Indium titanium tantalum cerium oxide target material and preparation method thereof
By adjusting the powder ratio and preparation process of indium titanium tantalum cerium target, combined with spray granulation and sintering treatment, the problem of insufficient controllability of the microstructure of indium titanium tantalum cerium target is solved, and high density and uniformity are achieved. Expand its applicability in the field of HJT batteries.
Patent Information
- Application Number
- CN202411294853.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-14
- Publication Date
- 2024-12-06
AI Technical Summary
The lack of expansion of the controllability and application scope of the microstructure of indium titanium tantalum cerium target in the prior art has led to its limited application in the field of HJT heterojunction solar cells.
By defining the mass ratio of indium oxide powder, titanium oxide powder, tantalum pentoxide powder, and cerium oxide powder, and combining wet grinding and spray granulation technology, indium titanium oxide with high relative density and controllable grain size were prepared. Tantalum cerium targets are degreased heat treatment and sintered heat treatment using specific sintering temperatures and times to regulate the microstructure of the target.
The relative density of indium titanium tantalum cerium targets has high composition distribution uniformity and controllable microstructure, which expands its applicability in the field of HJT batteries, and can adjust the grain size within the range of 9~25μm to meet the different Customer needs.
Smart Images

Figure CN119080476A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the field of target material preparation, and more specifically, relates to an indium titanium tantalum cerium oxide target material and a preparation method thereof. Background Art
[0002] HJT heterojunction solar cells have the advantages of high open circuit voltage, low temperature coefficient, symmetrical structure, low energy consumption, no photo-induced degradation, no potential-induced degradation, etc. In recent years, with the rapid development of the photovoltaic industry, the annual shipments have increased significantly. At present, the efficiency of the cells of the first-line HJT cell manufacturers using the double-sided microcrystalline process can reach 25.7%. Due to the poor conductivity of amorphous silicon thin film, the metallization step cannot be directly carried out. Therefore, it is necessary to deposit a layer of transparent conductive oxide (TCO) film between amorphous silicon and the electrode to improve the lateral collection of photogenerated carriers of amorphous silicon. On the one hand, the TCO film layer is responsible for the collection of carriers and the transfer to the front and rear metals. It needs to have a low contact resistance with Ag or Cu. On the other hand, as the outermost film layer, it needs to have a high transmittance. This requires the TCO film layer and its sputtering raw material-metal oxide target material to have the characteristics of wide bandgap and low resistance at the same time.
[0003] The indium titanium tantalum cerium oxide target film has been tested to have excellent performance of high optical transmittance, high carrier mobility, and high carrier concentration, and is widely used in the field of HJT heterojunction batteries. Therefore, the preparation of indium titanium tantalum cerium oxide targets with better performance and wider application range has a very important role in promoting the sustainable development of the above fields.
[0004] CN116835964A significantly improves the relative density of the target material while reducing the zirconium content introduced by grinding by limiting the composition ratio of each oxide powder and coordinating a specific preparation process. Patent CN116639956A improves the mobility and conductivity of the target material by adjusting the components in the target material. CN117185779A improves the relative density, bending strength and mobility of the target material by vacuuming the target blank and oxygenating it at a certain pressure before sintering.
[0005] The above technologies either improve target material density, conductivity and other parameters by controlling the proportion of doping elements and powder particle size, or improve target material relative density, bending strength and other properties by performing complex pretreatment on the target blank before sintering. However, there is a lack of research on the preparation of indium titanium tantalum cerium oxide targets, which have more controllable microstructures and a wider range of applications. Summary of the invention
[0006] In view of the above problems existing in the prior art, the object of the present invention is to provide an indium titanium tantalum cerium oxide target material with controllable microstructure and wide application range and a preparation method thereof.
