solid ratio is set to 0.35, the slag-based polymer not only exhibits excellent strength, but also can be smoothly cast and molded. Therefore, 0.35 is the optimal water-solid ratio.

[0112] When the slag content is 70%, the compressive strength is relatively small. When the content is 50%, the 28d compressive strength reaches 41.30MPa. This content can not only maintain a very high compressive strength, but also achieve the purpose of consuming a large amount of slag.

[0113] When the alkali content is between 3% and 4%, the compressive strength of the slag-based polymer continues to increase. The 3-day and 28-day compressive strengths are the highest when the alkali content is 4%. When the alkali content is 5%, the 7-day compressive strength reaches a peak value. However, as the alkali content further increases, the compressive strength begins to gradually decrease. This indicates that excessive alkali content has an inhibitory effect on the polymerization reaction of the slag-based polymer and has a negative impact on its performance.

[0114] As can be seen from Examples 16 to 18, when pressure molding is adopted, the compressive strength almost equal to that of 4 to 5% alkali content during casting molding can be obtained at a lower alkali content (2% and below), which saves the amount of alkali solution used to a certain extent, thereby reducing material costs and environmental burdens. As can be seen from Examples 19 to 20, when the slag mixing ratio is 30%, the admixture will improve its mechanical properties, but with the slag mixing ratio increasing to 50%, the admixture will have a negative impact on the strength of the slag-based polymer. Therefore, adding an appropriate amount of admixture when the slag mixing amount is 30% will improve the compressive strength of the slag-based polymer.

[0115] When the water reducer was used alone in Comparative Examples 3 to 7 without using a retarder, the fluidity of the obtained landfill base polymer was very poor, the sample failed to form, and the strength could not be measured. When the water reducers of the models of BNE-7702, SikaStabilizer-412MBF, SikaStabilizer-412MBF, SikaStabilizer SK 181, and SikaStabilizer ASA300 were added alone, there was basically no improvement in the fluidity of the landfill base polymer. When 40% ceramic mother liquid water reducer was added alone, the fluidity of the landfill base polymer was improved, but the effect was not as good as when the water reducer and retarder were added to the landfill base polymer together.

[0116] Fig.26 This is a comparison chart of the fluidity of the geopolymer slurry prepared in Example 18 (without adding retarder and water reducer, upper figure) and Example 21 (adding retarder and water reducer at the same time, lower figure). It can be seen that when no retarder and admixture are used, the fluidity of the slag base polymer obtained is very poor, and the fluidity of the slag base polymer is significantly improved after using retarder and admixture.

[0117] Fig. 27The images of the slag base polymer prepared when sodium hydroxide was used as the alkaline activator in Comparative Example 1 (upper picture) and the polymer directly crushed after being compressed (lower picture) show that when sodium hydroxide was used as the alkaline activator, a large amount of heat was released during the preparation process, and the polymer solidified rapidly without fluidity. The obtained test block had no strength and was directly crushed when subjected to a pressure of 5 MPa.

[0118] It can be seen from the above embodiments and comparative examples that the present invention uses slag and slag as geopolymer materials, and successfully develops a geopolymer with considerable compressive strength by reasonably controlling the slag dosage, alkali content, applied pressure, admixtures, etc., and can also use pressure molding to reduce the use of alkali activators, use appropriate admixtures to enhance the compressive strength of geopolymers, etc., while fully consuming slag, it can also reduce CO2 emissions, reduce costs, and save resources.

[0119] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A slag-based polymer, wherein the raw materials for preparing the polymer include waste slag, water glass and water; the waste slag includes engineering slag and slag, the mass content of engineering slag in the waste slag is ≤70%; the mass of Na2O in the water glass accounts for 1.5-7% of the mass of the waste slag; the total mass of water in the raw materials for preparing the polymer accounts for 30-45% of the mass of the waste slag.

2. The landfill base polymer according to claim 1, characterized in that: The particle size of the engineering slag is ≥80 mesh.

3. The landfill base polymer according to claim 1, characterized in that: The particle size of the slag is 50 to 1000 nm.

4. The landfill base polymer according to claim 1, characterized in that: The modulus of the water glass is 1.5 to 3.

5.

5. The landfill base polymer according to claim 1, characterized in that: The preparation raw materials also include additives; The mass of the admixture accounts for 0.4-1% of the mass of the waste slag.

6. The landfill base polymer according to claim 5, characterized in that: The admixtures include retarders and water reducers.

7. The landfill base polymer according to claim 5, characterized in that: The retarder includes BNE-7602; The water reducing agent includes one or more of ceramic water reducing agent mother liquor, BNE-7702, anti-mud water reducing agent, Sika Stabilizer-412MBF, SK 181, ASA300, 530P, 556P, 540P and 325C.

8. The method for preparing the landfill-based polymer according to any one of claims 1 to 7, comprising the following steps: The engineering slag, slag, water glass and water are mixed, and then formed and cured to obtain a slag base polymer; The forming includes casting forming or pressure forming.

9. The preparation method according to claim 8, characterized in that: The pressure of the pressure forming is 1 to 5 tons.

10. Use of the slag-based polymer according to any one of claims 1 to 7 or the slag-based polymer prepared by the preparation method according to any one of claims 8 to 9 as a building material.

Citation Information

Cited By

  • All-solid-waste self-excitation muck slurry and preparation method thereof