Preparation method of fine-grain high-strength indium titanium tantalum cerium oxide target material
Through the two-stage normal pressure sintering process, grain growth is suppressed, forming a uniformly refined microstructure, significantly improving the bending strength of indium titanium tantalum cerium targets, and solving the reduction in bending strength caused by traditional sintering methods. and target risk issues.
Patent Information
- Application Number
- CN202411294854.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-14
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2044-09-14
AI Technical Summary
The traditional degreasing-sintering-cooling sintering method causes the grains of indium titanium tantalum cerium targets to grow abnormally, forming an uneven microstructure, reducing the bending strength, increasing the risk of target cracking, and unable to meet the larger outer diameter and Mechanical performance requirements for higher weight targets during long-term use.
Using a two-stage normal pressure sintering process, first performs preliminary sintering at high temperatures, and then reduces and insulates within the set temperature range. The difference between grain boundary migration energy and grain boundary diffusion energy is used to inhibit grain growth and form a more uniform and refine microstructure.
The bending strength of indium titanium tantalum cerium targets has been significantly improved, and the application scenarios with higher strength requirements have been met, the risk of target cracking is reduced, and a more uniform microstructure has been obtained.
Smart Images

Figure CN119080477A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the field of target material preparation, and more specifically, relates to a fine-grained high-strength indium titanium tantalum cerium oxide target material and a preparation method thereof. Background Art
[0002] Oxide semiconductor films have excellent optoelectronic properties such as wide bandgap, low resistance, high light transmittance in the visible light region and high light reflectivity in the infrared spectral region. They have long been widely used in solar cells, flat panel displays, organic light-emitting diodes, low-emissivity glass, special function window coatings, transparent thin-film transistors and flexible electronic devices.
[0003] Indium titanium tantalum cerium oxide thin films are currently widely used in HJT heterojunction cells as the TCO layer between amorphous silicon and electrodes to improve the lateral collection of carriers and the transfer to the front and rear metals. Titanium tantalum cerium oxide targets are used as sputtering materials for the TCO layer with an average service life of about thirty days. It takes 2 to 3 days to replace new targets / sputtering baffles and resume production. In order to reduce the production window caused by target replacement, heterojunction battery manufacturers gradually use targets with larger outer diameters, higher weights, and longer service lives to replace the original small outer diameter targets. As the weight of the target material increases significantly, higher torque is also required to drive the target material to rotate during the sputtering process. At this time, if the strength of the target material is low, there is a risk of target cracking during long-term use, which puts forward new requirements for the mechanical properties of indium titanium tantalum cerium oxide targets, such as bending strength.
[0004] The mechanical properties of oxide targets are closely related to their microstructure, especially the grain size. It is generally believed that the smaller the grain size, the better the material toughness and the higher the strength. As a sintering process in the target preparation process, the traditional degreasing-sintering-cooling sintering method often uses a higher sintering temperature and a longer holding time to ensure the densification of the target, resulting in irregular grain growth and uneven microstructure at the end of sintering.
[0005] In the traditional degreasing-sintering-cooling sintering method, the target material is kept in a high temperature state for a long time in the later stage of sintering, which can easily lead to abnormal grain growth and form an uneven microstructure, resulting in a decrease in mechanical properties such as bending strength of the target material and a high risk of target cracking. Summary of the invention
[0006] In view of the above problems existing in the prior art, the object of the present invention is to provide a fine-grained high-strength indium titanium tantalum cerium oxide target material and a preparation method thereof.
[0007] To achieve the above purpose, the technical solution adopted by the present invention is: A method for preparing a fine-grained high-strength indium titanium tantalum cerium oxide target material comprises the following steps: (1) Weigh indium oxide powder, titanium oxide powder, tantalum pentoxide powder, and cerium oxide powder in a mass ratio of 95.5-97.5:0.3-2.0:0.3-2.0:0.3-1.5 respectively; (2) mixing and dispersing the powder weighed in step (1) with a dispersant and a binder, and obtaining a mixed slurry by wet grinding; (3) using the mixed slurry as a raw material to perform spray granulation to obtain a mixed oxide powder; (4) Using the mixed oxide powder as a raw material for pressing and molding to obtain a target blank; (5) The target blank is subjected to degreasing sintering and two-stage atmospheric pressure sintering in sequence to obtain an indium titanium tantalum cerium oxide target material, wherein the two-stage atmospheric pressure sintering comprises: Raise the temperature to 1400~1500℃ and keep it warm for 5~10h; lower the temperature to 1320~1370℃ and keep it warm for 35~50h.