[0007] To achieve the above purpose, the technical solution adopted by the present invention is: A method for preparing an indium titanium tantalum cerium oxide target material comprises the following steps: (1) Weigh indium oxide powder, titanium oxide powder, tantalum pentoxide powder, and cerium oxide powder in a mass ratio of 95.5-97.5:0.3-2.0:0.3-2.0:0.3-1.5 respectively; (2) mixing and dispersing the oxide powder weighed in step (1) with a dispersant and a binder, and obtaining a mixed slurry by wet grinding; (3) using the mixed slurry as a raw material to perform spray granulation to obtain a mixed oxide powder; (4) Using the mixed oxide powder as a raw material for pressing and molding to obtain a target blank; (5) The target blank is subjected to degreasing heat treatment and sintering heat treatment in sequence to obtain an indium titanium tantalum cerium oxide target material. The highest sintering temperature of the sintering heat treatment is 1350-1500° C. and the highest high temperature holding time is 15-30 hours.
[0008] The present application limits the maximum sintering temperature and the maximum high temperature holding time, and the indium titanium tantalum cerium oxide target material prepared can adjust the target material grain size within the range of 9 to 25 μm while maintaining a relatively stable density.
[0009] Preferably, in step (1), the purity of the indium oxide powder, titanium oxide powder, tantalum pentoxide powder and cerium oxide powder is 4N.
[0010] Preferably, the dispersant is one or more of triethylhexyl phosphate, polyvinyl pyrrolidone, sodium dodecyl sulfate, sodium dodecylbenzene sulfonate, polycarboxylic acid compounds, polyacrylates or sodium hexadecylbenzene sulfonate; Preferably, the binder is one or more of polyethylene glycol, polyvinyl butyral, carboxymethyl cellulose, polyacrylamide, and polyacrylic acid.
[0011] Preferably, in step (2), the mass of the dispersant added is 0.5-1.0% of the total mass of the oxide powder, dispersant and binder added; the mass of the binder added is 2.0-3.0% of the total mass of the oxide powder, dispersant and binder added.
[0012] Preferably, the solid content of the mixed slurry is 50-60%.
[0013] Preferably, in step (6), spray granulation is carried out using a spray drying tower.
[0014] Furthermore, the powder obtained after spray granulation is homogenized and sieved to obtain a mixed oxide powder with uniform particle size distribution.
[0015] More preferably, the particle size requirements of the mixed oxide powder are: D50 is 40-60 μm, and D90 is 70-100 μm.
[0016] Preferably, in step (7), the molding is performed by cold isostatic pressing after molding; Preferably, the molding pressure is 30-100 MPa; the pressing time is 40-120 s; Preferably, the cold isostatic pressing pressure is 150-400 MPa, and the pressing time is 30-180 s.
[0017] Preferably, in step (8): The degreasing heat treatment is as follows: in an air atmosphere, the temperature is raised to 500°C-700°C at a heating rate of 0.5-1°C / min, and the temperature is kept for 2-5 hours.
[0018] The sintering heat treatment is as follows: in an oxygen atmosphere, heating to 1350° C. to 1500° C. at a heating rate of 0.6 to 1.2° C. / min, and keeping the temperature for 15 to 30 hours.
[0019] The invention also discloses an indium titanium tantalum cerium oxide target material prepared by the preparation method.
[0020] Preferably, the grain size of the indium titanium tantalum cerium oxide target material is 9-25 μm, the relative density is ≥99.1%, and the bending strength is ≥120 MPa.
[0021] Compared with the prior art, the present invention has the following beneficial effects: The preparation method of the present application can adjust the grain size of the target material within a limited sintering temperature and sintering time range, actively adapt to the parameter requirements of different customers for the target material, and greatly expand the applicability of indium titanium tantalum cerium oxide target materials.
