Lightweight periclase-calcium hexaluminate-calcium zirconate aggregate and preparation method thereof
By using raw materials such as magnesium hydroxide and aluminum hydroxide to prepare lightweight magnesite-calcium hexaluminate-calcium zirconate aggregate, the problems of high thermal conductivity and insufficient thermal shock resistance of magnesium refractory materials are solved, and the low Magnesium refractory material with thermal conductivity, high strength and excellent thermal shock resistance.
Patent Information
- Application Number
- CN202411081652.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-08
- Publication Date
- 2024-12-06
AI Technical Summary
The existing magnesium refractory materials have high thermal conductivity, resulting in a lot of heat dissipation and insufficient thermal shock and corrosion resistance, making it difficult to meet the high-temperature industrial energy saving and emission reduction and use requirements of metallurgical furnace lining.
70.0-90.0 wt% magnesium hydroxide fine powder and 10.0-30.0 wt% aluminum hydroxide fine powder as raw materials, calcium carbonate fine powder, monoclinic zirconia fine powder and polyvinyl alcohol were used, and the machine was pressed and dried. With high-temperature insulation treatment, lightweight magnesite-calcium hexaluminate-calcium zirconate aggregate was prepared to form materials with low thermal conductivity, high strength and excellent thermal shock resistance.
The comprehensive effect of the material is achieved with low thermal conductivity, high porosity, high strength, excellent thermal shock resistance and good corrosion resistance, and significantly improve the high-temperature industrial performance of metallurgical furnace lining.
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of magnesium-aluminum aggregates, and specifically relates to a lightweight periclase-calcium hexaaluminate-calcium zirconate aggregate and a preparation method thereof. Background Art
[0002] Magnesia refractory materials are widely used in steel-making converters, electric furnaces, ladles and other metallurgical furnace linings due to their high melting point and excellent slag resistance. Existing magnesia refractory materials are prepared using dense electric melting or sintering magnesia sand raw materials to ensure that they have excellent performance. However, the high thermal conductivity of dense magnesia sand causes a large amount of heat to be dissipated from the lining of the metallurgical furnace, which is not conducive to energy conservation and emission reduction in high-temperature industries. For this reason, the low thermal conductivity and improvement of other properties of magnesia refractory materials have become one of the hot topics of concern to those skilled in the art.
[0003] The patented technology of "A method for preparing porous magnesium-aluminum spinel by reaction synthesis" (CN102795884A) uses magnesium oxide and aluminum powder as raw materials and utilizes the polymer oxidation combustion method to synthesize porous magnesium-aluminum spinel porous raw materials. Although the raw materials contain relatively few impurities, they have high thermal conductivity, low strength and poor thermal shock resistance.
[0004] The patented technology of "Nanopore porous periclase-magnesium aluminum spinel ceramic material and preparation method thereof" (CN107445593A) uses magnesite and aluminum sol as main raw materials and utilizes in-situ decomposition method to prepare porous periclase-magnesium aluminum spinel raw material. Although the thermal conductivity of this raw material is low, the magnesite raw material contains more impurities, so the strength and corrosion resistance of the raw material are poor.
[0005] The patented technology of "A method for preparing porous calcium hexaaluminate ceramics with uniform structure" (CN116217219A) uses CaCO3 powder and boehmite AlOOH powder as raw materials to prepare porous calcium hexaaluminate ceramic materials. Although the material is low in cost and the process is simple, it has a high apparent porosity and poor strength and thermal shock resistance.
[0006] The patented technology of "A method for preparing low thermal conductivity calcium zirconate material" (CN114057504A) uses calcium hydroxide and basic zirconium carbonate as raw materials to prepare low thermal conductivity calcium zirconate material. Although the material has good high-temperature mechanical properties, the material's apparent porosity is too high, resulting in the material's thermal shock resistance and corrosion resistance being difficult to meet the use requirements. Summary of the invention
[0007] The present invention aims to overcome the defects of the prior art and aims to provide a lightweight periclase-calcium hexaaluminate-calcium zirconate aggregate with high strength, high closed porosity, low thermal conductivity, excellent thermal shock resistance and corrosion resistance, and a preparation method thereof.
