Tundish containing beryllium oxide coating and preparation method thereof

By coating the beryllium oxide dispersion on the inner wall of the tundra and roasting it repeatedly, the problems of high cost of beryllium oxide tundra and reduced purity of beryllium powder are solved, and the high purity and thermal impact performance of beryllium powder are achieved, ensuring that the tundra Intimate bonding with the matrix and low cost preparation.

CN119080478AActive Publication Date: 2024-12-06NORTHWEST RARE METALS MATERIALS RESEARCH INSTITUTE NINGXIA CO LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202411133245.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-19
Publication Date
2024-12-06
Estimated Expiration
2044-08-19

AI Technical Summary

Technical Problem

In the prior art, when using inert gas atomization method to produce beryllium powder, the cost of the tundra material is beryllium oxide, which limits the development of atomized beryllium powder technology. In addition, the tundra of other materials will reduce the purity of beryllium powder and affect metallurgy. Product performance.

Method used

Using phosphoric acid as a binder to prepare beryllium oxide dispersion, and then calculating it after multiple coating of beryllium oxide dispersion on the inner wall of the cheap tundra, a kind of beryllium powder can be prepared to resist the thermal impact of metal beryllium melt and ensure the purity of beryllium powder. beryllium oxide-containing coating tundra.

Benefits of technology

The high purity and thermal impact performance of beryllium powder are achieved. The tundra is closely combined with the matrix and there is no residue falling off, reducing the preparation cost.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention discloses a tundish containing a beryllium oxide coating and a preparation method of the tundish, and relates to the technical field of tundish coating preparation. The preparation method comprises the following steps: S1, preparing a first mixed solution from phosphoric acid and deionized water, and then adding beryllium oxide powder and a defoaming agent to obtain a beryllium oxide dispersion liquid; s2, the tundish subjected to sand blasting treatment is immersed in the beryllium oxide dispersion liquid to be subjected to coating treatment for 2-3 times; and S3, the coated tundish is roasted, and the tundish containing the beryllium oxide coating with the thickness ranging from 1.5 mm to 2.0 mm is obtained. According to the method, firstly, phosphoric acid serves as a binder to prepare beryllium oxide dispersion liquid, then the inner wall of the tundish which is low in price is coated with the beryllium oxide dispersion liquid for multiple times, and then roasting is conducted to obtain the tundish containing the beryllium oxide coating, wherein the tundish can resist thermal shock of metal beryllium melt and can guarantee the purity of prepared beryllium powder.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of tundish coating preparation, and in particular relates to a tundish containing beryllium oxide coating and a preparation method thereof. Background Art

[0002] Metal beryllium has many excellent properties such as high elastic modulus, high toughness, easy processing, light weight, high specific stiffness, high specific strength, good thermal stability, high toughness, corrosion resistance, etc. It has broad application prospects in computer manufacturing, automobile industry, high-precision and high-speed welding machine manufacturing and other fields. Because metal beryllium has very strong thermal neutron scattering ability, as a high thermal conductivity, beryllium parts can still maintain their original size when the temperature changes by hundreds of degrees, making beryllium a special functional material and structural material. It has important applications in weapon systems, aerospace and nuclear industries, and has always been a national defense and military material that has attracted much attention at home and abroad.

[0003] The production method of metal beryllium is mainly powder metallurgy. At the same time, metal beryllium powder is mainly prepared by airflow impact method and inert gas atomization method. Beryllium powder prepared by airflow impact method has significant anisotropy. However, powder produced by inert gas atomization method has typical spherical particles, which can significantly reduce or eliminate the anisotropy of the billet. At the same time, spherical powder has good fluidity and high filling density.

[0004] The tundish is an indispensable part of the inert gas atomization powder production. If a prefabricated tundish made of other materials is used, the purity of the beryllium powder will be reduced, seriously affecting the performance of the powder metallurgy product. If a tundish made of beryllium oxide is used, the cost is high, which increases the preparation cost of atomized beryllium powder, thus limiting the development of atomized beryllium powder technology.