[0008] Furthermore, in step (1), the purity of the indium oxide powder, titanium oxide powder, tantalum pentoxide powder, and cerium oxide powder is 4N.
[0009] Further, the dispersant is one or more of triethylhexyl phosphate, polyvinyl pyrrolidone, sodium dodecyl sulfate, sodium dodecylbenzene sulfonate, polycarboxylic acid compounds, polyacrylates or sodium hexadecylbenzene sulfonate; Preferably, the binder is one or more of polyethylene glycol, polyvinyl butyral, carboxymethyl cellulose, polyacrylamide, and polyacrylic acid.
[0010] Furthermore, in step (2), the mass of the dispersant added is 0.5-1.0% of the total mass of the oxide powder, dispersant and binder added; the mass of the binder added is 2.0-3.0% of the total mass of the oxide powder, dispersant and binder added.
[0011] Furthermore, the solid content of the mixed slurry is 50-60%.
[0012] Furthermore, in step (3), a spray drying tower is used for spray granulation. The powder obtained after spray granulation is homogenized and sieved to obtain a mixed oxide powder with uniform particle size distribution.
[0013] More preferably, the particle size requirements of the mixed oxide powder are: D50 is 40-60 μm, and D90 is 70-100 μm.
[0014] Furthermore, in step (4), the molding is performed by cold isostatic pressing after molding; Preferably, the molding pressure is 30-100 MPa; the pressing time is 40-120 s; Preferably, the cold isostatic pressing pressure is 150-400 MPa, and the pressing time is 30-180 s.
[0015] Furthermore, in step (8): The degreasing heat treatment is as follows: in an air atmosphere, the temperature is raised to 500°C-700°C at a heating rate of 0.5-1°C / min, and the temperature is kept for 2-5 hours.
[0016] The two-stage atmospheric pressure sintering is as follows: in an oxygen atmosphere, heating to 1400-1500°C at a heating rate of 0.6-1.2°C / min, and keeping warm for 5-10 hours; cooling to 1320-1370°C at a cooling rate of 1-1.5°C / min, and keeping warm for 35-50 hours.
[0017] The invention also discloses an indium titanium tantalum cerium oxide target material prepared by the preparation method.
[0018] Furthermore, the indium titanium tantalum cerium oxide target material has a grain size of ≤8 μm, a relative density of ≥99.5%, and a bending strength of ≥160 MPa.
[0019] Compared with the prior art, the present invention has the following beneficial effects: This application creatively proposes a two-step sintering process for preparing indium titanium tantalum cerium oxide target material. Through this method, the microstructure of the obtained target material becomes more uniform, and the grain size is significantly refined, thereby significantly improving the bending strength. Specifically, due to the long-term heat preservation in the high temperature section, the one-step sintering will cause rapid grain growth in the later stage of sintering due to excessive grain boundary migration. The target material prepared by the two-step sintering method is first preliminarily sintered at a higher temperature to allow the target material to obtain a certain density. Subsequently, the difference between the grain boundary migration energy and the grain boundary diffusion energy of the target material is used to ensure grain boundary diffusion within the set temperature range while inhibiting grain boundary migration, thereby inhibiting grain growth and obtaining a more uniform and refined microstructure.
[0020] The indium titanium tantalum cerium oxide target material obtained by the preparation method of the present application has significantly improved strength and can meet the needs of application scenarios with higher strength requirements. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] The accompanying drawings are used to provide a further understanding of the present invention and constitute a part of the specification. Together with the embodiments of the present invention, they are used to explain the present invention and do not constitute a limitation of the present invention. In the accompanying drawings: Figure 1 This is a metallographic picture of the target obtained in Comparative Example 1; Figure 2 This is a bar graph of target grain size distribution obtained in Comparative Example 1; Figure 3 This is a metallographic picture of the target obtained in Example 1; Figure 4This is a bar graph of target grain size distribution obtained in Example 1; Figure 5 This is a metallographic picture of the target obtained in Comparative Example 2; Figure 6 This is a bar graph of target grain size distribution obtained in Comparative Example 2; Figure 7 This is a metallographic picture of the target obtained in Example 2; Figure 8 This is a bar graph of the target material grain size distribution obtained in Example 2. DETAILED DESCRIPTION
[0022] In order to facilitate the understanding of the present invention, the present invention will be described more comprehensively and meticulously below in conjunction with the accompanying drawings and preferred embodiments of the present invention, but the protection scope of the present invention is not limited to the following specific embodiments.