[0022] The indium titanium tantalum cerium oxide target material prepared by the method of the present invention has high relative density, good uniformity of component distribution and more controllable microstructure. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] The accompanying drawings are used to provide a further understanding of the present invention and constitute a part of the specification. Together with the embodiments of the present invention, they are used to explain the present invention and do not constitute a limitation of the present invention. In the accompanying drawings: Figure 1 This is a bar graph of target grain size distribution obtained in Example 1; Figure 2 This is a bar graph of target material grain size distribution obtained in Example 2; Figure 3 This is a bar graph of target grain size distribution obtained in Example 3; Figure 4 This is a bar graph of target grain size distribution obtained in Example 4; Figure 5 This is a bar graph of target grain size distribution obtained in Example 5; Figure 6 This is a bar graph of target grain size distribution obtained in Example 6; Figure 7 This is a bar graph of target grain size distribution obtained in Example 7; Figure 8 This is a bar graph of target material grain size distribution obtained in Example 8; Fig. 9 This is a bar graph of the target material grain size distribution obtained in Example 9. DETAILED DESCRIPTION
[0024] In order to facilitate the understanding of the present invention, the present invention will be described more comprehensively and meticulously below in conjunction with the accompanying drawings and preferred embodiments of the present invention, but the protection scope of the present invention is not limited to the following specific embodiments.
[0025] Unless otherwise defined, all the professional terms used below have the same meanings as those generally understood by those skilled in the art. The professional terms used herein are only for the purpose of describing specific embodiments and are not intended to limit the scope of protection of the present invention.
[0026] Unless otherwise specified, various raw materials, reagents, instruments and equipment used in the present invention can be purchased from the market or prepared by existing methods.
[0027] Example 1 (1) Accurately weigh a certain amount of indium oxide, titanium oxide, tantalum oxide, and cerium oxide powders according to a mass ratio of 96.5:0.5:1.5:1.5.
[0028] (2) The powder weighed in step (1) is added to a dispersion tank with polyvinyl pyrrolidone and polyethylene glycol for dispersion at a speed of 70 rpm for 30 min. The dispersed powder is pumped into a sand mill with an air pump for wet sand milling at 1000 rpm for 60 min to obtain a mixed slurry with a solid content of 60%.
[0029] (3) The slurry obtained in step (2) is spray granulated in a spray drying tower, and the powder is sieved to obtain a mixed oxide powder with uniform particle size distribution. The D50 of the mixed oxide powder is 44 μm and the D90 is 80 μm.
[0030] (4) The mixed oxide powder obtained in step (3) is added into a mold, and a target blank is obtained by molding and cold isostatic pressing. The molding pressure is 50 MPa, the pressing time is 60 s, and the cold isostatic pressing pressure is 150 MPa, and the pressing time is 60 s.
[0031] (5) The target blank obtained in step (4) was placed in a sintering furnace, and the temperature was raised to 600°C at 1°C / min, and kept at this temperature for 3 hours, and then the temperature was further raised to 1380°C at 0.65°C / min, and kept at this temperature for 15 hours. Thus, an indium titanium tantalum cerium oxide target material was obtained.
[0032] After testing, the relative density of the indium titanium tantalum cerium oxide target prepared in this embodiment is 99.12%. Figure 1 As shown, the grain size is 9.21μm and the bending strength is 147Mpa.
[0033] Example 2 Accurately weigh a certain amount of indium oxide, titanium oxide, tantalum oxide, and cerium oxide powders according to a mass ratio of 96.5:0.5:2.0:1.0.
[0034] (2) The powder weighed in step (1) is added to a dispersion tank with polyvinyl pyrrolidone and polyvinyl butyral for dispersion at a speed of 80 rpm for 30 min. The dispersed powder is pumped into a sand mill for wet sand grinding at 1100 rpm for 60 min to obtain a mixed slurry with a solid content of 60%.
[0035] (3) The slurry obtained in step (2) is spray granulated in a spray drying tower, and the powder is sieved to obtain a mixed oxide powder with uniform particle size distribution. The D50 of the mixed oxide powder is 47 μm and the D90 is 82 μm.
[0036] (4) The mixed oxide powder obtained in step (3) is added into a mold, and a target blank is obtained by molding and cold isostatic pressing. The molding pressure is 600 MPa, the pressing time is 100 s, and the cold isostatic pressing pressure is 180 MPa, and the pressing time is 70 s.