[0008] To achieve the above purpose, the technical solution adopted by the present invention is:
[0009] 70.0-90.0wt% of magnesium hydroxide fine powder and 10.0-30.0wt% of aluminum hydroxide fine powder are used as raw materials, and 2.0-8.0wt% of calcium carbonate fine powder, 1.0-3.0wt% of monoclinic zirconium oxide fine powder and 2.5-5.0wt% of polyvinyl alcohol are added to the raw materials, stirred evenly, pressed into shape by a machine, and dried; then kept warm at 600-1000°C for 1-4 hours, and then kept warm at 1400-1600°C for 1-6 hours, cooled, crushed, sieved, and packaged to obtain a lightweight periclase-calcium hexaaluminate-calcium zirconate aggregate.
[0010] The Mg(OH)2 content of the magnesium hydroxide fine powder is greater than 99wt%; the particle size of the magnesium hydroxide fine powder is 600-800μm.
[0011] The Al(OH)3 content of the aluminum hydroxide fine powder is greater than 99wt%; the particle size of the aluminum hydroxide fine powder is less than 20μm.
[0012] The CaCO3 content of the calcium carbonate fine powder is greater than 98wt%; the particle size of the calcium carbonate fine powder is less than 20μm.
[0013] The ZrO2 content of the monoclinic zirconia fine powder is greater than 98wt%; and the particle size of the monoclinic zirconia fine powder is less than 20μm.
[0014] The pH value of the polyvinyl alcohol is 6-8.
[0015] The pressure of the machine compression molding is 30-60 MPa.
[0016] The drying temperature is 90-110° C., and the drying time is 8-12 hours.
[0017] Due to the adoption of the above technical solution, the present invention has the following positive effects compared with the prior art:
[0018] The lightweight periclase-calcium hexaaluminate-calcium zirconate aggregate prepared by the present invention uses magnesium hydroxide with a particle size of 600-800 μm as a raw material, and the magnesium hydroxide can be decomposed in situ at 400-1000° C. to form agglomerates containing a large number of micro-nano pores and MgO microcrystals. At the same time, the Al2O3 and CaO formed by the decomposition of aluminum hydroxide fine powder and calcium carbonate fine powder are small in particle size and highly active, and the two can react to generate low melting point phases such as calcium monoaluminate and calcium dodecaaluminate. The low melting point phase exists in a liquid phase at high temperature, and the pores are closed in the agglomerate, so that most of the pores in the prepared lightweight periclase-calcium hexaaluminate-calcium zirconate aggregate exist in the form of closed pores, giving the prepared product a low thermal conductivity and high slag erosion resistance. At the same time, the formation of the liquid phase can promote material transmission and neck connection between agglomerates, improve the degree of bonding between agglomerates, and give the lightweight periclase-calcium hexaaluminate-calcium zirconate aggregate high strength.
[0019] In the present invention, as the sintering temperature increases, low melting point phases such as calcium monoaluminate and calcium dodecaaluminate heptaaluminate will further react with the remaining Al2O3 to generate calcium hexaaluminate with a high melting point. Since calcium hexaaluminate has a flaky structure, crack deflection can be promoted, ensuring that the prepared lightweight periclase-calcium hexaaluminate-calcium zirconate aggregate has excellent thermal shock resistance. Low melting point phases such as calcium monoaluminate and calcium dodecaaluminate heptaaluminate will also react with the added monoclinic zirconium oxide fine powder to generate calcium zirconate with a high melting point and good stability, further improving the corrosion resistance of the product.
[0020] The lightweight periclase-calcium hexaaluminate-calcium zirconate aggregate prepared by the present invention is tested to have the following characteristics: apparent porosity is 1.5-5.5%; closed porosity is 15.0-21.0%; average pore size is 0.20-0.70 μm; flexural strength is 140-170 MPa; thermal conductivity is 2.0-5.5 W / (m·k) at 500° C.; thermal shock stability has a residual strength retention rate of 82-92% after one water cooling at 900° C.