[0023] Unless otherwise defined, all the professional terms used below have the same meanings as those generally understood by those skilled in the art. The professional terms used herein are only for the purpose of describing specific embodiments and are not intended to limit the scope of protection of the present invention.
[0024] Unless otherwise specified, various raw materials, reagents, instruments and equipment used in the present invention can be purchased from the market or prepared by existing methods.
[0025] Example 1 (1) Accurately weigh 50 kg of indium oxide, titanium oxide, tantalum oxide, and cerium oxide powders in a mass ratio of 96.5:0.5:2.0:1.0.
[0026] (2) The powder weighed in step (1) was added to a dispersion tank with 350 g of polyvinyl pyrrolidone and 1050 g of polyvinyl butyral for dispersion at a speed of 90 rpm for 40 min. The dispersed powder was pumped into a sand mill for wet sand grinding at 1000 rpm for 120 min to obtain a mixed slurry with a solid content of 60%.
[0027] (3) spray granulation of the slurry obtained in step (2) in a spray drying tower, and sieving the powder to obtain a mixed oxide powder with uniform particle size distribution, wherein the D50 of the mixed oxide powder is 43 μm and the D90 is 79 μm; (4) The mixed oxide powder obtained in step (3) is added into a mold, and a target blank is obtained by molding and cold isostatic pressing. The molding pressure is 60 MPa, the pressing time is 100 s, and the cold isostatic pressing pressure is 180 MPa, and the pressing time is 70 s.
[0028] (5) The target blank obtained in step (4) is placed in a sintering furnace, and the temperature is raised to 600°C at a rate of 0.5°C / min, and kept in an air atmosphere for 3 hours. The temperature is then raised to 1450°C at a rate of 0.7°C / min, and kept in an oxygen atmosphere for 8 hours. The temperature is then lowered to 1370°C at a rate of 1.5°C / min, and kept in an oxygen atmosphere for 35 hours. An indium titanium tantalum cerium oxide target is obtained.
[0029] After testing, the relative density of the indium titanium tantalum cerium oxide target prepared in this embodiment is 99.45%, the grain size is 6.92μm, and the bending strength is 175Mpa.
[0030] Comparative Example 1 (1) Accurately weigh 50 kg of indium oxide, titanium oxide, tantalum oxide, and cerium oxide powders in a mass ratio of 96.5:0.5:2.0:1.0.
[0031] (2) The powder weighed in step (1) was added to a dispersion tank with 350 g of polyvinyl pyrrolidone and 1050 g of polyvinyl butyral for dispersion at a speed of 80 rpm for 30 min. The dispersed powder was pumped into a sand mill for wet sand grinding at 1100 rpm for 60 min to obtain a mixed slurry with a solid content of 60%.
[0032] (3) spray granulation of the slurry obtained in step (2) in a spray drying tower, and sieving the powder to obtain a mixed oxide powder with uniform particle size distribution, wherein the D50 of the mixed oxide powder is 47 μm and the D90 is 82 μm; (4) The mixed oxide powder obtained in step (3) is added into a mold, and a target blank is obtained by molding and cold isostatic pressing. The molding pressure is 60 MPa, the pressing time is 100 s, and the cold isostatic pressing pressure is 180 MPa, and the pressing time is 70 s.
[0033] (5) The target blank obtained in step (4) was placed in a sintering furnace, and the temperature was raised to 600°C at 0.5°C / min, and kept at this temperature for 3 hours. The temperature was then raised to 1380°C at 0.7°C / min, and kept at this temperature for 20 hours. Thus, an indium titanium tantalum cerium oxide target was obtained.
[0034] After testing, the relative density of the indium titanium tantalum cerium oxide target prepared in this embodiment is 99.35%, the grain size is 12.78μm, and the bending strength is 142Mpa.