[0037] (5) The target blank obtained in step (4) was placed in a sintering furnace, and the temperature was raised to 600°C at 0.5°C / min, and kept at this temperature for 3 hours. The temperature was then raised to 1380°C at 0.7°C / min, and kept at this temperature for 20 hours. Thus, an indium titanium tantalum cerium oxide target was obtained.
[0038] After testing, the relative density of the indium titanium tantalum cerium oxide target prepared in this embodiment is 99.35%. Figure 2 As shown, the grain size is 12.78μm and the bending strength is 142Mpa.
[0039] Example 3 (1) Accurately weigh a certain amount of indium oxide, titanium oxide, tantalum oxide, and cerium oxide powders according to a mass ratio of 97.0:0.5:1.5:1.0.
[0040] (2) The powder weighed in step (1) was added to a dispersion tank with sodium hexadecylbenzene sulfonate and polyacrylamide for dispersion at a speed of 60 rpm for 50 min. The dispersed powder was pumped into a sand mill for wet sand grinding at 1100 rpm for 50 min to obtain a mixed slurry with a solid content of 60%.
[0041] (3) The slurry obtained in step (2) is spray granulated in a spray drying tower, and the powder is sieved to obtain a mixed oxide powder with uniform particle size distribution. The D50 of the mixed oxide powder is 51 μm and the D90 is 75 μm.
[0042] (4) The mixed oxide powder obtained in step (3) is added into a mold, and a target blank is obtained by molding and cold isostatic pressing. The molding pressure is 70 MPa, the pressing time is 40 s, and the cold isostatic pressing pressure is 2000 MPa, and the pressing time is 40 s.
[0043] (5) The target blank obtained in step (4) was placed in a sintering furnace, and the temperature was raised to 500°C at 0.8°C / min, and kept at this temperature for 5 hours, and then the temperature was further raised to 1380°C at 0.7°C / min, and kept at this temperature for 25 hours. Thus, an indium titanium tantalum cerium oxide target material was obtained.
[0044] After testing, the relative density of the indium titanium tantalum cerium oxide target prepared in this embodiment is 99.23%. Figure 3 As shown, the grain size is 13.52μm and the bending strength is 140Mpa.
[0045] Example 4 (1) Accurately weigh a certain amount of indium oxide, titanium oxide, tantalum oxide, and cerium oxide powder according to a mass ratio of 97.5:0.5:1.5:1.0.
[0046] (2) The powder weighed in step (1) was added to a dispersion tank with sodium dodecylbenzene sulfonate and polyvinyl butyral for dispersion at a speed of 100 rpm for 30 min. The dispersed powder was pumped into a sand mill for wet sand grinding at 1300 rpm for 60 min to obtain a mixed slurry with a solid content of 60%.
[0047] (3) The slurry obtained in step (2) is spray granulated in a spray drying tower, and the powder is sieved to obtain a mixed oxide powder with uniform particle size distribution. The D50 of the mixed oxide powder is 45 μm and the D90 is 76 μm.
[0048] (4) The mixed oxide powder obtained in step (3) is added into a mold, and a target blank is obtained by molding and cold isostatic pressing. The molding pressure is 80 MPa, the pressing time is 100 s, and the cold isostatic pressing pressure is 250 MPa, and the pressing time is 30 s.
[0049] (5) The target blank obtained in step (4) was placed in a sintering furnace, and the temperature was raised to 500°C at 0.8°C / min, and kept at this temperature for 5 hours, and then the temperature was raised to 1430°C at 1.0°C / min, and kept at this temperature for 15 hours. Thus, an indium titanium tantalum cerium oxide target material was obtained.
[0050] After testing, the relative density of the indium titanium tantalum cerium oxide target prepared in this embodiment is 99.26%. Figure 4 As shown, the grain size is 13.17μm and the bending strength is 145Mpa.
[0051] Example 5 (1) Accurately weigh a certain amount of indium oxide, titanium oxide, tantalum oxide, and cerium oxide powders in a mass ratio of 97.0:1.0:1.0:1.0.