[0021] Therefore, the lightweight periclase-calcium hexaaluminate-calcium zirconate aggregate prepared by the present invention has the characteristics of high closed porosity, low thermal conductivity, high strength, excellent thermal shock resistance and excellent corrosion resistance. DETAILED DESCRIPTION
[0022] The present invention is further described below in conjunction with specific embodiments, but is not intended to limit the scope of protection thereof:
[0023] A lightweight periclase-calcium hexaaluminate-calcium zirconate aggregate and a preparation method thereof. The preparation method described in this specific embodiment is:
[0024] 70.0-90.0wt% of magnesium hydroxide fine powder and 10.0-30.0wt% of aluminum hydroxide fine powder are used as raw materials, and 2.0-8.0wt% of calcium carbonate fine powder, 1.0-3.0wt% of monoclinic zirconium oxide fine powder and 2.5-5.0wt% of polyvinyl alcohol are added to the raw materials, stirred evenly, pressed into shape by a machine, and dried; then kept warm at 600-1000°C for 1-4 hours, and then kept warm at 1400-1600°C for 1-6 hours, cooled, crushed, sieved, and packaged to obtain a lightweight periclase-calcium hexaaluminate-calcium zirconate aggregate.
[0025] The Mg(OH)2 content of the magnesium hydroxide fine powder is greater than 99 wt%.
[0026] The Al(OH)3 content of the aluminum hydroxide fine powder is greater than 99 wt%.
[0027] The CaCO3 content of the calcium carbonate fine powder is greater than 98 wt%.
[0028] The ZrO2 content of the monoclinic zirconium oxide fine powder is greater than 98 wt%.
[0029] The pH value of the polyvinyl alcohol is 6-8.
[0030] The pressure of the machine compression molding is 30-60 MPa.
[0031] The drying temperature is 90-110° C., and the drying time is 8-12 hours.
[0032] In this specific implementation mode:
[0033] The particle size of the magnesium hydroxide fine powder is 600 to 800 μm;
[0034] The particle size of the aluminum hydroxide fine powder is less than 20 μm;
[0035] The particle size of the calcium carbonate fine powder is less than 20 μm;
[0036] The particle size of the monoclinic zirconium oxide fine powder is less than 20 μm.
[0037] This will not be described in detail in the embodiments.
[0038] Example 1
[0039] A lightweight periclase-calcium hexaaluminate-calcium zirconate aggregate and a preparation method thereof. The preparation method described in this embodiment is:
[0040] 70.0wt% of magnesium hydroxide fine powder and 30.0wt% of aluminum hydroxide fine powder are used as raw materials, and 2.0wt% of calcium carbonate fine powder, 1.0wt% of monoclinic zirconium oxide fine powder and 2.5wt% of polyvinyl alcohol are added to the raw materials, stirred evenly, pressed into shape by a machine, and dried; then kept warm at 600°C for 4 hours, and then kept warm at 1400°C for 1 hour, cooled, crushed, sieved, and packaged to obtain a lightweight periclase-calcium hexaaluminate-calcium zirconate aggregate.
[0041] The magnesium hydroxide fine powder has a Mg(OH)2 content of 99.1 wt%.
[0042] The Al(OH)3 content of the aluminum hydroxide fine powder is 99.6 wt%.
[0043] The CaCO3 content of the calcium carbonate fine powder is 98.3 wt%.
[0044] The ZrO2 content of the monoclinic zirconium oxide fine powder is 98.2 wt%.
[0045] The pH value of the polyvinyl alcohol is 6.
[0046] The pressure of the machine compression molding is 30MPa.
[0047] The drying temperature is 90° C. and the drying time is 12 hours.
[0048] The lightweight periclase-calcium hexaaluminate-calcium zirconate aggregate prepared in this embodiment was tested and found to have an apparent porosity of 1.5%; a closed porosity of 15.0%; an average pore size of 0.20 μm; a flexural strength of 170 MPa; a thermal conductivity of 5.5 W / (m·k) at 500°C; and a thermal shock stability of 92% residual strength after one water cooling at 900°C.
[0049] Example 2
[0050] A lightweight periclase-calcium hexaaluminate-calcium zirconate aggregate and a preparation method thereof. The preparation method described in this embodiment is:
[0051] 90.0wt% of magnesium hydroxide fine powder and 10.0wt% of aluminum hydroxide fine powder are used as raw materials, and 8.0wt% of calcium carbonate fine powder, 3.0wt% of monoclinic zirconium oxide fine powder and 5.0wt% of polyvinyl alcohol are added to the raw materials, stirred evenly, pressed into shape by a machine, and dried; then kept warm at 1000°C for 1 hour, and then kept warm at 1600°C for 6 hours, cooled, crushed, sieved, and packaged to obtain a lightweight periclase-calcium hexaaluminate-calcium zirconate aggregate.