[0005] Therefore, the existing technology needs to be improved. Summary of the invention

[0006] In order to solve the above technical problems, the present invention provides a tundish containing beryllium oxide coating and a preparation method thereof. In the method, a beryllium oxide dispersion is first prepared using phosphoric acid as a binder, and then the beryllium oxide dispersion is coated on the inner wall of the low-cost tundish for multiple times and then calcined to obtain a tundish containing beryllium oxide coating that can resist the thermal shock of metal beryllium melt and ensure the purity of the obtained beryllium powder.

[0007] In a first aspect, the present invention provides a method for preparing a tundish containing beryllium oxide coating, wherein the tundish containing beryllium oxide coating is used for atomizing and powdering metal beryllium, and the preparation method comprises the following steps:

[0008] Step S1, mixing phosphoric acid and deionized water at a first speed stirring condition, and then continuing to stir for a first preset time to obtain a first mixed solution, slowly adding beryllium oxide powder to the first mixed solution at a second speed stirring condition, and then adding a defoaming agent to obtain a second mixed solution, and then continuing to stir the second mixed solution at a second speed for a second preset time to obtain a beryllium oxide dispersion;

[0009] The mass ratio of the phosphoric acid to the deionized water is 1:1 to 2:1, the mass ratio of the beryllium oxide powder to the first mixed solution is 1:2 to 1:3, the volume content of the defoaming agent is 0.8 to 1.2%, and the speed of adding the beryllium oxide powder to the first mixed solution is 200 to 300 g / min;

[0010] Step S2, immersing the sandblasted tundish in the beryllium oxide dispersion for 2 to 3 times of coating treatment;

[0011] Step S3, calcining the coated tundish to obtain a tundish containing a beryllium oxide coating with a thickness of 1.5 to 2.0 mm.

[0012] According to the method for preparing a tundish containing beryllium oxide coating according to the first aspect of the present invention, in step S2, the specific process of the coating treatment is as follows:

[0013] The sandblasted tundish is tilted at a preset angle and immersed in the beryllium oxide dispersion for a third preset time, and then the tundish coated with the beryllium oxide dispersion is taken out and allowed to remain in the air until no liquid drips, and then placed in a constant temperature and humidity environment to dry.

[0014] According to the method for preparing a tundish containing beryllium oxide coating as described in the first aspect of the present invention, the tundish after sandblasting is immersed in the beryllium oxide dispersion at an angle of 30° to 45°.

[0015] According to the method for preparing a tundish containing beryllium oxide coating as described in the first aspect of the present invention, during the second coating or the third coating, the tundish is immersed in the beryllium oxide dispersion for 4 to 6 seconds.

[0016] According to the method for preparing a tundish containing beryllium oxide coating described in the first aspect of the present invention, the constant temperature is 24-25° C., the constant humidity is 60-70%, and the drying time is 5-7 hours.

[0017] According to the method for preparing a tundish containing beryllium oxide coating described in the first aspect of the present invention, in the step S3, the heating rate of the roasting is 1.8-2.2°C / min, the target temperature of the roasting is 1050-1350°C, and the holding time of the roasting is 1.8-2.2h.

[0018] According to the method for preparing a tundish containing beryllium oxide coating according to the first aspect of the present invention, in the step S1, the first rotation speed is 180-220 r / min, and the first preset time is 13-17 min;

[0019] The second rotation speed is 480-520 r / min, and the second preset time is 4-6 min.

[0020] According to the method for preparing a tundish containing beryllium oxide coating according to the first aspect of the present invention, in the step S1, the average particle size of the beryllium oxide powder is 1.0 to 1.5 μm, and the purity of the beryllium oxide powder is higher than 98.5 wt.%;

[0021] The mass concentration of the phosphoric acid is 98%.