[0052] (2) The powder weighed in step (1) is added to a dispersion tank with polyvinyl pyrrolidone and polyacrylamide for dispersion at a speed of 60 rpm for 60 min. The dispersed powder is pumped into a sand mill for wet sand grinding at 1000 rpm for 120 min to obtain a mixed slurry with a solid content of 60%.
[0053] (3) The slurry obtained in step (2) is spray granulated in a spray drying tower, and the powder is sieved to obtain a mixed oxide powder with uniform particle size distribution. The D50 of the mixed oxide powder is 52 μm and the D90 is 80 μm.
[0054] (4) The mixed oxide powder obtained in step (3) is added into a mold, and a target blank is obtained by molding and cold isostatic pressing. The molding pressure is 50 MPa, the pressing time is 120 s, and the cold isostatic pressing pressure is 250 MPa, and the pressing time is 50 s.
[0055] (5) The target blank obtained in step (4) was placed in a sintering furnace, and the temperature was raised to 600°C at 0.5°C / min, and kept at this temperature for 4 hours. The temperature was then raised to 1430°C at 1.2°C / min, and kept at this temperature for 20 hours. Thus, an indium titanium tantalum cerium oxide target was obtained.
[0056] After testing, the relative density of the indium titanium tantalum cerium oxide target prepared in this embodiment is 99.31%. Figure 5 As shown, the grain size is 14.25μm and the bending strength is 140Mpa.
[0057] Example 6 (1) Accurately weigh a certain amount of indium oxide, titanium oxide, tantalum oxide, and cerium oxide powders according to a mass ratio of 97.0:0.5:1.25:1.25.
[0058] (2) The powder weighed in step (1) is added to a dispersion tank with polyvinyl pyrrolidone and polyacrylamide for dispersion at a speed of 150 rpm for 70 min. The dispersed powder is pumped into a sand mill with an air pump for wet sand milling at 1200 rpm for 120 min to obtain a mixed slurry with a solid content of 60%.
[0059] (3) The slurry obtained in step (2) is spray granulated in a spray drying tower, and the powder is homogenized and sieved to obtain a mixed oxide powder with uniform particle size distribution. The D50 of the mixed oxide powder is 47 μm and the D90 is 78 μm.
[0060] (4) The mixed oxide powder obtained in step (3) is added into a mold, and a target blank is obtained by molding and cold isostatic pressing. The molding pressure is 30 MPa, the pressing time is 120 s, and the cold isostatic pressing pressure is 300 MPa, and the pressing time is 40 s.
[0061] (5) The target blank obtained in step (4) was placed in a sintering furnace, and the temperature was raised to 700°C at 0.5°C / min, and kept at this temperature for 2 hours. The temperature was then raised to 1430°C at 0.6°C / min, and kept at this temperature for 25 hours. Thus, an indium titanium tantalum cerium oxide target was obtained.
[0062] After testing, the relative density of the indium titanium tantalum cerium oxide target prepared in this embodiment is 99.22%. Figure 6 As shown, the grain size is 17.69μm and the bending strength is 136Mpa.
[0063] Example 7 (1) Accurately weigh a certain amount of indium oxide, titanium oxide, tantalum oxide, and cerium oxide powders according to a mass ratio of 95.5:2.0:1.0:1.5.
[0064] (2) The powder weighed in step (1) was added to a dispersion tank with sodium dodecylbenzene sulfonate and polyacrylamide for dispersion at a speed of 120 rpm for 40 min. The dispersed powder was pumped into a sand mill for wet sand grinding at 1000 rpm for 150 min to obtain a mixed slurry with a solid content of 60%.
[0065] (3) The slurry obtained in step (2) is spray granulated in a spray drying tower, and the powder is sieved to obtain a mixed oxide powder with uniform particle size distribution. The D50 of the mixed oxide powder is 53 μm and the D90 is 82 μm.
[0066] (4) The mixed oxide powder obtained in step (3) is added into a mold, and a target blank is obtained by molding and cold isostatic pressing. The molding pressure is 80 MPa, the pressing time is 40 s, and the cold isostatic pressing pressure is 250 MPa, and the pressing time is 70 s.