[0052] The magnesium hydroxide fine powder has a Mg(OH)2 content of 99.2 wt%.
[0053] The Al(OH)3 content of the aluminum hydroxide fine powder is 99.4 wt%.
[0054] The CaCO3 content of the calcium carbonate fine powder is 98.1 wt%.
[0055] The ZrO2 content of the monoclinic zirconium oxide fine powder is 98.5 wt%.
[0056] The pH value of the polyvinyl alcohol is 7.
[0057] The pressure of the machine compression molding is 40MPa.
[0058] The drying temperature is 100° C. and the drying time is 11 hours.
[0059] The lightweight periclase-calcium hexaaluminate-calcium zirconate aggregate prepared in this embodiment was tested: the apparent porosity was 5.5%; the closed porosity was 21.0%; the average pore size was 0.70μm; the flexural strength was 140MPa; the thermal conductivity was 2.0W / (m·k) at 500℃; the thermal shock stability was 82% after one water cooling at 900℃.
[0060] Example 3
[0061] A lightweight periclase-calcium hexaaluminate-calcium zirconate aggregate and a preparation method thereof. The preparation method described in this embodiment is:
[0062] 80.0wt% of magnesium hydroxide fine powder and 20.0wt% of aluminum hydroxide fine powder are used as raw materials, and 5.0wt% of calcium carbonate fine powder, 2.0wt% of monoclinic zirconium oxide fine powder and 4.0wt% of polyvinyl alcohol are added to the raw materials, stirred evenly, pressed into shape by a machine, and dried; then kept warm at 800°C for 2 hours, and then kept warm at 1500°C for 4 hours, cooled, crushed, sieved, and packaged to obtain lightweight periclase-calcium hexaaluminate-calcium zirconate aggregate.
[0063] The Mg(OH)2 content of the magnesium hydroxide fine powder is 99.4 wt%.
[0064] The Al(OH)3 content of the aluminum hydroxide fine powder is 99.1 wt%.
[0065] The CaCO3 content of the calcium carbonate fine powder is 98.2 wt%.
[0066] The ZrO2 content of the monoclinic zirconium oxide fine powder is 98.1 wt%.
[0067] The pH value of the polyvinyl alcohol is 8.
[0068] The pressure of the machine compression molding is 45MPa.
[0069] The drying temperature is 110° C. and the drying time is 8 hours.
[0070] The lightweight periclase-calcium hexaaluminate-calcium zirconate aggregate prepared in this embodiment was tested and found to have an apparent porosity of 3.6%; a closed porosity of 17.8%; an average pore size of 0.52 μm; a flexural strength of 150 MPa; a thermal conductivity of 3.4 W / (m·k) at 500°C; and a thermal shock stability of 86% of residual strength after one water cooling at 900°C.
[0071] Example 4
[0072] A lightweight periclase-calcium hexaaluminate-calcium zirconate aggregate and a preparation method thereof. The preparation method described in this embodiment is:
[0073] 75.0wt% of magnesium hydroxide fine powder and 25.0wt% of aluminum hydroxide fine powder are used as raw materials, and 7.0wt% of calcium carbonate fine powder, 2.5wt% of monoclinic zirconium oxide fine powder and 3.0wt% of polyvinyl alcohol are added to the raw materials, stirred evenly, pressed into shape by a machine, and dried; then kept warm at 900°C for 3 hours, and then kept warm at 1550°C for 3 hours, cooled, crushed, sieved, and packaged to obtain lightweight periclase-calcium hexaaluminate-calcium zirconate aggregate.
[0074] The magnesium hydroxide fine powder has a Mg(OH)2 content of 99.5 wt%.
[0075] The Al(OH)3 content of the aluminum hydroxide fine powder is 99.3 wt%.
[0076] The CaCO3 content of the calcium carbonate fine powder is 98.5 wt%.