[0035] Figure 1 , Figure 2 They are respectively the metallographic picture of the target material obtained in Comparative Example 1 and the histogram of the grain size distribution of the target material obtained. Figure 3 , Figure 4They are the metallographic picture of the target material obtained in Example 1 and the bar chart of the grain size distribution of the target material obtained. It can be seen that the preparation method of the present application can obtain an indium titanium tantalum cerium oxide target material with a more uniform and refined microstructure, and its strength is also significantly improved.
[0036] Comparative Example 2 (1) Accurately weigh 50 kg of indium oxide, titanium oxide, tantalum oxide, and cerium oxide powders in a mass ratio of 96.5.0:1.0:1.5:1.0.
[0037] (2) The powder weighed in step (1) was added to a dispersion tank with 350 g of polyvinyl pyrrolidone and 1050 g of polyvinyl butyral for dispersion at a speed of 80 rpm for 30 min. The dispersed powder was pumped into a sand mill for wet sand grinding at 1100 rpm for 60 min to obtain a mixed slurry with a solid content of 60%.
[0038] (3) spray granulation of the slurry obtained in step (2) in a spray drying tower, and sieving the powder to obtain a mixed oxide powder with uniform particle size distribution, wherein the D50 of the mixed oxide powder is 53 μm and the D90 is 82 μm; (4) The mixed oxide powder obtained in step (3) is added into a mold, and a target blank is obtained by molding and cold isostatic pressing. The molding pressure is 60 MPa, the pressing time is 100 s, and the cold isostatic pressing pressure is 180 MPa, and the pressing time is 70 s.
[0039] (5) The target blank obtained in step (4) is placed in a sintering furnace, and the temperature is raised to 600°C at a rate of 0.5°C / min, and kept at this temperature for 3 h in an air atmosphere. The temperature is then raised to 1530°C at a rate of 0.7°C / min, and kept at this temperature for 8 h in an oxygen atmosphere. The temperature is then lowered to 1380°C at a rate of 1.5°C / min and kept at this temperature for 35 h to obtain an indium titanium tantalum cerium oxide target.
[0040] After testing, the relative density of the indium oxide titanium tantalum cerium titanium tantalum cerium target prepared in this comparative example is 99.24%, the grain size is 15.25μm, and the bending strength is 135Mpa.
[0041] Example 2 (1) Accurately weigh 50 kg of indium oxide, titanium oxide, tantalum oxide, and cerium oxide powders in a mass ratio of 96.5:1.0:1.5:1.0.
[0042] (2) The powder weighed in step (1) was added to a dispersion tank with 350 g of polyvinyl pyrrolidone and 1050 g of polyvinyl butyral for dispersion at a speed of 80 rpm for 30 min. The dispersed powder was pumped into a sand mill for wet sand grinding at 1100 rpm for 60 min to obtain a mixed slurry with a solid content of 60%.
[0043] (3) spray granulation of the slurry obtained in step (2) in a spray drying tower, and sieving the powder to obtain a mixed oxide powder with uniform particle size distribution, wherein the D50 of the mixed oxide powder is 53 μm and the D90 is 76 μm; (4) The mixed oxide powder obtained in step (3) is added into a mold, and a target blank is obtained by molding and cold isostatic pressing. The molding pressure is 60 MPa, the pressing time is 100 s, and the cold isostatic pressing pressure is 180 MPa, and the pressing time is 70 s.
[0044] (5) The target blank obtained in step (4) is placed in a sintering furnace, and the temperature is raised to 600°C at a rate of 0.5°C / min, and kept in an air atmosphere for 3 hours. The temperature is then raised to 1430°C at a rate of 0.7°C / min, and kept in an oxygen atmosphere for 8 hours. The temperature is then lowered to 1350°C at a rate of 1.5°C / min, and kept in an oxygen atmosphere for 35 hours. An indium titanium tantalum cerium oxide target is obtained.
[0045] After testing, the relative density of the indium oxide titanium tantalum cerium titanium tantalum cerium target prepared in this comparative example is 99.28%, the grain size is 7.45μm, and the bending strength is 167 Mpa.
[0046] Figure 5 , Figure 6 They are respectively the metallographic picture of the target material obtained in Comparative Example 2 and the histogram of the grain size distribution of the target material obtained. Figure 7 , Figure 8 They are the metallographic picture of the target material obtained in Example 2 and the bar chart of the grain size distribution of the target material obtained. It can be seen that the preparation method of the present application can obtain an indium titanium tantalum cerium oxide target material with a more uniform and refined microstructure, and its strength is also significantly improved.