[0067] (5) The target blank obtained in step (4) was placed in a sintering furnace, and the temperature was raised to 600°C at 0.6°C / min, and kept at this temperature for 3 hours, and then the temperature was further raised to 1480°C at 1.0°C / min, and kept at this temperature for 25 hours. Thus, an indium titanium tantalum cerium oxide target material was obtained.
[0068] After testing, the relative density of the indium titanium tantalum cerium oxide target prepared in this embodiment is 99.19%. Figure 7 As shown, the grain size is 19.42μm and the bending strength is 132Mpa.
[0069] Example 8 (1) Accurately weigh a certain amount of indium oxide, titanium oxide, tantalum oxide, and cerium oxide powders according to a mass ratio of 96.0:1.5:1.5:1.0.
[0070] (2) The powder weighed in step (1) was added to a dispersion tank with sodium dodecylbenzene sulfonate and polyethylene glycol for dispersion at a speed of 150 rpm for 40 min. The dispersed powder was pumped into a sand mill for wet sand grinding at 1300 rpm for 80 min to obtain a mixed slurry with a solid content of 60%.
[0071] (3) The slurry obtained in step (2) is spray granulated in a spray drying tower, and the powder is sieved to obtain a mixed oxide powder with uniform particle size distribution. The D50 of the mixed oxide powder is 56 μm and the D90 is 83 μm.
[0072] (4) The mixed oxide powder obtained in step (3) is added into a mold, and a target blank is obtained by molding and cold isostatic pressing. The molding pressure is 60 MPa, the pressing time is 70 s, and the cold isostatic pressing pressure is 300 MPa, and the pressing time is 40 s.
[0073] (5) The target blank obtained in step (4) is placed in a sintering furnace, and the temperature is raised to 600°C at 0.7°C / min, and kept at this temperature for 3 hours, and then the temperature is further raised to 1480°C at 0.8°C / min, and kept at this temperature for 20 hours. Thus, an indium titanium tantalum cerium oxide target is obtained.
[0074] After testing, the relative density of the indium titanium tantalum cerium oxide target prepared in this embodiment is 99.14%. Figure 8 As shown, the grain size is 20.54μm and the bending strength is 124Mpa.
[0075] Example 9 (1) Accurately weigh a certain amount of indium oxide, titanium oxide, tantalum oxide, and cerium oxide powders according to a mass ratio of 96.5:1.0:1.0:1.5.
[0076] (2) The powder weighed in step (1) was added to a dispersion tank with sodium dodecylbenzene sulfonate and polyethylene glycol for dispersion at a speed of 150 rpm for 30 min. The dispersed powder was pumped into a sand mill for wet sand grinding at 1200 rpm for 150 min to obtain a mixed slurry with a solid content of 60%.
[0077] (3) The slurry obtained in step (2) is spray granulated in a spray drying tower, and the powder is sieved to obtain a mixed oxide powder with uniform particle size distribution. The D50 of the mixed oxide powder is 43 μm and the D90 is 71 μm.
[0078] (4) The mixed oxide powder obtained in step (3) is added into a mold, and a target blank is obtained by molding and cold isostatic pressing. The molding pressure is 70 MPa, the pressing time is 60 s, and the cold isostatic pressing pressure is 300 MPa, and the pressing time is 30 s.
[0079] (5) The target blank obtained in step (4) was placed in a sintering furnace, and the temperature was raised to 700°C at 0.8°C / min, and kept at this temperature for 3 hours. The temperature was then raised to 1480°C at 0.9°C / min, and kept at this temperature for 25 hours. Thus, an indium titanium tantalum cerium oxide target was obtained.
[0080] After testing, the relative density of the indium titanium tantalum cerium oxide target prepared in this embodiment is 99.10%. Fig. 9 As shown, the grain size is 22.43μm and the bending strength is 121Mpa.