[0022] According to the method for preparing a tundish containing a beryllium oxide coating as described in the first aspect of the present invention, the tundish is an alumina tundish.

[0023] The second aspect of the present invention provides a tundish containing beryllium oxide coating prepared by the method for preparing a tundish containing beryllium oxide coating as described above, wherein the vacuum degree of the storage environment of the tundish containing beryllium oxide coating is 0.01-10Pa.

[0024] The solution proposed by the present invention has the following technical effects:

[0025] The invention firstly uses phosphoric acid as a binder to prepare a beryllium oxide dispersion, and then coats the beryllium oxide dispersion on the inner wall of a low-cost tundish for many times and then bakes it to obtain a tundish containing a beryllium oxide coating that can resist the thermal shock of a metal beryllium melt and ensure the purity of the obtained beryllium powder.

[0026] In addition, the beryllium oxide-containing coating tundish prepared by the present invention is tightly combined with the base tundish without any residue falling off. DETAILED DESCRIPTION

[0027] In order to make the purpose, technical solution and advantages of the embodiments of the present invention clearer, the technical solution in the embodiments of the present invention will be described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0028] In a first aspect of the present embodiment, a method for preparing a tundish containing beryllium oxide coating is provided. The tundish containing beryllium oxide coating is used for atomizing and powdering metal beryllium. The preparation method comprises the following steps:

[0029] Step S1, mixing phosphoric acid and deionized water under a first speed stirring condition, and then continuing to stir for a first preset time to obtain a first mixed solution, slowly adding beryllium oxide powder to the first mixed solution under a second speed stirring condition, and then adding a defoaming agent to obtain a second mixed solution, and then continuing to stir the second mixed solution at a second speed for a second preset time to obtain a beryllium oxide dispersion.

[0030] Among them, the mass ratio of the phosphoric acid to deionized water is 1:1-2:1, preferably 3:2; the mass ratio of the beryllium oxide powder to the first mixed solution is 1:2-1:3, preferably 3:7; the volume content of the defoaming agent is 0.8-1.2%, preferably 1%; the speed of adding the beryllium oxide powder to the first mixed solution is 200-300 g / min, preferably 240-260 g / min.

[0031] Step S2, immersing the sandblasted tundish in the beryllium oxide dispersion for 2 to 3 times of coating treatment.

[0032] Step S3, calcining the coated tundish to obtain a tundish containing a beryllium oxide coating with a thickness of 1.5 to 2.0 mm.

[0033] In step S1, phosphoric acid and deionized water are mixed under a first speed stirring condition and then continuously stirred for a first preset time to obtain a first mixed solution, beryllium oxide powder is slowly added to the first mixed solution under a second speed stirring condition and then a defoaming agent is added to obtain a second mixed solution, and then the second mixed solution is continuously stirred at a second speed for a second preset time to obtain a beryllium oxide dispersion.

[0034] In this embodiment, phosphoric acid is used as a binder to increase the viscosity of the beryllium oxide dispersion.

[0035] When preparing the beryllium oxide dispersion, this embodiment uses continuous stirring to make the raw materials more evenly mixed, so as to ensure the uniformity of the dispersion of beryllium oxide in the solution and the uniformity of the coating of beryllium oxide on the tundish. At the same time, mixing phosphoric acid and deionized water under stirring can quickly dissipate heat and avoid danger.

[0036] In addition, by adding a defoaming agent and controlling the speed of adding beryllium oxide powder, it is possible to avoid excessive bubbles in the beryllium oxide dispersion to affect the bonding strength between the beryllium oxide coating and the tundish substrate or the risk of the coating falling off.

[0037] In some embodiments, in step S1, the first rotation speed is 180-220 r / min, and the first preset time is 13-17 min;

[0038] The second rotation speed is 480-520 r / min, and the second preset time is 4-6 min.