[0047] The above are only preferred embodiments of the present invention and are not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the scope of the present invention.
Claims
1. A method for preparing a fine-grained high-strength indium titanium tantalum cerium oxide target, characterized in that: The following steps are involved: (1) Weigh indium oxide powder, titanium oxide powder, tantalum pentoxide powder, and cerium oxide powder in a mass ratio of 95.5-97.5:0.3-2.0:0.3-2.0:0.3-1.5 respectively; (2) mixing and dispersing the powder weighed in step (1) with a dispersant and a binder, and obtaining a mixed slurry by wet grinding; (3) using the mixed slurry as a raw material to perform spray granulation to obtain a mixed oxide powder; (4) Using the mixed oxide powder as a raw material for pressing and molding to obtain a target blank; (5) The target blank is subjected to degreasing sintering and two-stage atmospheric pressure sintering in sequence to obtain an indium titanium tantalum cerium oxide target material, wherein the two-stage atmospheric pressure sintering comprises: Raise the temperature to 1400~1500℃ and keep it warm for 5~10h; Cool down to 1320~1370℃ and keep warm for 35~50h.
2. The preparation method according to claim 1, characterized in that In step (1), the purity of indium oxide powder, titanium oxide powder, tantalum pentoxide powder and cerium oxide powder is 4N.
3. The preparation method according to claim 1, characterized in that: The dispersant is one or more of triethylhexyl phosphate, polyvinyl pyrrolidone, sodium dodecyl sulfate, sodium dodecylbenzene sulfonate, polycarboxylic acid compounds, polyacrylate, and sodium hexadecylbenzene sulfonate; Preferably, the binder is one or more of polyethylene glycol, polyvinyl butyral, carboxymethyl cellulose, polyacrylamide, and polyacrylic acid.
4. The preparation method according to claim 1, characterized in that: In step (2), the mass of the dispersant is 0.5-1.0% of the total mass of the oxide powder, the dispersant and the binder; the mass of the binder is 2.0-3.0% of the total mass of the oxide powder, the dispersant and the binder.
5. The preparation method according to claim 1 or 4, characterized in that: The solid content of the mixed slurry is 50-60%.
6. The preparation method according to claim 1, characterized in that: In step (3), spray granulation is performed using a spray drying tower; the powder obtained after spray granulation is homogenized and sieved to obtain a mixed oxide powder with uniform particle size distribution.
7. The preparation method according to claim 1, characterized in that: In step (4), the molding is performed by first molding and then cold isostatic pressing; Preferably, the molding pressure is 30-100 MPa; the pressing time is 40-120 s; Preferably, the cold isostatic pressing pressure is 150-400 MPa, and the pressing time is 30-180 s.
8. The preparation method according to claim 1, characterized in that: In step (5): The degreasing heat treatment is as follows: in an air atmosphere, the temperature is raised to 500°C to 700°C at a heating rate of 0.5 to 1°C / min, and the temperature is kept for 2 to 5 hours; The two-stage atmospheric pressure sintering is as follows: in an oxygen atmosphere, heating to 1400-1500°C at a heating rate of 0.6-1.2°C / min, and keeping warm for 5-10 hours; cooling to 1320-1370°C at a cooling rate of 1-1.5°C / min, and keeping warm for 35-50 hours.
9. An indium titanium tantalum cerium oxide target prepared by the preparation method according to any one of claims 1 to 8.
10. The indium titanium tantalum cerium oxide target material according to claim 9, characterized in that The indium titanium tantalum cerium oxide target material has a grain size of ≤8μm, a relative density of ≥99%, and a bending strength of ≥160Mpa.
Citation Information
Patent Citations
Preparation method of tubular indium gallium zinc oxide (In2Ga2ZnO7) fine-grain high-density cracking-free target material
CN115894010A
High-mobility indium titanium cerium tantalum oxide target material and preparation method thereof
CN116639956A
Preparation method of high-density indium oxide doped cerium-titanium-tantalum target material
CN117185779A
Zirconia / titanium oxide / cerium oxide doped rare earth tantalum / niobate reta / nbo4 ceramic powder and preparation method thereof
US20220112132A1
Itio rotary target and preparation method therefor
WO2021169418A1
Cited By
Preparation method of doped metal oxide ingot
CN119751021A