[0077] The ZrO2 content of the monoclinic zirconium oxide fine powder is 98.4 wt%.
[0078] The pH value of the polyvinyl alcohol is 6.5.
[0079] The pressure of the machine compression molding is 50MPa.
[0080] The drying temperature is 100° C. and the drying time is 9 hours.
[0081] The lightweight periclase-calcium hexaaluminate-calcium zirconate aggregate prepared in this embodiment was tested and found to have an apparent porosity of 2.4%; a closed porosity of 19.5%; an average pore size of 0.31 μm; a flexural strength of 165 MPa; a thermal conductivity of 2.6 W / (m·k) at 500°C; and a thermal shock stability of 90% residual strength after one water cooling at 900°C.
[0082] Example 5
[0083] A lightweight periclase-calcium hexaaluminate-calcium zirconate aggregate and a preparation method thereof. The preparation method described in this embodiment is:
[0084] 85.0wt% of magnesium hydroxide fine powder and 15.0wt% of aluminum hydroxide fine powder are used as raw materials, and 4.0wt% of calcium carbonate fine powder, 1.5wt% of monoclinic zirconium oxide fine powder and 3.5wt% of polyvinyl alcohol are added to the raw materials, stirred evenly, pressed into shape by a machine, and dried; then kept warm at 700°C for 3 hours, and then kept warm at 1450°C for 5 hours, cooled, crushed, sieved, and packaged to obtain lightweight periclase-calcium hexaaluminate-calcium zirconate aggregate.
[0085] The Mg(OH)2 content of the magnesium hydroxide fine powder is 99.4 wt%.
[0086] The Al(OH)3 content of the aluminum hydroxide fine powder is 99.2 wt%.
[0087] The CaCO3 content of the calcium carbonate fine powder is 98.4 wt%.
[0088] The ZrO2 content of the monoclinic zirconium oxide fine powder is 98.7 wt%.
[0089] The pH value of the polyvinyl alcohol is 7.5.
[0090] The pressure of the machine compression molding is 60MPa.
[0091] The drying temperature is 90° C. and the drying time is 10 hours.
[0092] The lightweight periclase-calcium hexaaluminate-calcium zirconate aggregate prepared in this embodiment was tested: the apparent porosity was 2.9%; the closed porosity was 19.3%; the average pore size was 0.62μm; the flexural strength was 152MPa; the thermal conductivity was 3.8W / (m·k) at 500℃; the thermal shock stability was 87% after one water cooling at 900℃.
[0093] Compared with the prior art, this specific implementation has the following positive effects:
[0094] The lightweight periclase-calcium hexaaluminate-calcium zirconate aggregate prepared in this specific embodiment uses magnesium hydroxide with a particle size of 600-800 μm as a raw material, and the magnesium hydroxide can be decomposed in situ at 400-1000°C to form agglomerates containing a large number of micro-nano pores and MgO microcrystals. At the same time, the Al2O3 and CaO formed by the decomposition of aluminum hydroxide fine powder and calcium carbonate fine powder are small in particle size and highly active, and the reaction of the two can generate low melting point phases such as calcium aluminate and calcium heptadecaluminate. The low melting point phase exists in a liquid phase at high temperature, and the pores are closed in the agglomerate, so that most of the pores in the prepared lightweight periclase-calcium hexaaluminate-calcium zirconate aggregate exist in the form of closed pores, giving the manufactured product a low thermal conductivity and high slag erosion resistance. At the same time, the formation of the liquid phase can promote material transmission and neck connection between agglomerates, improve the degree of bonding between agglomerates, and give the lightweight periclase-calcium hexaaluminate-calcium zirconate aggregate high strength.
[0095] In this specific embodiment, as the sintering temperature increases, low melting point phases such as calcium monoaluminate and calcium dodecaaluminate heptaaluminate will further react with the remaining Al2O3 to generate high melting point calcium hexaaluminate. Since calcium hexaaluminate has a flaky structure, it can promote crack deflection, ensuring that the prepared lightweight periclase-calcium hexaaluminate-calcium zirconate aggregate has excellent thermal shock resistance. Low melting point phases such as calcium monoaluminate and calcium dodecaaluminate heptaaluminate will also react with the added monoclinic zirconium oxide fine powder to generate calcium zirconate with high melting point and good stability, further improving the corrosion resistance of the product.