[0039] Since the viscosity of the mixed liquid increases with the continuous addition of beryllium oxide powder, the stirring speed needs to be increased. However, in order to reduce the generation of bubbles in the mixed liquid, the stirring speed cannot be too high and the stirring time cannot be too long.

[0040] In some embodiments, in step S1, the average particle size of the beryllium oxide powder is 1.0 to 1.5 μm, and the purity of the beryllium oxide powder is higher than 98.5 wt.%;

[0041] The mass concentration of the phosphoric acid is 98%.

[0042] Beryllium oxide powder with an average particle size below 1.0 μm or above 1.5 μm is prone to agglomeration in the solution, affecting the coating effect. Beryllium oxide is highly toxic, and powder with a smaller particle size can be easily inhaled by the human body.

[0043] In some embodiments, the defoaming agent is polyether-modified silicone.

[0044] In some embodiments, the tundish is an alumina tundish.

[0045] In step S2, the tundish after sandblasting is immersed in the beryllium oxide dispersion for coating treatment 2 to 3 times, preferably 2 times.

[0046] Compared with a single coating, the multiple coatings in this embodiment can make the coating more uniform, and at the same time increase the bonding strength and thermal shock resistance of the coating and the tundish substrate; however, if the beryllium oxide coating is too thick, it is easy to increase the risk of falling off. Therefore, the present invention limits the number of coatings to 2 to 3 times so that the coating reaches 1.5 to 2.0 mm.

[0047] In some embodiments, in step S2, the specific process of the coating treatment is as follows:

[0048] The sandblasted tundish is tilted at a preset angle and immersed in the beryllium oxide dispersion for a third preset time, and then the tundish coated with the beryllium oxide dispersion is taken out and allowed to remain in the air until no liquid drips, and then placed in a constant temperature and humidity environment to dry.

[0049] Preferably, the tundish is continuously rotated during the coating process so that the beryllium oxide dispersion is more evenly coated on the surface of the tundish substrate.

[0050] In some embodiments, the sandblasted tundish is tilted at 30° to 45° and immersed in the beryllium oxide dispersion.

[0051] The beryllium oxide dispersion of this embodiment has a certain viscosity. If the tundish is horizontally or vertically immersed in the beryllium oxide dispersion during the coating process, bubbles will be generated, making it impossible for the coating to be tightly combined with the tundish substrate, increasing the risk of the coating falling off later.

[0052] In some embodiments, during the second or third coating, the tundish is immersed in the beryllium oxide dispersion for 4 to 6 seconds to avoid the first coating from falling off due to long-term immersion in the beryllium oxide dispersion.

[0053] In some embodiments, the constant temperature is 24-25° C., the constant humidity is 60-70%, and the drying time is 5-7 hours.

[0054] A constant temperature and humidity environment can prevent the coating from cracking during the drying process.

[0055] Specifically, the specific process of the sandblasting is as follows:

[0056] A 90-mesh alumina powder was sprayed onto the inner wall of the tundish using a sandblasting machine to increase the surface roughness of the inner wall of the tundish, and then the tundish was cleaned.

[0057] In step S3, the coated tundish is calcined to obtain a tundish containing a beryllium oxide coating with a thickness of 1.5 to 2.0 mm.

[0058] In some embodiments, in step S3, the heating rate of the calcination is 1.8-2.2°C / min, the target temperature of the calcination is 1050-1350°C, and the holding time of the calcination is 1.8-2.2h, so as to enhance the bonding strength between the coating and the tundish substrate and avoid the coating from falling off.

[0059] In a second aspect of the present embodiment, a tundish containing beryllium oxide coating is prepared by the method for preparing a tundish containing beryllium oxide coating as described above, wherein the vacuum degree of the storage environment of the tundish containing beryllium oxide coating is 0.01-10Pa.

[0060] Storing the beryllium oxide-coated tundish under vacuum can effectively reduce the risk of coating shedding.