[0081] The sintering temperature, holding time, and the measured relative density, grain size, and flexural strength values in Examples 1 to 9 are summarized in Table 1.
[0082] It can be seen that the indium titanium tantalum cerium oxide target prepared by the method of the present application has high relative density and good uniformity of component distribution. The target grain size can be adjusted to actively adapt to the parameter requirements of different customers for the target material, which greatly expands the applicability of the indium titanium tantalum cerium oxide target.
[0083] Table 1 The above are only preferred embodiments of the present invention and are not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the scope of the present invention.
Claims
1. A method for preparing an indium titanium tantalum cerium oxide target, characterized in that: The following steps are involved: (1) Weigh indium oxide powder, titanium oxide powder, tantalum pentoxide powder, and cerium oxide powder in a mass ratio of 95.5-97.5:0.3-2.0:0.3-2.0:0.3-1.5 respectively; (2) mixing and dispersing the oxide powder weighed in step (1) with a dispersant and a binder, and obtaining a mixed slurry by wet grinding; (3) using the mixed slurry as a raw material to perform spray granulation to obtain a mixed oxide powder; (4) Using the mixed oxide powder as a raw material for pressing and molding to obtain a target blank; (5) The target blank is subjected to degreasing heat treatment and sintering heat treatment in sequence to obtain an indium titanium tantalum cerium oxide target material. The highest sintering temperature of the sintering heat treatment is 1350-1500° C. and the highest high temperature holding time is 15-30 hours.
2. The preparation method according to claim 1, characterized in that In step (1), the purity of indium oxide powder, titanium oxide powder, tantalum pentoxide powder and cerium oxide powder is 4N.
3. The preparation method according to claim 1, characterized in that: The dispersant is one or more of triethylhexyl phosphate, polyvinyl pyrrolidone, sodium dodecyl sulfate, sodium dodecylbenzene sulfonate, polycarboxylic acid compounds, polyacrylate, and sodium hexadecylbenzene sulfonate; Preferably, the binder is one or more of polyethylene glycol, polyvinyl butyral, carboxymethyl cellulose, polyacrylamide, and polyacrylic acid.
4. The preparation method according to claim 1, characterized in that: In step (2), the mass of the dispersant is 0.5-1.0% of the total mass of the oxide powder, the dispersant and the binder; the mass of the binder is 2.0-3.0% of the total mass of the oxide powder, the dispersant and the binder.
5. The preparation method according to claim 1 or 4, characterized in that: The solid content of the mixed slurry is 50-60%.
6. The preparation method according to claim 1, characterized in that: In step (3), spray granulation is performed using a spray drying tower; the powder obtained after spray granulation is homogenized and sieved to obtain a mixed oxide powder with uniform particle size distribution.
7. The preparation method according to claim 1, characterized in that: In step (4), the molding is performed by first molding and then cold isostatic pressing; Preferably, the molding pressure is 30-100 MPa; the pressing time is 40-120 s; Preferably, the cold isostatic pressing pressure is 150-400 MPa, and the pressing time is 30-180 s.
8. The preparation method according to claim 1, characterized in that: In step (5): The degreasing heat treatment is as follows: in an air atmosphere, the temperature is raised to 500°C to 700°C at a heating rate of 0.5 to 1°C / min, and the temperature is kept for 2 to 5 hours; The sintering heat treatment is as follows: in an oxygen atmosphere, heating to 1350° C. to 1500° C. at a heating rate of 0.6 to 1.2° C. / min, and keeping the temperature for 15 to 30 hours.
9. An indium titanium tantalum cerium oxide target prepared by the preparation method according to any one of claims 1 to 8.
10. The indium titanium tantalum cerium oxide target material according to claim 9, characterized in that The grain size of the indium titanium tantalum cerium oxide target material is 9-25 μm, the relative density is ≥99.1%, and the bending strength is ≥120 MPa.
Citation Information
Patent Citations
High-mobility indium titanium cerium tantalum oxide target material and preparation method thereof
CN116639956A
Cited By
Preparation method and application of indium cerium oxide target material
CN121135374A