[0096] The lightweight periclase-calcium hexaaluminate-calcium zirconate aggregate prepared in this specific embodiment has been tested: the apparent porosity is 1.5-5.5%; the closed porosity is 15.0-21.0%; the average pore size is 0.20-0.70 μm; the flexural strength is 140-170 MPa; the thermal conductivity is 2.0-5.5 W / (m·k) at 500°C; the thermal shock stability is 82-92% of the residual strength retention rate after one water cooling at 900°C.
[0097] Therefore, the lightweight periclase-calcium hexaaluminate-calcium zirconate aggregate prepared in this specific embodiment has the characteristics of high closed porosity, low thermal conductivity, high strength, excellent thermal shock resistance and excellent corrosion resistance.
Claims
1. A method for preparing a lightweight periclase-calcium hexaaluminate-calcium zirconate aggregate, characterized in that: 70.0-90.0wt% of magnesium hydroxide fine powder and 10.0-30.0wt% of aluminum hydroxide fine powder are used as raw materials, and 2.0-8.0wt% of calcium carbonate fine powder, 1.0-3.0wt% of monoclinic zirconium oxide fine powder and 2.5-5.0wt% of polyvinyl alcohol are added to the raw materials, stirred evenly, pressed into shape by a machine, and dried; then kept warm at 600-1000°C for 1-4 hours, and then kept warm at 1400-1600°C for 1-6 hours, cooled, crushed, sieved, and packaged to obtain a lightweight periclase-calcium hexaaluminate-calcium zirconate aggregate.
2. The method for preparing the lightweight periclase-calcium hexaaluminate-calcium zirconate aggregate according to claim 1, characterized in that The Mg(OH)2 content of the magnesium hydroxide fine powder is greater than 99wt%; the particle size of the magnesium hydroxide fine powder is 600-800μm.
3. The method for preparing the lightweight periclase-calcium hexaaluminate-calcium zirconate aggregate according to claim 1, characterized in that The Al(OH)3 content of the aluminum hydroxide fine powder is greater than 99wt%; the particle size of the aluminum hydroxide fine powder is less than 20μm.
4. The method for preparing the lightweight periclase-calcium hexaaluminate-calcium zirconate aggregate according to claim 1, characterized in that The CaCO3 content of the calcium carbonate fine powder is greater than 98wt%; the particle size of the calcium carbonate fine powder is less than 20μm.
5. The method for preparing the lightweight periclase-calcium hexaaluminate-calcium zirconate aggregate according to claim 1, characterized in that The ZrO2 content of the monoclinic zirconia fine powder is greater than 98wt%; and the particle size of the monoclinic zirconia fine powder is less than 20μm.
6. The method for preparing the lightweight periclase-calcium hexaaluminate-calcium zirconate aggregate according to claim 1, characterized in that The pH value of the polyvinyl alcohol is 6-8.
7. The method for preparing the lightweight periclase-calcium hexaaluminate-calcium zirconate aggregate according to claim 1, characterized in that The pressure of the machine compression molding is 30-60 MPa.
8. The method for preparing lightweight periclase-calcium hexaaluminate-calcium zirconate aggregate according to claim 1, characterized in that The drying temperature is 90-110° C., and the drying time is 8-12 hours.
9. A lightweight periclase-calcium hexaaluminate-calcium zirconate aggregate, characterized in that The lightweight periclase-calcium hexaaluminate-calcium zirconate aggregate is a lightweight periclase-calcium hexaaluminate-calcium zirconate aggregate prepared by the method for preparing lightweight periclase-calcium hexaaluminate-calcium zirconate aggregate according to any one of claims 1 to 8.
Citation Information
Patent Citations
Preparation method for synthesizing porous magnesium aluminate spinel by reacting
CN102795884A
Nano-aperture porous periclase-magnesium aluminate spinel ceramic material and preparation method thereof
CN107445593A
Low-thermal-conductivity calcium zirconate material and preparation method thereof
CN114057504A
Preparation method of porous calcium hexaluminate ceramic with uniform structure
CN116217219A
Micropore high-strength corundum-calcium hexaluminate composite refractory raw material and preparation method thereof