[0061] Example 1

[0062] The first step is to mix phosphoric acid with a mass concentration of 98% and deionized water at a stirring speed of 200 r / min, and then continue to stir for 15 minutes to obtain a first mixed solution, add beryllium oxide powder with an average particle size of 1.2 μm and a purity higher than 98.5 wt.% to the first mixed solution at a stirring speed of 500 r / min, and then add a polyether-modified silicone defoamer to obtain a second mixed solution, and then continue to stir the second mixed solution at a speed of 500 r / min for 5 minutes to obtain a beryllium oxide dispersion. Among them, the mass ratio of phosphoric acid to deionized water is 3:2, the mass ratio of beryllium oxide powder to the first mixed solution is 3:7, the volume content of the polyether-modified silicone defoamer is 1.0%, and the speed of adding beryllium oxide powder to the first mixed solution is 240-260 g / min.

[0063] In the second step, a 90-mesh alumina powder is sprayed onto the inner wall of the tundish using a sandblasting machine, and then the tundish is cleaned.

[0064] The third step is to tilt the sandblasted tundish at 40 degrees and immerse it in the beryllium oxide dispersion for two coating treatments. During the second coating, the tundish is immersed in the beryllium oxide dispersion for 5 seconds; each time the tundish coated with the beryllium oxide dispersion is taken out and left in the air until there is no liquid dripping, and then placed in a drying room at a constant temperature of 24.5°C and a constant humidity of 65% for 6 hours.

[0065] The fourth step is to calcine the coated tundish to obtain a tundish with a beryllium oxide coating having a thickness of 1.8 mm, wherein the calcination heating rate is 2°C / min, the calcination target temperature is 1200°C, and the calcination holding time is 2h.

[0066] The fifth step is to store the beryllium oxide-containing coating tundish in an environment with a vacuum degree of 0.01 to 10 Pa after the coating quality is inspected.

[0067] The beryllium oxide coating of the beryllium oxide-containing tundish prepared in Example 1 has a thickness of 1.8 mm, and the coating is tightly bonded to the substrate tundish without any residue falling off. At the same time, the beryllium oxide coating has no microcracks after being impacted by a 1350-1380° C. metal beryllium melt, and the beryllium oxide content of the prepared beryllium powder meets the use standard.

[0068] Example 2

[0069] The first step is to mix phosphoric acid with a mass concentration of 98% and deionized water at a stirring speed of 180 r / min and continue to stir for 17 minutes to obtain a first mixed solution, add beryllium oxide powder with an average particle size of 1.0 μm and a purity higher than 98.5 wt.% to the first mixed solution at a stirring speed of 480 r / min, and then add a polyether-modified silicone defoamer to obtain a second mixed solution, and then continue to stir the second mixed solution at a speed of 480 r / min for 6 minutes to obtain a beryllium oxide dispersion. Among them, the mass ratio of phosphoric acid to deionized water is 1:1, the mass ratio of beryllium oxide powder to the first mixed solution is 1:2, the volume content of the polyether-modified silicone defoamer is 1.2%, and the speed of adding beryllium oxide powder to the first mixed solution is 240-300 g / min.

[0070] In the second step, a 90-mesh alumina powder is sprayed onto the inner wall of the tundish using a sandblasting machine, and then the tundish is cleaned.

[0071] The third step is to tilt the sandblasted tundish at 30 degrees and immerse it in the beryllium oxide dispersion for two coating treatments. During the second coating, the tundish is immersed in the beryllium oxide dispersion for 4 seconds; each time the tundish coated with the beryllium oxide dispersion is taken out and left in the air until there is no liquid dripping, and then placed in a drying room at a constant temperature of 24°C and a constant humidity of 60% for 7 hours.

[0072] The fourth step is to calcine the coated tundish to obtain a tundish with a beryllium oxide coating with a thickness of 2.0 mm, wherein the calcination heating rate is 1.8°C / min, the calcination target temperature is 1050°C, and the calcination holding time is 2.2h.

[0073] The fifth step is to store the beryllium oxide-containing coating tundish in an environment with a vacuum degree of 0.01 to 10 Pa after the coating quality is inspected.

[0074] The beryllium oxide coating of the beryllium oxide-containing tundish prepared in Example 2 has a thickness of 2.0 mm, and the coating is tightly bonded to the substrate tundish without any residue falling off. At the same time, the beryllium oxide coating has no microcracks after being impacted by a 1350-1380° C. metal beryllium melt, and the beryllium oxide content of the prepared beryllium powder meets the use standard.

[0075] Example 3

[0076] The first step is to mix phosphoric acid with a mass concentration of 98% and deionized water at a stirring speed of 220 r / min and continue to stir for 13 minutes to obtain a first mixed solution, add beryllium oxide powder with an average particle size of 1.5 μm and a purity higher than 98.5 wt.% to the first mixed solution at a stirring speed of 520 r / min, and then add a polyether-modified silicone defoamer to obtain a second mixed solution, and then continue to stir the second mixed solution at a speed of 520 r / min for 4 minutes to obtain a beryllium oxide dispersion. Among them, the mass ratio of phosphoric acid to deionized water is 2:1, the mass ratio of beryllium oxide powder to the first mixed solution is 1:3, the volume content of the polyether-modified silicone defoamer is 0.8%, and the speed of adding beryllium oxide powder to the first mixed solution is 200-240 g / min.

[0077] In the second step, a 90-mesh alumina powder is sprayed onto the inner wall of the tundish using a sandblasting machine, and then the tundish is cleaned.

[0078] The third step is to immerse the sandblasted tundish at an angle of 45 degrees in the beryllium oxide dispersion for three times of coating. During the second coating, the tundish is immersed in the beryllium oxide dispersion for 6 seconds; each time the tundish coated with the beryllium oxide dispersion is taken out and held in the air until no liquid drips, and then placed in a drying room at a constant temperature of 25°C and a constant humidity of 70% for 5 hours.

[0079] The fourth step is to calcine the coated tundish to obtain a tundish with a beryllium oxide coating with a thickness of 1.5 mm, wherein the calcination heating rate is 2.2°C / min, the calcination target temperature is 1350°C, and the calcination holding time is 1.8h.

[0080] The fifth step is to store the beryllium oxide-containing coating tundish in an environment with a vacuum degree of 0.01 to 10 Pa after the coating quality is inspected.

[0081] The beryllium oxide coating of the beryllium oxide-containing tundish prepared in Example 3 has a thickness of 1.5 mm, and the coating is tightly bonded to the substrate tundish without any residue falling off. At the same time, the beryllium oxide coating has no microcracks after being impacted by a 1350-1380° C. metal beryllium melt, and the beryllium oxide content of the prepared beryllium powder meets the use standard.

[0082] In summary, the solution proposed by the present invention has the following technical effects:

[0083] The invention firstly uses phosphoric acid as a binder to prepare a beryllium oxide dispersion, and then coats the beryllium oxide dispersion on the inner wall of a low-cost tundish for many times and then bakes it to obtain a tundish containing a beryllium oxide coating that can resist the thermal shock of a metal beryllium melt and ensure the purity of the obtained beryllium powder.

[0084] In addition, the beryllium oxide-containing coating tundish prepared by the present invention is tightly combined with the base tundish without any residue falling off.

[0085] Please note that the technical features of the above embodiments can be combined arbitrarily. In order to make the description concise, all possible combinations of the technical features in the above embodiments are not described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification. The above embodiments only express several implementation methods of the present application, and their descriptions are relatively specific and detailed, but they cannot be understood as limiting the scope of the invention patent. It should be pointed out that for ordinary technicians in this field, without departing from the concept of the present application, several variations and improvements can be made, which all belong to the scope of protection of the present application. Therefore, the scope of protection of the patent in this application shall be based on the attached claims.

Claims

1. A method for preparing a tundish containing beryllium oxide coating, wherein the tundish containing beryllium oxide coating is used for atomizing and powdering metal beryllium. It is characterized in that The preparation method comprises the following steps: Step S1, mixing phosphoric acid and deionized water at a first speed stirring condition, and then continuing to stir for a first preset time to obtain a first mixed solution, slowly adding beryllium oxide powder to the first mixed solution at a second speed stirring condition, and then adding a defoaming agent to obtain a second mixed solution, and then continuing to stir the second mixed solution at a second speed for a second preset time to obtain a beryllium oxide dispersion; The mass ratio of the phosphoric acid to the deionized water is 1:1 to 2:1, the mass ratio of the beryllium oxide powder to the first mixed solution is 1:2 to 1:3, the volume content of the defoaming agent is 0.8 to 1.2%, and the speed of adding the beryllium oxide powder to the first mixed solution is 200 to 300 g / min; Step S2, immersing the sandblasted tundish in the beryllium oxide dispersion for 2 to 3 times of coating treatment; Step S3, calcining the coated tundish to obtain a tundish containing a beryllium oxide coating with a thickness of 1.5 to 2.0 mm.

2. The method for preparing a tundish containing beryllium oxide coating according to claim 1, It is characterized in that In step S2, the specific process of the coating treatment is as follows: The sandblasted tundish is tilted at a preset angle and immersed in the beryllium oxide dispersion for a third preset time, and then the tundish coated with the beryllium oxide dispersion is taken out and allowed to remain in the air until no liquid drips, and then placed in a constant temperature and humidity environment to dry.

3. The method for preparing a tundish containing beryllium oxide coating according to claim 2, It is characterized in that The sandblasted tundish is tilted at 30° to 45° and immersed in the beryllium oxide dispersion.

4. The method for preparing a tundish containing beryllium oxide coating according to claim 2, It is characterized in that During the second coating or the third coating, the tundish is immersed in the beryllium oxide dispersion for 4 to 6 seconds.

5. The method for preparing a tundish containing beryllium oxide coating according to claim 2, It is characterized in that The constant temperature is 24-25° C., the constant humidity is 60-70%, and the drying time is 5-7 hours.

6. The method for preparing a tundish containing beryllium oxide coating according to claim 1, It is characterized in that In the step S3, the heating rate of the calcination is 1.8-2.2°C / min, the target temperature of the calcination is 1050-1350°C, and the holding time of the calcination is 1.8-2.2h.

7. The method for preparing a tundish containing beryllium oxide coating according to claim 1, It is characterized in that In the step S1, the first rotation speed is 180-220 r / min, and the first preset time is 13-17 min; The second rotation speed is 480-520 r / min, and the second preset time is 4-6 min.

8. The method for preparing a tundish containing beryllium oxide coating according to claim 1, It is characterized in that In the step S1, the average particle size of the beryllium oxide powder is 1.0 to 1.5 μm, and the purity of the beryllium oxide powder is higher than 98.5 wt.%; The mass concentration of the phosphoric acid is 98%.

9. The method for preparing a tundish containing beryllium oxide coating according to claim 1, It is characterized in that The tundish is an alumina tundish.

10. A tundish containing beryllium oxide coating prepared according to the method for preparing a tundish containing beryllium oxide coating according to any one of claims 1 to 9, It is characterized in that The vacuum degree of the storage environment of the beryllium oxide-containing tundish is 0.01-10Pa.

Citation Information

Patent Citations

  • Metal oxide based refractory ceramic hard-en - acid

    CH507883A

  • No title available

    GB1234043A

  • Crucible and heater assembly

    GB1535688A

  • Improvements in the manufacture and production of valuable hydrocarbons

    GB302253A

  • Improvements in or relating to wehnelt cathodes

    GB309578A